Heavy metal settling agent and application thereof
By modifying and grafting the montmorillonite, a crosslinked structure was formed, and a heavy metal precipitant was modified by dithiocarbamic acid, the problem of poor adsorption effect in low temperature environments in the prior art was solved, and the problem of poor adsorption effect in low temperature environments was achieved. Efficient and stable heavy metal removal effect.
Patent Information
- Application Number
- CN202410976346.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing heavy metal sedimentants have poor adsorption effect on heavy metals under low temperature environments, and their adsorption performance is unstable, which affects the effect of wastewater treatment.
Using dithiocarbamic acid modified composite and polyacrylamide, the montmorillonite is initially modified, grafted and secondary modification to form a cross-linked network structure, enhancing the adsorption capacity and stability, and through disulfide Carbamation reaction produces heavy metal precipitants.
Maintaining good heavy metal chelation and settlement performance at low temperatures improves the removal rate of heavy metals such as nickel, chromium, cobalt, lead, mercury and manganese, and ensuring the stability and efficiency of wastewater treatment.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heavy metal sedimentation agents, and specifically relates to a heavy metal sedimentation agent and application thereof. Background Art
[0002] Although the rapid development of emerging industries has brought great convenience to people's lives, various mining, metal smelting, electroplating industry, fertilizer industry, etc. produce a large amount of heavy metal-containing wastewater, which is discharged into the environmental water bodies, causing a sharp increase in the heavy metal content in the environmental water bodies, causing serious environmental pollution, and can cause acute and chronic poisoning of humans and animals. It can accumulate in the human body and bioaccumulate in the food chain, causing various diseases and even death, which seriously threatens human health.
[0003] At present, the treatment methods for heavy metal wastewater mainly include chemical precipitation, electrolysis, ion exchange, membrane treatment, solvent extraction and replacement, among which chemical precipitation is the lowest cost and simplest method, and it is also the preferred method for heavy metal wastewater treatment; Therefore, providing a method for removing heavy metal ions in sewage with simple operation and low production cost is a difficult problem that needs to be developed urgently in the prior art.
[0004] In response to this, technicians have developed a heavy metal precipitator, which is a sulfur-containing compound that stably combines with heavy metals through sulfur groups and undergoes chemical reactions to form stable organic metal compounds that are not easily soluble and form solid precipitation in aqueous solutions, which can then be separated and removed; Heavy metal precipitator Heavy metal precipitator has strong chelating ability, can effectively react chemically with heavy metals to generate insoluble substances, and has good toxicological and biological properties and high operational safety.
[0005] CN110655160A discloses a preparation method for heavy metal capture gold, comprising: step 1, dissolving sodium polyacrylate in distilled water, then adding sodium alginate and ultrasonically stirring until completely dissolved to obtain a sodium alginate-sodium polyacrylate mixed solution; step 2, vacuum distilling the sodium polyacrylate dissolved solution to form a viscous liquid, then adding it to a mold and slightly heating it to solidify it into a spherical shape, then spraying the sodium alginate-sodium polyacrylate mixed solution on the surface of the sodium polyacrylate ball, and drying it at a constant temperature to form a microsphere structure; step 3, adding carbon disulfide and dimethylamine to anhydrous ethanol and stirring them evenly to form a viscous state, and then slowly injecting them into the center of the above-mentioned microspheres with a syringe to obtain a coated microsphere structure; step 4, dissolving calcium chloride in ethanol water to form a dilute solution, then spraying the dilute calcium chloride solution on the surface of the microspheres, and letting it stand to obtain coated microspheres; step 5, coating the surface of the coated microspheres with absorbent paper, letting it stand at a constant temperature for 2-4 hours, and removing it to obtain heavy metal capture microspheres.
[0006] The heavy metal capture agent prepared by this method achieves a rapid flocculation effect, prevents the residue of flocculant, and improves the treatment effect of heavy metals. However, it is greatly affected by the environment, has a poor adsorption effect on heavy metals in a low temperature environment, and has unstable adsorption performance for heavy metals. Summary of the invention
[0007] In order to solve the technical problems existing in the prior art, the present invention provides a heavy metal sedimentation agent and application thereof, which has a good adsorption effect on heavy metals and still has a good adsorption effect on heavy metals in a low temperature environment.
[0008] In view of the above technical problems, the present invention adopts the following technical solutions: A heavy metal sedimentation agent, comprising a dithiocarbamic acid modified compound and polyacrylamide; The mass ratio of the dithiocarbamic acid modified composite to polyacrylamide is 18.1:2.8; The preparation method of the dithiocarbamic acid modified composite is as follows: 1. Preparation of modified montmorillonite (1) Preliminary modification Mixing montmorillonite with deionized water, then adding stearic acid and polyvinyl pyrrolidone, and subjecting the mixture to ball milling treatment under ultrasonic action, wherein the ball milling medium is zirconium oxide ball, the ball milling speed is 175-188 rpm, the ultrasonic frequency is 55-60 kHz, the ultrasonic power is 134-144 W, the treatment time is 35-40 min, and drying is performed to obtain the preliminary modified montmorillonite; The particle size of the montmorillonite is 310-340nm, the mass content of SiO2 is 58.5-58.9%, and the mass content of Al2O3 is 14.2-14.5%; The mass ratio of the montmorillonite, deionized water, stearic acid and polyvinyl pyrrolidone is 15-19:116-125:1.3-1.6:1.6-2.0; (2) Secondary modification The preliminarily modified montmorillonite is placed in a sealed container, and then an ethanol solution and polyethylene glycol are introduced, after being stirred evenly, kH560 is added, the temperature is raised to 73-79°C at a rate of 1.0-1.5°C / min, the pressure is controlled to be 1.1-1.3MPa, and the reaction is stirred for 5.8-6.2h. After the stirring reaction is completed, the temperature is lowered to room temperature, filtered and dried to obtain the modified montmorillonite; The mass concentration of the ethanol solution is 40-44; The mass ratio of the primary modified montmorillonite, ethanol solution, polyethylene glycol and kH560 is 12-14:145-155:1.6-1.8:1.2-1.4.
[0009] 2. Grafting The modified montmorillonite is placed in N, N-dimethylformamide, ethylenediamine and polyethyleneimine are added, and after stirring evenly, formaldehyde guar gum is added, and ultrasonic treatment is performed. The ultrasonic time is 18-22 minutes, and the ultrasonic power is 124-135W. After the ultrasonic treatment, stirring reaction is carried out in a nitrogen atmosphere. The reaction temperature is 68-72°C, the reaction time is 6.4-6.6h, and the stirring speed is 115-124rpm. After the reaction is completed, filtering, washing, and drying are performed to obtain a composite; The mass volume ratio of the modified montmorillonite and N,N-dimethylformamide is 5.1-5.5 g:38.-420 mL; The mass ratio of the modified montmorillonite, ethylenediamine, polyethyleneimine and aldehyded guar gum is 5.1-5.5:6.0-6.4:4.5-4.9:3.5-3.7; The preparation method of the aldehyde-modified guar gum comprises the following steps: dissolving 6.8-7.2 g of guar gum in 90-94 g of deionized water, adding 12.5-13.2 g of hydrogen peroxide, stirring evenly and drying to obtain the aldehyde-modified guar gum.
[0010] 3. Dithiocarbamate reaction The complex is placed in a sodium hydroxide solution, mixed evenly, and then carbon disulfide is added dropwise under stirring, the dropping rate is controlled to be 1.0-1.4 mL / min, and the stirring speed is 137-146 rpm. After the addition is completed, the temperature is increased to 38-42° C. and stirred for reaction for 4.2-4.4 hours. After the reaction is completed, the dithiocarbamic acid modified complex is obtained by drying; The mass concentration of the sodium hydroxide solution is 28-32%; The mass ratio of the complex, sodium hydroxide solution and carbon disulfide is 9.6-10.3 g:364-375 mL:9.5-10.5 mL.
[0011] The invention discloses an application of a heavy metal precipitator in wastewater, wherein the addition amount of the heavy metal precipitator is 0.5 g / L.
[0012] Compared with the prior art, the present invention has achieved the following beneficial effects: 1. The present invention firstly performs a preliminary modification on montmorillonite. Under the action of ultrasonic-ball milling synergistic treatment, high-speed collisions occur between montmorillonites, resulting in lattice distortion and lattice defects inside, increasing the specific surface area of montmorillonite, enhancing the activity of montmorillonite, and making montmorillonite present a state of being dispersed alone. While increasing the specific surface area, the particle size distribution is more uniform, and the dispersion performance is improved. Then, secondary modification is performed to make the montmorillonite surface rich in epoxy groups. In the grafting step, the epoxy groups on the surface of montmorillonite react with the amino groups of ethylenediamine and polyethyleneimine through a ring-opening reaction, and the ethylenediamine and polyethyleneimine react with each other. The amino group of ethyleneimine can react with the aldehyde group of aldehyded guar gum, so that ethylenediamine, polyethyleneimine, montmorillonite and guar gum are firmly combined together to form a cross-linked network structure with large adsorption capacity and good stability. The surface contains abundant active sites such as primary amine, secondary amine and tertiary amine, which can chelate and adsorb heavy metal ions, thereby improving the adsorption and sedimentation performance of heavy metals. Finally, the heavy metal sedimentation agent modified with dithiocarbamic acid has good sedimentation performance and stability for heavy metals, and still has good heavy metal chelation ability at low temperature and stable sedimentation performance. 2. The heavy metal precipitator of the present invention controls the pH of wastewater to 4.2, the treatment temperature is 25°C, the nickel removal rate in wastewater is 98.33-98.75%, the chromium removal rate is 99.02-99.32%, the cobalt removal rate is 97.15-97.62%, the lead removal rate is 96.94-97.34%, the mercury removal rate is 95.99-96.58%, and the manganese removal rate is 96.14-96.65%; 3. The heavy metal precipitator of the present invention controls the pH value of wastewater to 4.2 and the treatment temperature to 5°C. The nickel removal rate in the wastewater is 94.40-96.58%, the chromium removal rate is 94.47-96.44%, the cobalt removal rate is 93.75-95.86%, the lead removal rate is 91.41-93.93%, the mercury removal rate is 91.19-92.72%, and the manganese removal rate is 92.68-94.23%. DETAILED DESCRIPTION
[0013] In order to more clearly understand the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described.
[0014] Example 1 A heavy metal sedimentation agent, comprising a dithiocarbamic acid modified compound and polyacrylamide; the mass ratio of the dithiocarbamic acid modified compound to the polyacrylamide is 18.3:3.1; The preparation method of the dithiocarbamic acid modified composite is as follows: 1. Preparation of modified montmorillonite (1) Preliminary modification 17 g of montmorillonite was mixed with 120 g of deionized water, and then 1.4 g of stearic acid and 1.8 g of polyvinyl pyrrolidone were added, and ball milling was performed under ultrasonic action. The ball milling medium was zirconium oxide balls, the ball milling speed was 180 rpm, the ultrasonic frequency was 57 kHz, the ultrasonic power was 140 W, the processing time was 37 min, and after drying, a preliminary modified montmorillonite was obtained; The particle size of the montmorillonite is 320 nm, the mass content of SiO2 is 58.7%, and the mass content of Al2O3 is 14.3%; (2) Secondary modification 13 g of the preliminary modified montmorillonite was placed in a sealed container, and then 150 g of ethanol solution and 1.7 g of polyethylene glycol were introduced, and after being stirred evenly, 1.3 g of kH560 was added, and the temperature was raised to 76 ° C at a rate of 1.2 ° C / min, and the pressure was controlled to be 1.2 MPa, and the reaction was stirred for 6.0 h. After the stirring reaction was completed, the temperature was lowered to room temperature, filtered and dried to obtain modified montmorillonite; The mass concentration of the ethanol solution is 42%.
[0015] 2. Grafting 5.3 g of modified montmorillonite was placed in 400 mL of N, N-dimethylformamide, 6.2 g of ethylenediamine and 4.7 g of polyethyleneimine were added, and after stirring, 3.6 g of aldehyded guar gum was added, and ultrasonic treatment was performed. The ultrasonic time was 20 min and the ultrasonic power was 130 W. After the ultrasonic treatment, stirring reaction was carried out in a nitrogen atmosphere. The reaction temperature was 70 ° C., the reaction time was 6.5 h, and the stirring speed was 120 rpm. After the reaction was completed, the composite was filtered, washed and dried to obtain a composite. The preparation method of the aldehyde-modified guar gum comprises the following steps: dissolving 7 g of guar gum in 92 g of deionized water, adding 13 g of hydrogen peroxide, stirring evenly and drying to obtain the aldehyde-modified guar gum.
[0016] 3. Dithiocarbamate reaction 10 g of the complex was placed in 370 mL of sodium hydroxide solution, mixed evenly, and then 10 mL of carbon disulfide was added dropwise under stirring, with the dropping rate controlled at 1.2 mL / min and the stirring speed at 142 rpm. After the addition was completed, the temperature was raised to 40° C. and stirred for reaction for 4.3 h. After the reaction was completed, the dithiocarbamic acid-modified complex was obtained by drying; The mass concentration of the sodium hydroxide solution is 30%.
[0017] Example 2 A heavy metal sedimentation agent, comprising a dithiocarbamic acid modified compound and polyacrylamide; the mass ratio of the dithiocarbamic acid modified compound to the polyacrylamide is 18.1:2.8; The preparation method of the dithiocarbamic acid modified composite is as follows: 1. Preparation of modified montmorillonite (1) Preliminary modification 15 g of montmorillonite was mixed with 116 g of deionized water, and then 1.3 g of stearic acid and 1.6 g of polyvinyl pyrrolidone were added, and ball milling was performed under ultrasonic action. The ball milling medium was zirconium oxide balls, the ball milling speed was 175 rpm, the ultrasonic frequency was 55 kHz, the ultrasonic power was 134 W, the processing time was 35 min, and after drying, a preliminary modified montmorillonite was obtained; The particle size of the montmorillonite is 310 nm, the mass content of SiO2 is 58.5%, and the mass content of Al2O3 is 14.2%; (2) Secondary modification 12g of the preliminary modified montmorillonite was placed in a sealed container, and then 145g of ethanol solution and 1.6g of polyethylene glycol were introduced, and after stirring evenly, 1.2g of kH560 was added, and the temperature was raised to 73°C at a rate of 1.0°C / min, and the pressure was controlled to be 1.1MPa, and the reaction was stirred for 5.8h. After the stirring reaction was completed, the temperature was lowered to room temperature, filtered and dried to obtain modified montmorillonite; The mass concentration of the ethanol solution is 40%.
[0018] 2. Grafting 5.1 g of modified montmorillonite was placed in 380 mL of N, N-dimethylformamide, 6.0 g of ethylenediamine and 4.5 g of polyethyleneimine were added, and after stirring, 3.5 g of aldehyded guar gum was added, and ultrasonic treatment was performed. The ultrasonic time was 18 min and the ultrasonic power was 124 W. After the ultrasonic treatment, stirring reaction was carried out in a nitrogen atmosphere. The reaction temperature was 68 ° C. The reaction time was 6.4 h and the stirring speed was 115 rpm. After the reaction was completed, the composite was filtered, washed and dried to obtain a composite. The preparation method of the aldehyde-modified guar gum comprises the following steps: dissolving 6.8 g of guar gum in 90 g of deionized water, adding 12.5 g of hydrogen peroxide, stirring evenly and drying to obtain the aldehyde-modified guar gum.
[0019] 3. Dithiocarbamate reaction 9.6 g of the complex was placed in 364 mL of sodium hydroxide solution, mixed evenly, and then 9.5 mL of carbon disulfide was added dropwise under stirring, with the dropping rate controlled at 1.0 mL / min and the stirring speed at 137 rpm. After the addition was completed, the temperature was raised to 38° C. and stirred for reaction for 4.2 h. After the reaction was completed, the dithiocarbamic acid-modified complex was obtained by drying; The mass concentration of the sodium hydroxide solution is 28%.
[0020] Example 3 A heavy metal sedimentation agent, comprising a dithiocarbamic acid modified compound and polyacrylamide; the mass ratio of the dithiocarbamic acid modified compound to the polyacrylamide is 18.5:3.3; The preparation method of the dithiocarbamic acid modified composite is as follows: 1. Preparation of modified montmorillonite (1) Preliminary modification 19 g of montmorillonite was mixed with 125 g of deionized water, and then 1.6 g of stearic acid and 2.0 g of polyvinyl pyrrolidone were added, and ball milling was performed under ultrasonic action. The ball milling medium was zirconia balls, the ball milling speed was 188 rpm, the ultrasonic frequency was 60 kHz, the ultrasonic power was 144 W, the processing time was 40 min, and after drying, a preliminary modified montmorillonite was obtained; The particle size of the montmorillonite is 340 nm, the mass content of SiO2 is 58.9%, and the mass content of Al2O3 is 14.5%; (2) Secondary modification 14 g of the preliminary modified montmorillonite was placed in a sealed container, and then 155 g of ethanol solution and 1.8 g of polyethylene glycol were introduced, and after stirring evenly, 1.4 g of kH560 was added, and the temperature was raised to 79 ° C at a rate of 1.5 ° C / min, and the pressure was controlled to be 1.3 MPa, and the reaction was stirred for 6.2 hours. After the stirring reaction was completed, the temperature was lowered to room temperature, filtered and dried to obtain modified montmorillonite; The mass concentration of the ethanol solution is 44%.
[0021] 2. Grafting 5.5 g of modified montmorillonite was placed in 420 mL of N, N-dimethylformamide, 6.4 g of ethylenediamine and 4.9 g of polyethyleneimine were added, and 3.7 g of aldehyded guar gum was added after stirring evenly, and ultrasonic treatment was performed. The ultrasonic time was 22 min and the ultrasonic power was 135 W. After the ultrasonic treatment, stirring reaction was carried out in a nitrogen atmosphere. The reaction temperature was 72 ° C. The reaction time was 6.6 h and the stirring speed was 124 rpm. After the reaction was completed, the composite was filtered, washed and dried to obtain a composite. The preparation method of the aldehyde-modified guar gum comprises the following steps: dissolving 7.2 g of guar gum in 94 g of deionized water, adding 13.2 g of hydrogen peroxide, stirring evenly and drying to obtain the aldehyde-modified guar gum.
[0022] 3. Dithiocarbamate reaction 10.3 g of the complex was placed in 375 mL of sodium hydroxide solution, mixed evenly, and then 10.5 mL of carbon disulfide was added dropwise under stirring, with the dropping rate controlled at 1.4 mL / min and the stirring speed at 146 rpm. After the addition was completed, the temperature was raised to 42° C. and stirred for reaction for 4.4 h. After the reaction was completed, the dithiocarbamic acid-modified complex was obtained by drying; The mass concentration of the sodium hydroxide solution is 32%.
[0023] Comparative Example 1 Based on Example 1, the changes are that the step of preparing modified montmorillonite is omitted, and in the grafting step, an equal amount of modified montmorillonite is replaced by montmorillonite, and the other operations are the same.
[0024] Comparative Example 2 Based on Example 1, the changes are as follows: In the grafting step, the aldehyded guar gum was replaced by guar gum in equal amounts; The grafting step is to mix 5.3g of modified montmorillonite, 6.2g of ethylenediamine and 4.7g of polyethyleneimine, add 3.6g of guar gum, and perform ultrasonic treatment. The ultrasonic time is 20min and the ultrasonic power is 130W. After the ultrasonic treatment, a composite is obtained; The rest of the operations are the same.
[0025] The raw wastewater of a factory has a pH of 4.2, a nickel content of 120 mg / L, a chromium content of 107 mg / L, a cobalt content of 30 mg / L, a lead content of 29 mg / L, a mercury content of 12.3 mg / L, and a manganese content of 5.4 mg / L.
[0026] Test Example 1 Take 5 samples of the factory's raw wastewater, each sample is 1000 mL, the sample temperature is 25°C, then add 0.5g of the heavy metal precipitator of Example 1-3 and Comparative Example 1-2 respectively, stir at 25°C and 500rpm for 3.0min, then test the heavy metal content in the wastewater, calculate the heavy metal removal rate, and the calculation results are as follows:
[0027] Test Example 2 Take 5 samples of the factory's raw wastewater, each sample is 1000 mL, the sample temperature is 5°C, then add 0.5g of the heavy metal precipitator of Example 1-3 and Comparative Example 1-2 respectively, stir at 5°C and 500rpm for 3.0min, then test the heavy metal content in the wastewater, calculate the heavy metal removal rate, and the calculation results are as follows:
[0028] The invention firstly performs a preliminary modification on montmorillonite, and under the action of ultrasonic-ball milling synergistic treatment, high-speed collision occurs between montmorillonites, so that lattice distortion and lattice defects are generated inside, the specific surface area of montmorillonite is increased, the activity of montmorillonite is enhanced, and the montmorillonite is in a state of being dispersed alone. While increasing the specific surface area, the particle size distribution is more uniform, and the dispersion performance is improved. Then, secondary modification is performed to make the montmorillonite surface rich in epoxy groups. In the grafting step, the epoxy groups on the surface of the montmorillonite undergo a ring-opening reaction with the amino groups of ethylenediamine and polyethyleneimine, and the ethylenediamine and polyethyleneimine react with each other. The amino group of ethyleneimine can react with the aldehyde group of aldehyded guar gum, so that ethylenediamine, polyethyleneimine, montmorillonite and guar gum are firmly combined together to form a cross-linked network structure with large adsorption capacity and good stability. The surface contains abundant active sites such as primary amines, secondary amines and tertiary amines, which chelate and adsorb heavy metal ions, thereby improving the adsorption and sedimentation performance of heavy metals. Finally, the heavy metal sedimentation agent modified with dithiocarbamic acid has good sedimentation performance for heavy metals and good stability. It still has good heavy metal chelating ability at low temperatures and stable sedimentation performance.
[0029] Comparative Example 1 omits the modification step of montmorillonite. Montmorillonite is easy to agglomerate, has a small specific surface area, and has poor adsorption capacity. In addition, in the grafting step, montmorillonite does not contain epoxy groups and cannot undergo a ring-opening reaction with amine compounds, thereby failing to form a stable cross-linked network structure. Ultimately, the prepared dithiocarbamic acid-modified composite has poor chelating ability for heavy metal ions and poor stability. Comparative Example 2 is only a physical mixture of modified montmorillonite, amine compounds and guar gum, which have poor binding ability and cannot form a stable cross-linked network structure, ultimately resulting in poor stability of the prepared dithiocarbamic acid modified composite and poor chelating ability for heavy metal ions.
[0030] Unless otherwise specified, all ratios and percentages described in the present invention are by mass ratios and percentages are by mass percentages.
[0031] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A heavy metal sedimentation agent, It is characterized in that The heavy metal sedimentation agent includes a dithiocarbamic acid modified compound and polyacrylamide; The preparation method of the dithiocarbamic acid modified composite comprises the steps of preparing modified montmorillonite, grafting and dithiocarbamate reaction; The modified montmorillonite comprises the steps of primary modification and secondary modification; The step of the initial modification is to mix montmorillonite with deionized water, then add stearic acid and polyvinyl pyrrolidone, and perform ball milling under ultrasonic action, wherein the ball milling medium is zirconium oxide balls, the ball milling speed is 175-188 rpm, the ultrasonic frequency is 55-60 kHz, the ultrasonic power is 134-144 W, the processing time is 35-40 min, and after drying, the primary modified montmorillonite is obtained; The secondary modification step is to place the primary modified montmorillonite in a sealed container, then introduce ethanol solution and polyethylene glycol, stir evenly, add kH560, heat to 73-79°C at a rate of 1.0-1.5°C / min, control the pressure to 1.1-1.3MPa, stir and react for 5.8-6.2h, and after the stirring reaction is completed, cool to room temperature, filter and dry to obtain modified montmorillonite; The grafting step comprises placing the modified montmorillonite in N,N-dimethylformamide, adding ethylenediamine and polyethyleneimine, stirring evenly, adding aldehyded guar gum, and performing ultrasonic treatment, wherein the ultrasonic time is 18-22 minutes, the ultrasonic power is 124-135W, and after the ultrasonic treatment, stirring reaction is performed in a nitrogen atmosphere, the reaction temperature is 68-72°C, the reaction time is 6.4-6.6h, and the stirring speed is 115-124rpm. After the reaction is completed, filtering, washing, and drying are performed to obtain a composite.
2. A heavy metal sedimentation agent according to claim 1, It is characterized in that The mass ratio of the dithiocarbamic acid modified composite to polyacrylamide is 18.1:2.
8.
3. A heavy metal sedimentation agent according to claim 1, It is characterized in that In the preliminary modification step, the particle size of the montmorillonite is 310-340nm, and the SiO 2 The mass content is 58.5-58.9%, Al 2 O 3 The mass content is 14.2-14.5%; The mass ratio of the montmorillonite, deionized water, stearic acid and polyvinyl pyrrolidone is 15-19:116-125:1.3-1.6:1.6-2.
0.
4. A heavy metal sedimentation agent according to claim 1, It is characterized in that In the step of secondary modification, the mass concentration of the ethanol solution is 40-44; The mass ratio of the primary modified montmorillonite, ethanol solution, polyethylene glycol and kH560 is 12-14:145-155:1.6-1.8:1.2-1.
4.
5. A heavy metal sedimentation agent according to claim 1, It is characterized in that In the grafting step, the mass volume ratio of the modified montmorillonite and N,N-dimethylformamide is 5.1-5.5 g:38.-420 mL; The mass ratio of the modified montmorillonite, ethylenediamine, polyethyleneimine and aldehyded guar gum is 5.1-5.5:6.0-6.4:4.5-4.9:3.5-3.
7.
6. A heavy metal sedimentation agent according to claim 1, It is characterized in that In the grafting step, the preparation method of the aldehyde-modified guar gum is as follows: 6.8-7.2 g of guar gum is dissolved in 90-94 g of deionized water, 12.5-13.2 g of hydrogen peroxide is added, the mixture is stirred evenly and then dried to obtain the aldehyde-modified guar gum.
7. A heavy metal sedimentation agent according to claim 1, It is characterized in that The steps of the dithiocarbamate reaction are as follows: placing the complex in a sodium hydroxide solution, mixing evenly, adding carbon disulfide dropwise under stirring, controlling the dropping rate to be 1.0-1.4 mL / min, and the stirring speed to be 137-146 rpm; after the addition is completed, raising the temperature to 38-42° C., stirring and reacting for 4.2-4.4 hours; after the reaction is completed, drying to obtain the dithiocarbamate modified complex.
8. A heavy metal sedimentation agent according to claim 7, It is characterized in that In the dithiocarbamate reaction step, the mass concentration of the sodium hydroxide solution is 28-32%; The mass ratio of the complex, sodium hydroxide solution and carbon disulfide is 9.6-10.3 g:364-375 mL:9.5-10.5 mL.
9. Use of the heavy metal sedimentation agent according to any one of claims 1 to 8, It is characterized in that The added amount of the heavy metal precipitant is 0.5 g / L.
Citation Information
Patent Citations
Preparation method of heavy metal trapping agent
CN110655160A
Cited By
Method for removing impurity metal cations in wet-process phosphoric acid
CN121247743A
A method for removing impurity metal cations from wet-process phosphoric acid
CN121247743B