Microcapsule for self-repairing concrete and preparation method thereof
By using microcapsules prepared with polyethylene wax, paraffin and nano-silica materials, diisocyanate compounds are used for self-repair, the problem of reducing durability caused by concrete cracks is solved, and the effect of rapid self-repair and strong adaptability is achieved , improves the crack resistance and service life of concrete.
Patent Information
- Application Number
- CN202411051464.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Concrete is prone to cracks during use, resulting in low tensile strength and reduced durability. Cracks provide channels for corrosive substances to penetrate, aggravate chemical corrosion and steel bar corrosion, shorten service life, and the existing self-repair technology is effective in humid environments. Poor or negatively affects mechanical properties.
Polyethylene wax, paraffin and nano-silica are used as wall materials and diisocyanate compounds are used as core materials. Microcapsules are prepared by melting, dispersion and condensation method, and microcapsules are obtained for self-healing concrete by ultrasonic dispersion and drying. The microcapsules are at the cracks. The core material is released by the crack and curing reaction for self-healing.
Based on the appropriate mechanical properties and sealing properties, rapid self-repair is achieved, making up for the shortcomings of the existing technology, adapt to a variety of environmental conditions, and improving the durability and service life of concrete.
Smart Images

Figure CN118930104A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of concrete repair materials, and in particular to a microcapsule for self-repairing concrete and a preparation method thereof. Background Art
[0002] Concrete has the advantages of low cost, easy use and good durability, and has become the most important building material. However, due to the inherent defects of concrete such as high brittleness and low tensile strength, cracks will inevitably appear during use, thereby reducing the strength of concrete and reducing the safety of buildings. At the same time, cracks will provide channels for corrosive substances in the environment to penetrate into the concrete, aggravating the chemical erosion of concrete and the corrosion of its internal steel bars, greatly shortening the service life of concrete. As concrete is increasingly used in special projects such as underground infrastructure, hydropower stations, and nuclear power plants, it is even more important to improve the durability of concrete. In order to extend the service life of buildings, reduce the difficulty of repair, and reduce maintenance costs, the self-repair technology of concrete has become a research hotspot in the scientific and engineering communities of various countries. Self-repair is a common phenomenon and function in organisms. The development of self-repairing concrete is not only a new way to realize the functionalization of traditional building materials, but also has important guiding significance for ensuring the long-term durability and service life of concrete structural engineering.
[0003] Cracks in concrete will affect the appearance and safety of buildings. As the depth of concrete cracks increases, the load capacity will decrease sharply. At the same time, cracks will become harmful ions in the environment (Cl - and SO4 2- The chemical corrosion of concrete and the corrosion of its internal steel bars will infiltrate into the channels inside the concrete, aggravating the chemical corrosion of concrete and the corrosion of its internal steel bars, resulting in reduced durability of concrete and greatly shortening the service life of concrete. Concrete buildings are generally believed to have a service life of 50 to 150 years. However, most building structures begin to show damage after more than ten years or even a few years of service. In the investigation of the service status of concrete structure buildings, it was found that for civil and public buildings with relatively good use environment, the service life can reach 50 years, but most industrial and open-air buildings need major repairs after 25 to 30 years of use. The time for buildings in harmful media is even shorter, only 15 to 20 years, so a lot of manpower and material resources are consumed every year for the maintenance of damaged concrete buildings.
[0004] Although a lot of research has been done on the self-repair of concrete cracks using technologies such as osmotic crystallization, microbial method, hollow fiber method and microcapsule method, the osmotic crystallization self-repair technology needs to be carried out in a humid environment and takes a long time to repair; microbial self-repair also needs to be carried out in a humid environment, and the presence of microorganisms and substrates has an adverse effect on the mechanical properties of concrete; hollow fiber self-repair technology is easy to break during the concrete mixing process and is difficult to apply. Compared with these self-repair technologies, microcapsule self-repair technology has the advantages of strong environmental adaptability and fast repair speed, and has good application prospects. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a microcapsule for self-repairing concrete and a preparation method thereof.
[0006] The technical solution provided by the present invention is as follows:
[0007] In a first aspect, the present invention provides a method for preparing microcapsules for self-repairing concrete, the preparation method comprising the following steps:
[0008] heating the wall material to obtain a liquid wall material;
[0009] The core material is added to the liquid wall material, heated and stirred, and then a cooling liquid is added and stirred continuously to obtain a microcapsule suspension;
[0010] Ultrasonic dispersion of the microcapsule suspension is performed, followed by filtration and drying to obtain the microcapsules for self-repairing concrete;
[0011] The wall material includes at least one of polyethylene wax, paraffin wax and nano silicon dioxide;
[0012] The core material includes a diisocyanate compound.
[0013] Furthermore, the wall material is composed of polyethylene wax, paraffin wax and nano silicon dioxide in a weight ratio of 5:5:1.
[0014] Furthermore, the diisocyanate compound includes toluene diisocyanate; and the particle size of the nano-silicon dioxide is 20 nm.
[0015] Furthermore, the coolant includes perfluorotributylamine.
[0016] Furthermore, the weight ratio of the wall material, the core material and the coolant is 1:2:5.
[0017] Furthermore, the temperature when the wall material was heated was 120° C., and the stirring speed was 60 rpm.
[0018] Furthermore, when the core material is added into the liquid wall material and heated and stirred, the temperature is 120° C. and the stirring speed is 800 rpm.
[0019] Furthermore, when the cooling liquid was added and the stirring was continued, the stirring speed was 800 rpm, and the cooling end point temperature was 20°C.
[0020] Furthermore, the working condition parameters of the ultrasonic dispersion include: ultrasonic power of 500W, and ultrasonic dispersion time of 30 minutes.
[0021] In a second aspect, the present invention provides a microcapsule for self-repairing concrete, wherein the microcapsule for self-repairing concrete is prepared by the preparation method described in any one of the first aspects.
[0022] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0023] The present invention provides a microcapsule for self-repairing concrete and a preparation method thereof. The present invention uses polyethylene wax, paraffin wax and nano-silicon dioxide as wall materials and diisocyanate compounds as core materials, and prepares microcapsules for self-repairing concrete with suitable mechanical properties, excellent sealing properties and good self-repairing effects through a melt-dispersion condensation method, thereby making up for the deficiencies of the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0026] Figure 1 Self-repairing mechanism of microcapsules for self-repairing concrete provided by the present invention Figure 1 .
[0027] Figure 2 Self-repairing mechanism of microcapsules for self-repairing concrete provided by the present invention Figure 2 .
[0028] Figure 3 This is a schematic diagram of the preparation process of paraffin-coated TDI microcapsules provided in Example 1 of the present invention.
[0029] Figure 4 Schematic diagram of the preparation process of TDI microcapsules coated with nano-silicon dioxide / paraffin / polyethylene wax composite wall material provided in Example 3 of the present invention.
[0030] Figure 5 The surface crack repair rate of the nano-silicon dioxide / paraffin / polyethylene wax composite wall material coated TDI microcapsules provided in Example 3 of the present invention at temperatures set to 10°C, 30°C, 50°C, and 60°C and a relative humidity of 50% RH; wherein, Figure 5 Figure a in the middle shows the surface crack repair rate at 10°C. Figure 5 Figure b in the middle shows the surface crack repair rate at 30°C. Figure 5 Figure c in the middle shows the surface crack repair rate at 50°C. Figure 5 Figure d in the middle shows the surface crack repair rate at 60°C.
[0031] Figure 6 The surface crack repair rate of the microcapsules provided in Example 1 of the present invention at temperatures of 10°C, 30°C, 50°C, and 60°C and a relative humidity of 50% RH; wherein, Figure 6 Figure a in the middle shows the surface crack repair rate at 10°C. Figure 6 Figure b in the middle shows the surface crack repair rate at 30°C. Figure 6 Figure c in the middle shows the surface crack repair rate at 50°C. Figure 6 Figure d in the middle shows the surface crack repair rate at 60°C.
[0032] Figure 7 The surface crack repair rate of the microcapsules provided in Example 2 of the present invention at temperatures of 10°C, 30°C, 50°C, and 60°C and a relative humidity of 50% RH; wherein, Figure 7 Figure a in the middle shows the surface crack repair rate at 10°C. Figure 7 Figure b in the middle shows the surface crack repair rate at 30°C. Figure 7 Figure c in the middle shows the surface crack repair rate at 50°C. Figure 7 Figure d in the middle shows the surface crack repair rate at 60°C.
[0033] Figure 8 SEM image of TDI microcapsules coated with nano-silicon dioxide / paraffin / polyethylene wax composite wall material provided in Example 3 of the present invention Figure 1 .
[0034] Fig. 9 SEM image of TDI microcapsules coated with nano-silicon dioxide / paraffin / polyethylene wax composite wall material provided in Example 3 of the present invention Figure 2 .
[0035] Fig.10 SEM image of TDI microcapsules coated with nano-silicon dioxide / paraffin / polyethylene wax composite wall material provided in Example 3 of the present invention Figure 3 . DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0038] In a first aspect, the present invention provides a method for preparing microcapsules for self-repairing concrete, the preparation method comprising the following steps:
[0039] heating the wall material to obtain a liquid wall material;
[0040] The core material is added to the liquid wall material, heated and stirred, and then a cooling liquid is added and stirred continuously to obtain a microcapsule suspension;
[0041] Ultrasonic dispersion of the microcapsule suspension is performed, followed by filtration and drying to obtain the microcapsules for self-repairing concrete;
[0042] The wall material includes at least one of polyethylene wax, paraffin wax and nano silicon dioxide;
[0043] The core material includes a diisocyanate compound.
[0044] The present invention provides a method for preparing microcapsules for self-repairing concrete. The present invention uses polyethylene wax, paraffin wax and nano-silicon dioxide as wall materials and diisocyanate compounds as core materials, and prepares microcapsules for self-repairing concrete with suitable mechanical properties, excellent sealing properties and good self-repairing effects through a melt-dispersion condensation method, thereby making up for the deficiencies of the prior art.
[0045] The self-repairing mechanism of the microcapsules for self-repairing concrete provided by the present invention is shown in the figure Figure 1 and Figure 2 As shown in the figure, the process includes the following: Toluene diisocyanate (TDI) has a very low viscosity (20°C, 3.2 mPa·s), and isocyanate is highly reactive with compounds containing active hydrogen (such as water). When subjected to stress at the crack tip, the microcapsules rupture to release the TDI core material, which easily penetrates into the crack due to its low viscosity and reacts with the water or moisture in the crack to cure, thus healing the damage and cracks in the concrete without the addition of a curing agent.
[0046] In some specific embodiments, the wall material is composed of polyethylene wax, paraffin wax and nano silicon dioxide in a weight ratio of 5:5:1.
[0047] In some specific embodiments, the physical and chemical property parameters of the polyethylene wax include: a molecular weight of 3000-5000.
[0048] In some specific embodiments, the diisocyanate compound includes toluene diisocyanate, referred to as TDI; the particle size of the nano-silicon dioxide is 300 Å to 500 Å.
[0049] In some specific embodiments, the cooling liquid includes perfluorotributylamine.
[0050] In some specific embodiments, the weight ratio of the wall material, the core material and the coolant is 1:2:5.
[0051] In some specific embodiments, the wall material is heated at a temperature of 120° C. and a stirring speed of 600 rpm.
[0052] In some specific embodiments, the temperature when the core material is added into the liquid wall material and heated and stirred is 120° C. and the stirring speed is 800 rpm.
[0053] In some specific embodiments, the stirring speed when the cooling liquid is added and the stirring is continued is 800 rpm, and the cooling end point temperature is 20°C.
[0054] In some specific embodiments, the working condition parameters of the ultrasonic dispersion include: ultrasonic power of 500W, and ultrasonic dispersion time of 30 minutes.
[0055] In a second aspect, based on the same inventive concept, the present invention provides a microcapsule for self-repairing concrete, wherein the microcapsule for self-repairing concrete is prepared by the preparation method described in any one of the first aspects.
[0056] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0057] Example 1
[0058] This example provides a microcapsule for self-repairing concrete, specifically a paraffin-coated TDI microcapsule made of paraffin as the wall material, such as Figure 3 As shown, the preparation method includes the following steps:
[0059] Step (1): heating paraffin wax at 75° C. to obtain a liquid wall material;
[0060] Step (2): adding the core material (specifically TDI) to the liquid wall material obtained in step (1) and heating and stirring at a temperature of 75° C. and a stirring speed of 600 rpm, then adding a coolant (specifically perfluorotributylamine) and continuing stirring at a stirring speed of 600 rpm, and cooling to 20° C. to obtain a microcapsule suspension; wherein the weight ratio of the wall material, the core material and the coolant is 1:2:5;
[0061] Step (3): pour the microcapsule suspension obtained in step (2) into a beaker and oscillate with ultrasound at an ultrasonic power of W for 30 minutes; then filter out the microcapsules and dry them in a vacuum oven at 40° C. for 24 hours to obtain the microcapsules for self-repairing concrete.
[0062] Example 2
[0063] This example provides a microcapsule for self-repairing concrete, specifically a paraffin wax / polyethylene wax composite wall material coated TDI microcapsule made of a wall material composed of paraffin wax and polyethylene wax in a weight ratio of 1:1, and the preparation method thereof includes the following process:
[0064] Step (1): heating polyethylene wax at 120° C. to prepare liquid polyethylene wax, then adding paraffin wax at 120° C. and continuing to stir to obtain liquid wall material;
[0065] Step (2): adding the core material (specifically TDI) to the liquid wall material obtained in step (1) and heating and stirring at a temperature of 120° C. and a stirring speed of 800 rpm, then adding a coolant (specifically perfluorotributylamine) and continuing stirring at a stirring speed of 800 rpm, and cooling to 20° C. to obtain a microcapsule suspension; wherein the weight ratio of the wall material, the core material and the coolant is 1:2:5;
[0066] Step (3): pour the microcapsule suspension obtained in step (2) into a beaker and oscillate it with ultrasound at an ultrasonic power of 500 W for 30 minutes; then filter out the microcapsules and dry them in a vacuum oven at 40° C. for 24 hours to obtain the microcapsules for self-repairing concrete.
[0067] Example 3
[0068] This example provides a microcapsule for self-repairing concrete, specifically a nano-silicon dioxide / paraffin / polyethylene wax composite wall material coated with TDI microcapsule made of a wall material composed of polyethylene wax, paraffin wax and nano-silicon dioxide in a weight ratio of 5:5:1, such as Figure 4 As shown, the preparation method includes the following steps:
[0069] Step (1): heating polyethylene wax at 120° C. to prepare liquid polyethylene wax, then adding paraffin wax at 120° C. and continuing to stir to obtain a paraffin wax / polyethylene wax mixture; finally adding nano-silicon dioxide at 120° C. and continuing to stir to obtain a liquid wall material;
[0070] Step (2): adding the core material (specifically TDI) to the liquid wall material obtained in step (1) and heating and stirring at a temperature of 120° C. and a stirring speed of 800 rpm, then adding a coolant (specifically perfluorotributylamine) and continuing stirring at a stirring speed of 800 rpm, and cooling to 20° C. to obtain a microcapsule suspension; wherein the weight ratio of the wall material, the core material and the coolant is 1:2:5;
[0071] Step (3): pour the microcapsule suspension obtained in step (2) into a beaker and oscillate it with ultrasound at an ultrasonic power of 500 W for 30 minutes; then filter out the microcapsules and dry them in a vacuum oven at 40° C. for 24 hours to obtain the microcapsules for self-repairing concrete.
[0072] Test Case
[0073] In this example, the self-repairing concrete microcapsules provided in Examples 1 to 3 were used for performance testing.
[0074] Test method: According to the weight ratio in Table 1, the solid components were stirred in a mortar mixer for 90 seconds, and then water was added and stirred for 90 seconds to prepare cement mortar; then the cement mortar was poured into molds with sizes of 70.7mm×70.7mm×70.7mm and φ100mm×200mm, respectively, and the molds were removed after 24 hours, and the molds were moved into a standard curing room (20±2℃, 95% relative humidity) for curing for 28 days; the cement mortar test blocks after standard curing for 28 days were taken out and placed in a QZ-27 constant temperature and humidity chamber (Dongguan Qinzhuo Environmental Testing Equipment Co., Ltd., China). The temperatures were set to 10℃, 30℃, 50℃, and 60℃, and the relative humidity was 50%RH, respectively, to test the surface crack repair effect of the cement mortar test blocks.
[0075] Table 1
[0076] Sample No. cement water sand Microcapsules AM0 100 50 300 - AM1 100 50 300 3 (Example 1) AM2 100 50 300 3 (Example 2) AM3 100 50 300 3 (Example 3)
[0077] Compared with the AM0 sample (without adding microcapsules), the AM1 sample (using the microcapsules prepared in Example 1) and the AM2 sample (using the microcapsules prepared in Example 2), the AM3 sample using the microcapsules for self-repairing concrete provided in Example 3 of the present invention has the best surface crack repair effect. Figure 5 , Figure 6 , Figure 7 As shown by Figure 5 , Figure 6 and Figure 7 It can be seen that compared with paraffin wall microcapsules or paraffin / polyethylene wax composite wall microcapsules, nano-silica / paraffin / polyethylene wax composite wall microcapsules have higher core material content and sealing performance, ensuring that more TDI can participate in the self-healing reaction to generate solidified products to heal cracks, thereby improving the crack self-healing performance of cement mortar.
[0078] In addition, the SEM image of the microcapsules for self-repairing concrete provided in Example 3 of the present invention is as follows: Figure 8 , Fig. 9 and Fig.10 shown.
[0079] In summary, the present invention provides a self-repairing concrete microcapsule and a preparation method thereof. By using a specific proportion of an organic phase change medium, kaolin and hydrotalcite for use in combination, the phase change enthalpy of the organic phase change medium is effectively improved, and a self-repairing concrete microcapsule is successfully prepared, which further broadens the application scope of existing self-repairing concrete microcapsules and has broad practical application value.
[0080] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0081] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing microcapsules for self-repairing concrete, characterized in that: The preparation method comprises the following steps: heating the wall material to obtain a liquid wall material; The core material is added to the liquid wall material, heated and stirred, and then a cooling liquid is added and stirred continuously to obtain a microcapsule suspension; Ultrasonic dispersion of the microcapsule suspension is performed, followed by filtration and drying to obtain the microcapsules for self-repairing concrete; The wall material includes at least one of polyethylene wax, paraffin wax and nano silicon dioxide; The core material includes a diisocyanate compound.
2. The method for preparing the self-repairing concrete microcapsule according to claim 1, characterized in that: The wall material is composed of polyethylene wax, paraffin wax and nano silicon dioxide in a weight ratio of 5:5:
1.
3. The method for preparing microcapsules for self-repairing concrete according to claim 1, characterized in that: The diisocyanate compound includes toluene diisocyanate; and the particle size of the nano-silicon dioxide is 20 nm.
4. The method for preparing microcapsules for self-repairing concrete according to claim 1, characterized in that: The cooling liquid includes perfluorotributylamine.
5. The method for preparing microcapsules for self-repairing concrete according to claim 1, characterized in that: The weight ratio of the wall material, the core material and the coolant is 1:2:
5.
6. The method for preparing microcapsules for self-repairing concrete according to claim 1, characterized in that: The temperature when the wall material was heated was 120° C., and the stirring rotation speed was 600 rpm.
7. The method for preparing microcapsules for self-repairing concrete according to claim 1, characterized in that: The core material was added into the liquid wall material and heated and stirred at a temperature of 120° C. and a stirring speed of 800 rpm.
8. The method for preparing microcapsules for self-repairing concrete according to claim 1, characterized in that: The stirring speed when adding the coolant and continuing stirring was 800 rpm, and the cooling end point temperature was 20°C.
9. The method for preparing microcapsules for self-repairing concrete according to claim 1, characterized in that: The working condition parameters of the ultrasonic dispersion include: ultrasonic power of 500W and ultrasonic dispersion time of 30 minutes.
10. A microcapsule for self-repairing concrete, characterized in that: The microcapsules for self-repairing concrete are prepared by the preparation method according to any one of claims 1 to 9.