High-precision ceramic 3D printing slurry as well as preparation method and application thereof
By using specific formulas of high-precision ceramic 3D printing slurry and preparation methods in ceramic 3D printing, the problem of high absorption of light and insufficient curing depth of ceramic slurry is solved, and high-precision ceramic 3D printing molding and improvement are achieved The accuracy and strength of the product are eliminated and the risk of cracking is avoided.
Patent Information
- Application Number
- CN202411427008.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In ceramic 3D printing, the high absorption of light by existing slurries leads to overflow of light, insufficient curing depth, affecting printing accuracy and product intensity, and it is difficult to completely discharge the photosensitive resin during degreasing, increasing the risk of cracking.
Using high-precision ceramic 3D printing slurry, including ceramic powder, photosensitive resin, dispersant, ultraviolet absorber, composite plasticizer and curing accelerator, prepared by vacuum defoaming and ball mill mixing, combined with segmented degreasing technology, optimized formula The component ratio is to reduce the light absorption amount and increase the curing depth to ensure the smooth discharge of the photosensitive resin.
It effectively reduces the spillover phenomenon of light, improves the efficiency of light energy utilization and curing depth, avoids the problems of low intensity and cracking caused by insufficient curing, and achieves high-precision photocuring 3D printing molding and mass production quality improvement.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the field of 3D printing slurry, and in particular to a high-precision ceramic 3D printing slurry and a preparation method and application thereof. Background Art
[0002] Ceramic materials have the characteristics of high hardness and brittleness, which makes the processing of ceramics very difficult. Ceramic 3D printing, as an additive manufacturing technology, can be printed and manufactured according to the three-dimensional design model of the product. It has a high degree of design freedom and has become a better method for preparing complex shapes. The methods of ceramic 3D printing include laser selective sintering, fused deposition modeling, direct writing, inkjet printing, photocuring, etc. However, the products printed by laser selective sintering, fused deposition modeling and direct writing have the disadvantages of poor precision and poor density. The inkjet printing method has the disadvantages of easy sedimentation of product ink and easy clogging of nozzles in the process of printing products. In the process of printing products, photocuring has the advantages of high precision and easy batch production, and has become the main production method for high-precision ceramic molding. However, traditional ceramic slurry often faces the following key problems in the process of 3D printing photocuring, which limits its further application and promotion.
[0003] First, the ceramic slurry needs to use light curing technology during the 3D printing process, that is, using a light source of a specific wavelength to irradiate the ceramic slurry to cause the photosensitive resin component in it to undergo a curing reaction. However, existing ceramic slurries often have a high absorption of light, which not only leads to low efficiency in light energy utilization, but also easily causes light spillover, affecting printing accuracy and molding quality. Light spillover will not only cause unnecessary curing at the edge of the print, but may also interfere with the printing process in adjacent areas, causing shape distortion or poor interlayer bonding.
[0004] Secondly, the control of curing depth during the photocuring process is particularly critical. Insufficient curing depth will weaken the bonding between the printed layers, thus affecting the strength and stability of the entire printed product. In ceramic slurries, due to the complex composition, photosensitive resin content and property differences, it is often difficult to obtain the ideal curing depth, which in turn leads to the problem of low product strength.
[0005] Finally, the photosensitive resin acts as a temporary support during the printing process, but if it is not completely discharged during the degreasing stage, the failure of the photosensitive resin to be discharged means that the degreasing process may not be complete. Incomplete degreasing will result in a large amount of organic residue inside the ceramic green body. These organics will rapidly pyrolyze at high temperatures, producing a large amount of gas and volatile substances, thereby forming pores and cracks inside the green body. These residual photosensitive resins will significantly reduce the strength and stability of the support structure. The weakening of the support structure will make it unable to provide sufficient support during the sintering process, thereby increasing the risk of cracking.
[0006] The disclosure of the above background technology content is only used to assist in understanding the inventive concept and technical solution of the present invention. It does not necessarily belong to the prior art of this patent application, nor does it necessarily provide technical guidance. In the absence of clear evidence that the above content has been disclosed before the filing date of this patent application, the above background technology should not be used to evaluate the novelty and creativity of the present application. Summary of the invention
[0007] In order to solve the technical problems that the existing ceramic slurry often absorbs a high amount of light and easily causes light spillover, the curing depth during light curing is insufficient to cause low product strength, and the photosensitive resin fails to be discharged during the degreasing stage to increase the risk of cracking, the present invention proposes a high-precision ceramic 3D printing slurry and a preparation method and application thereof, which not only effectively reduces the ceramic slurry's absorption of light and reduces the light spillover phenomenon, thereby improving the efficiency of light energy utilization during printing and ensuring the curing width, but also ensures the curing depth at the same time, thereby avoiding the problem of low strength of printed products caused by insufficient curing; and is conducive to the formation of degreasing channels in the degreasing stage, so that the photosensitive resin is smoothly discharged, avoiding the problem of product cracking; realizes high-precision light-curing 3D printing molding, and improves the product precision and the quality of mass production.
[0008] In order to achieve the above object, the technical solution of the present invention is as follows: In one aspect, the present invention provides a high-precision ceramic 3D printing slurry, comprising the following components: Ceramic powder; Photosensitive resin; Dispersants; UV absorbers; A composite plasticizer, wherein the composite plasticizer comprises any of polyethylene glycol 200, polyethylene glycol 400, polypropylene glycol 400, dibutyl phthalate and dioctyl phthalate; Hydrogen abstraction type photoinitiator; The curing accelerator includes any one or more of triethylamine, triethanolamine and organic tertiary amine compounds.
[0009] The present invention proposes a high-precision ceramic 3D printing slurry and a preparation method and application thereof, which not only effectively reduces the amount of light absorbed by the ceramic slurry and reduces the light spillover phenomenon, thereby improving the light energy utilization efficiency in the printing process and ensuring the curing width, but also ensuring the curing depth, thereby avoiding the problem of low strength of the printed product due to insufficient curing; and is conducive to the formation of degreasing channels in the degreasing stage, so that the photosensitive resin can be discharged smoothly, avoiding the problem of product cracking; realizes high-precision light-curing 3D printing molding, and improves the product precision and the quality of mass production.
[0010] As a preferred technical solution, the weight ratio of the ceramic powder, the photosensitive resin, the dispersant, the ultraviolet absorber, the composite plasticizer, the hydrogen abstraction photoinitiator and the curing accelerator is (6.25-4): (0.6-0.5): (0.125-0.09): (0.013-0.008): (0.4-0.3): (0.015-0.008): (0.012-0.007).
[0011] As a preferred technical solution, the ceramic powder includes any one or more of zirconia, alumina, zirconia toughened alumina ceramics and alumina toughened zirconia ceramics.
[0012] As a preferred technical solution, the photosensitive resin includes any of isobornyl acrylate, 1,6-hexanediol diacrylate, iminodiacetic acid, trimethylolpropane triacrylate and ethoxylated pentaerythritol tetraacrylate.
[0013] As a preferred technical solution, the ultraviolet absorber includes: any one or more of N-(2-ethoxyphenyl)-N'-(2-ethylphenyl)-oxalamide, 2-(2'-hydroxy-3', 5'-di-tert-butylphenyl)-5-chlorobenzotriazole), [2-hydroxy-4-(octyloxy)phenyl]phenyl ketone and benzotriazole ultraviolet absorbers; The dispersant includes: any one or more of dispersant BYK110, dispersant BYK218, dispersant BYK111, and dispersant KOS110.
[0014] As a preferred technical solution, the hydrogen abstraction type photoinitiator includes any one or more of benzophenone, 4,4'-di(N,N-dimethylamino)benzophenone, isopropylthioxanthone, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone and 4-dimethylamino-ethyl benzoate.
[0015] On the other hand, the present invention provides a method for preparing a high-precision ceramic 3D printing slurry, which prepares the high-precision ceramic 3D printing slurry as described in any one of the above items, comprising the following steps: S1: weighing a photosensitive resin, a dispersant, an ultraviolet absorber, a composite plasticizer, a hydrogen abstraction type photoinitiator and a curing accelerator according to a weight ratio, adding them into a vacuum degassing machine, and mixing them at a speed of 500 to 2000 rpm for 2 to 10 minutes to obtain a mixture; S2: adding the obtained mixture and the ceramic powder weighed according to the weight ratio into a ball mill, and mixing at a speed of 100 to 300 rpm for 5 to 12 hours to obtain a premixed slurry; S3 vacuum degasses the premixed slurry to obtain high-precision ceramic 3D printing slurry.
[0016] As a preferred technical solution, the vacuum defoaming time of the premixed slurry in step S3 is 10 to 30 minutes.
[0017] On the other hand, according to the application of the high-precision ceramic 3D printing slurry in 3D printed products as described in any of the above items, the high-precision ceramic 3D printing slurry is solidified layer by layer by a ceramic 3D printer to form a ceramic green body, and the ceramic green body is degreased in sections.
[0018] As a preferred technical solution, the temperature of the segmented degreasing is ≤600°C, and the rate of the segmented degreasing is 0.1-1°C / min.
[0019] The present invention provides a high-precision ceramic 3D printing slurry and a preparation method and application thereof, which have the following beneficial effects: 1) It not only effectively reduces the amount of light absorbed by the ceramic slurry and reduces the light spillover phenomenon, thereby improving the efficiency of light energy utilization during the printing process and ensuring the curing width, but also ensures the curing depth, thereby avoiding the problem of low strength of the printed product due to insufficient curing; and it is conducive to the formation of degreasing channels in the degreasing stage, so that the photosensitive resin can be discharged smoothly, avoiding the problem of product cracking; it realizes high-precision light-curing 3D printing, improving the product precision and the quality of mass production; 2) The addition of UV absorber can absorb part of the UV light, which can not only reduce the demand for curing light and improve light sensitivity, but also ensure the curing width and depth of the product and improve the accuracy of the product; However, adding only UV absorber will lead to weaker curing of the product, poor green strength of ceramic molding, and poor three-point bending strength. Therefore, it needs to be compounded with curing accelerator. The added curing accelerator combined with hydrogen abstraction type photoinitiator can effectively inhibit the oxygen inhibition effect of photocuring, effectively reduce the amount of light absorbed by the ceramic slurry, reduce the light spillover phenomenon, ensure the curing width, and improve the curing efficiency. The curing accelerator is preferably any one or more of triethylamine, triethanolamine and organic tertiary amine compounds. Tertiary amines can reduce the quenching effect of oxygen molecules, and can quickly terminate peroxyl radicals to generate α-amine radicals that can effectively initiate monomer polymerization, thereby promoting the curing reaction. Amines, as oxygen donors, are deprived of α-H by free radicals to generate α-amine radicals that are more likely to combine with triplet oxygen to form peroxyl radicals, consuming oxygen to reduce the reaction between oxygen and chain free radicals, thereby promoting the curing reaction. The composite plasticizer is preferably any of polyethylene glycol 200, polyethylene glycol 400, polypropylene glycol 400, dibutyl phthalate and dioctyl phthalate. Since different types of multiple plasticizers are compounded, the decomposition temperatures of each plasticizer in the thermal degreasing stage are different, and the first degreasing part of the composite plasticizer will form a degreasing channel, which is beneficial to the discharge of subsequent resin and avoids cracking of the product. By purposefully selecting and compounding the formula components in the present application, not only is the amount of light absorbed by the ceramic slurry effectively reduced, the light spillover phenomenon is reduced, thereby improving the efficiency of light energy utilization during the printing process and ensuring the curing width, but also ensuring the curing depth, thereby avoiding the problem of low strength of the printed product due to insufficient curing; and in the degreasing stage, it is conducive to the formation of degreasing channels, so that the photosensitive resin can be discharged smoothly, avoiding the problem of product cracking; high-precision light-curing 3D printing is achieved, and the product precision and mass production quality are improved.
[0020] 3) Optimizing the ratio of the formula components, preferably the weight of the composite plasticizer accounts for 30%-40% of the weight of the high-precision ceramic 3D printing slurry. Optimizing the weight ratio of the composite plasticizer can effectively avoid the problem of product cracking after degreasing and sintering, and improve the three-point bending strength; 4) The composite plasticizer is preferably any of polyethylene glycol 200, polyethylene glycol 400, polypropylene glycol 400, dibutyl phthalate and dioctyl phthalate. The composite plasticizer has a long carbon chain and polar groups (such as ester groups and hydroxyl groups). These groups interact with the photosensitive resin of the polymer chain in the slurry, thereby reducing the viscosity of the slurry system and making the slurry have better fluidity. Different types of plasticizers are used to work synergistically to improve the flexibility of the photosensitive resin in the slurry and improve the three-point bending strength. DETAILED DESCRIPTION
[0021] The preferred embodiments of the present invention are described in detail below.
[0022] The manufacturers of dispersant BYK110, dispersant BYK218 and dispersant BYK111 in the present invention are all BYK Chemical, and the manufacturer of dispersant KOS110 is Guangzhou Kang Oushuang Trading Co., Ltd.
[0023] The organic tertiary amine compound in Example 2 of the present invention is specifically an organic tertiary amine P115 C20H 31 O6N (tertiary amine accelerator containing reactive groups), the manufacturer is Nanjing Jiazhong Chemical Technology Co., Ltd.
[0024] The present invention provides a high-precision ceramic 3D printing slurry, comprising the following components: Ceramic powder; Photosensitive resin; Dispersants; Ultraviolet absorber, the ultraviolet absorber includes: any one or more of N-(2-ethoxyphenyl)-N'-(2-ethylphenyl)-oxalamide (ultraviolet absorber UV321), 2-(2'-hydroxy-3', 5'-di-tert-butylphenyl)-5-chlorobenzotriazole (ultraviolet absorber UV327), [2-hydroxy-4-(octyloxy)phenyl]phenyl ketone (ultraviolet absorber UV531) and benzotriazole ultraviolet absorber (ultraviolet absorber UV329); A composite plasticizer, wherein the composite plasticizer comprises any of polyethylene glycol 200 (PEG200), polyethylene glycol 400 (PEG400), polypropylene glycol 400 (PPG400), dibutyl phthalate (DBP) and dioctyl phthalate (DOP); Hydrogen abstraction type photoinitiator; A curing accelerator, wherein the curing accelerator comprises any one or more of triethylamine, triethanolamine and organic tertiary amine compounds; The present invention proposes a high-precision ceramic 3D printing slurry, which not only effectively reduces the amount of light absorbed by the ceramic slurry and reduces the light spillover phenomenon, thereby improving the light energy utilization efficiency in the printing process and ensuring the curing width, but also ensures the curing depth, thereby avoiding the problem of low strength of the printed product due to insufficient curing; and is conducive to the formation of degreasing channels in the degreasing stage, so that the photosensitive resin can be discharged smoothly, avoiding the problem of product cracking; realizes high-precision light-curing 3D printing molding, and improves the product precision and the quality of mass production.
[0025] Preferably, the weight ratio of the ceramic powder, the photosensitive resin, the dispersant, the ultraviolet absorber, the composite plasticizer, the hydrogen abstraction photoinitiator and the curing accelerator is (6.25-4): (0.6-0.5): (0.125-0.09): (0.013-0.008): (0.4-0.3): (0.015-0.008): (0.012-0.007), and the weight of the composite plasticizer accounts for 30%-40% of the weight of the high-precision ceramic 3D printing slurry.
[0026] Preferably, the ceramic powder includes any one or more of zirconia, alumina, zirconia-toughened alumina ceramics, and alumina-toughened zirconia ceramics.
[0027] Preferably, the photosensitive resin includes any of isobornyl acrylate (IBOA), 1,6-hexanediol diacrylate (HDDA), iminodiacetic acid (IDA), trimethylolpropane triacrylate (TMPTA), and ethoxylated pentaerythritol tetraacrylate (PPTTA).
[0028] Preferably, the dispersant includes: any one or more of dispersant BYK110, dispersant BYK218, dispersant BYK111, and dispersant KOS110.
[0029] Preferably, the hydrogen abstraction type photoinitiator includes any one or more of benzophenone (BP), 4,4'-di(N,N-dimethylamino)benzophenone (MK), isopropylthioxanthone (ITX), 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone (907) and 4-dimethylamino-ethyl benzoate (EDB).
[0030] The present invention provides a method for preparing a high-precision ceramic 3D printing slurry, and the high-precision ceramic 3D printing slurry as described in any one of the above items is prepared, comprising the following steps: S1: weighing a photosensitive resin, a dispersant, an ultraviolet absorber, a composite plasticizer, a hydrogen abstraction type photoinitiator and a curing accelerator according to a weight ratio, adding them into a vacuum degassing machine, and mixing them at a speed of 500 to 2000 rpm for 2 to 10 minutes to obtain a mixture; S2: adding the obtained mixture and the ceramic powder weighed according to the weight ratio into a ball mill, and mixing at a speed of 100 to 300 rpm for 5 to 12 hours to obtain a premixed slurry; S3 vacuum degasses the premixed slurry for 10 to 30 minutes to obtain a high-precision ceramic 3D printing slurry.
[0031] According to the application of the high-precision ceramic 3D printing slurry in 3D printed products described in any of the above items, the high-precision ceramic 3D printing slurry is solidified layer by layer by a ceramic 3D printer to form a ceramic green body, and the ceramic green body is degreased in sections; the temperature of the sectioned degreasing is ≤600°C, and the rate of the sectioned degreasing is 0.1-1°C / min.
[0032] The printing accuracy of 3D printed products is mainly reflected by the curing width of the product. Under the premise of ensuring a certain curing depth of the product, the curing width of the product should be reduced as much as possible to improve the accuracy of the product. The Beer-Lambert law shows that the curing depth Cd is as follows:
[0033] In the formula, C d is the solidification thickness, in μm; D p is the penetration depth in μm; E is the exposure energy in mJ / cm 2 ; E c is the critical exposure energy, in mJ / cm 2 ; The curing width is based on the following:
[0034] In the formula, C w is the curing width, in μm; w0 is the laser radius, in μm; C d is the solidification thickness, in μm; D p is the penetration depth in μm; UV laser has a smaller laser radius, but the addition of ceramic powder causes light scattering, which causes the propagation direction of light to change from vertical to horizontal when UV irradiates the slurry, resulting in a larger curing width. The curing decay of ceramics is mainly affected by the following:
[0035] Where S is the scattering factor, in μm -1 ; A is the absorption influence factor of the initiator and absorber, in μm -1 ; φ is the volume fraction, unit is vol%; The addition of UV absorber can absorb part of the UV light, which can not only reduce the demand for curing light and improve light sensitivity, but also ensure the curing width and depth of the product and improve the accuracy of the product; However, adding only UV absorber will lead to weaker curing of the product, poor green strength of ceramic molding, and poor three-point bending strength. Therefore, it needs to be compounded with curing accelerator. The added curing accelerator combined with hydrogen abstraction type photoinitiator can effectively inhibit the oxygen inhibition effect of photocuring, effectively reduce the amount of light absorbed by the ceramic slurry, reduce the light spillover phenomenon, and improve the curing efficiency. The hydrogen abstraction type photoinitiator has an aromatic ketone structure. After absorbing light energy, it reacts with the amine curing accelerator in a bimolecular manner. The nitrogen atom in the curing accelerator loses an electron due to the excited hydrogen abstraction type initiator. The hydrogen on the α-C adjacent to the nitrogen becomes acidic and easily loses a proton to form active amine free radicals centered on C. These free radicals have high reactivity and can quickly undergo polymerization reactions with monomers. After formation, the active amine free radicals not only participate in the polymerization reaction, but also react with oxygen, thereby consuming oxygen in the system. This reduces the chance of oxygen reacting with chain free radicals and effectively suppresses the oxygen inhibition effect. Tertiary amine curing accelerators can also protect chain free radicals from being destroyed by oxygen through their specific chemical properties, such as rapid termination of peroxyl radicals, further inhibiting the oxygen inhibition effect; they can effectively inhibit the oxygen inhibition effect of photocuring, effectively reducing the amount of light absorbed by the ceramic slurry (this is because more light energy is used to initiate polymerization reactions rather than being absorbed by the slurry. Hydrogen abstraction photoinitiators have efficient light absorption properties and can absorb most of the light energy irradiated to the surface of the slurry. This light energy is then converted into chemical energy to initiate polymerization reactions), reducing light spillover (this is because light energy is more efficiently converted into chemical energy. When the hydrogen abstraction photoinitiator absorbs light energy, its molecules transition from the ground state to the excited state. In the excited state, the hydrogen abstraction photoinitiator can more easily undergo bimolecular action with the amine curing accelerator to form active amine radicals. In this process, light energy is efficiently converted into chemical energy to drive the polymerization reaction), ensuring the curing width and improving the curing efficiency.
[0036] The curing accelerator is preferably any one or more of triethylamine, triethanolamine and organic tertiary amine compounds. Tertiary amines can reduce the quenching effect of oxygen molecules, and can quickly terminate peroxyl radicals to generate α-amine radicals that can effectively initiate monomer polymerization, thereby promoting the curing reaction. Amines, as oxygen donors, are deprived of α-H by free radicals to generate α-amine radicals that are more likely to combine with triplet oxygen to form peroxyl radicals, consuming oxygen to reduce the reaction between oxygen and chain free radicals, thereby promoting the curing reaction. The composite plasticizer is preferably any of polyethylene glycol 200, polyethylene glycol 400, polypropylene glycol 400, dibutyl phthalate and dioctyl phthalate. Because different types of multiple plasticizers are compounded, the decomposition temperature of each plasticizer in the thermal degreasing stage is different. The first degreasing part of the composite plasticizer will form a degreasing channel, which is conducive to the discharge of subsequent resins and avoids the cracking of the product. The weight of the composite plasticizer is preferably 30%-40% of the weight of the high-precision ceramic 3D printing slurry. Optimizing the weight ratio of the composite plasticizer can effectively avoid the problem of product cracking after degreasing and sintering of the product, and improve the three-point bending strength; By purposefully selecting the formula components of high-precision ceramic 3D printing slurry and optimizing the ratio of the formula components, the present application not only effectively reduces the amount of light absorbed by the ceramic slurry and reduces the light spillover phenomenon, thereby improving the efficiency of light energy utilization in the printing process and ensuring the curing width, but also ensuring the curing depth, thereby avoiding the problem of low strength of the printed product due to insufficient curing; and is conducive to the formation of degreasing channels in the degreasing stage, so that the photosensitive resin can be discharged smoothly, avoiding the problem of product cracking; achieving high-precision light-curing 3D printing molding, improving product precision and the quality of mass production.
[0037] Example 1 The present invention provides a method for preparing a high-precision ceramic 3D printing slurry, comprising the following steps: S1 weighs 50g of photosensitive resin, 12.5g of dispersant BYK111, 0.8g of ultraviolet absorber UV321, 30g of composite plasticizer, 1.5g of hydrogen abstraction type photoinitiator and 1.2g of triethanolamine, adds them into a vacuum degassing machine, mixes at a speed of 500rpm for 10min, and obtains a mixture; wherein the photosensitive resin is a mixture of 1,6-hexanediol diacrylate (HDDA) and trimethylolpropane triacrylate (TMPTA), and the weight ratio of 1,6-hexanediol diacrylate (HDDA) and trimethylolpropane triacrylate (TMPTA) in the mixture of 1,6-hexanediol diacrylate (HDDA) and trimethylolpropane triacrylate (TMPTA) is 3:1; the composite plasticizer is polypropylene glycol The invention relates to a mixture of polypropylene glycol 400 (PPG400) and dibutyl phthalate (DBP), wherein the weight ratio of polypropylene glycol 400 (PPG400) and dibutyl phthalate (DBP) in the mixture of polypropylene glycol 400 (PPG400) and dibutyl phthalate (DBP) is 2:1; the hydrogen abstraction type photoinitiator is a mixture of isopropyl thioxanthone and 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, wherein the weight ratio of isopropyl thioxanthone and 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone in the mixture of isopropyl thioxanthone and 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone is 2:1; S2: adding the obtained mixture and 625 g of ZrO2 ceramic powder into a ball mill, and mixing at a speed of 100 rpm for 12 h to obtain a premixed slurry; S3 vacuum degasses the premixed slurry for 10 minutes to prepare a high-precision ceramic 3D printing slurry; The application of the prepared high-precision ceramic 3D printing slurry in 3D printing products includes the following steps: S401 uses a ceramic 3D printer to solidify high-precision ceramic 3D printing slurry layer by layer to form a ceramic green body; S402: placing the ceramic green body into a degreasing furnace, raising the degreasing temperature from room temperature to 200°C, and the degreasing rate is 0.1-0.5°C / min; S403 continues to heat up to the medium temperature range, the degreasing temperature rises from 200°C to 400°C, the degreasing rate is 0.3-1°C / min, and the holding time is maintained for at least 1 hour; S404 is heated from the medium temperature range to the high temperature range, the degreasing temperature is raised from 400°C to 600°C, and the temperature is kept for 4 to 6 hours. The degreasing rate is 0.1 to 0.5°C / min, and a ceramic matrix with higher purity is obtained.
[0038] Example 2 The present invention provides a method for preparing a high-precision ceramic 3D printing slurry, comprising the following steps: S1 weighs 60g of photosensitive resin, 10g of dispersant BYK218, 1.3g of [2-hydroxy-4-(octyloxy)phenyl]phenyl ketone, 35g of composite plasticizer, 1.5g of hydrogen abstraction type photoinitiator and 0.7g of organic tertiary amine compound, adds them into a vacuum degassing machine, and mixes them at a speed of 2000rpm for 2min to obtain a mixture; wherein the photosensitive resin is a mixture of 1,6-hexanediol diacrylate (HDDA) and ethoxylated pentaerythritol tetraacrylate (PPTTA), and the weight ratio of 1,6-hexanediol diacrylate (HDDA) to ethoxylated pentaerythritol tetraacrylate (PPTTA) in the mixture of 1,6-hexanediol diacrylate (HDDA) and ethoxylated pentaerythritol tetraacrylate (PPTTA) is 4:1; The composite plasticizer is a mixture of polypropylene glycol 400 (PPG400) and dioctyl phthalate (DOP), and the weight ratio of polypropylene glycol 400 (PPG400) and dioctyl phthalate (DOP) in the mixture is 1:1; the hydrogen abstraction type photoinitiator is a mixture of isopropyl thioxanthone and 4-dimethylamino-ethyl benzoate, and the weight ratio of isopropyl thioxanthone and 4-dimethylamino-ethyl benzoate in the mixture is 2:1; the organic tertiary amine compound is an organic tertiary amine P115 C20H31O6N (a tertiary amine accelerator containing a reactive group); S2: adding the obtained mixture and 400 g of Al2O3 ceramic powder into a ball mill, and mixing at 300 rpm for 5 h to obtain a premixed slurry; S3 vacuum degasses the premixed slurry for 30 minutes to prepare a high-precision ceramic 3D printing slurry; The application of the prepared high-precision ceramic 3D printing slurry in 3D printing products includes the following steps: S401 uses a ceramic 3D printer to solidify high-precision ceramic 3D printing slurry layer by layer to form a ceramic green body; S402: placing the ceramic green body into a degreasing furnace, raising the degreasing temperature from room temperature to 200°C, and the degreasing rate is 0.1-0.5°C / min; S403 continues to heat up to the medium temperature range, the degreasing temperature rises from 200°C to 400°C, the degreasing rate is 0.3-1°C / min, and the holding time is maintained for at least 1 hour; S404 is heated from the medium temperature range to the high temperature range, the degreasing temperature is raised from 400°C to 600°C, and the temperature is kept for 4 to 6 hours. The degreasing rate is 0.1 to 0.5°C / min, and a ceramic matrix with higher purity is obtained.
[0039] Example 3 The present invention provides a method for preparing a high-precision ceramic 3D printing slurry, comprising the following steps: S1 weighs 52g of photosensitive resin, 9g of dispersant KOS110, 1g of ultraviolet absorber UV329, 32g of composite plasticizer, 0.8g of hydrogen abstraction type photoinitiator and 1g of triethylamine, adds them into a vacuum degassing machine, mixes at a speed of 1500rpm for 2min, and obtains a mixture; wherein the photosensitive resin is a mixture of 1,6-hexanediol diacrylate, iminodiacetic acid and trimethylolpropane triacrylate, and the mixture of 1,6-hexanediol diacrylate (HDDA), iminodiacetic acid (IDA) and trimethylolpropane triacrylate (TMPTA) is 1,6-hexanediol diacrylate (HDDA), iminodiacetic acid (IDA) and trimethylolpropane triacrylate. The weight ratio of trimethylolpropane phthalate (TMPTA) is 6:3:1; the composite plasticizer is a mixture of dibutyl phthalate (DBP) and polyethylene glycol 200 (PEG200), and the weight ratio of dibutyl phthalate (DBP) and polyethylene glycol 200 (PEG200) in the mixture of dibutyl phthalate (DBP) and polyethylene glycol 200 (PEG200) is 3:1; the hydrogen abstraction type photoinitiator is a mixture of benzophenone and 4,4'-di(N,N-dimethylamino)benzophenone, and the weight ratio of benzophenone and 4,4'-di(N,N-dimethylamino)benzophenone in the mixture of benzophenone and 4,4'-di(N,N-dimethylamino)benzophenone is 1:1; S2: adding the obtained mixture and 420 g of zirconia toughened alumina ceramic powder into a ball mill, and mixing at a speed of 200 rpm for 10 h to obtain a premixed slurry; S3 vacuum degasses the premixed slurry for 30 minutes to obtain high-precision ceramic 3D printing slurry; The application of the prepared high-precision ceramic 3D printing slurry in 3D printing products includes the following steps: S401 uses a ceramic 3D printer to solidify high-precision ceramic 3D printing slurry layer by layer to form a ceramic green body; S402: placing the ceramic green body into a degreasing furnace, raising the degreasing temperature from room temperature to 200°C, and the degreasing rate is 0.1-0.5°C / min; S403 continues to heat up to the medium temperature range, the degreasing temperature rises from 200°C to 400°C, the degreasing rate is 0.3-1°C / min, and the holding time is maintained for at least 1 hour; S404 is heated from the medium temperature range to the high temperature range, the degreasing temperature is raised from 400°C to 600°C, and the temperature is kept for 4 to 6 hours. The degreasing rate is 0.1 to 0.5°C / min, and a ceramic matrix with higher purity is obtained.
[0040] Comparative Example 1 Comparative Example 1 provides a method for preparing a high-precision ceramic 3D printing slurry, comprising the following steps: S1 weighed 50g of photosensitive resin, 12.5g of dispersant BYK111, 30g of composite plasticizer, 1.5g of hydrogen abstraction type photoinitiator and 1.2g of triethanolamine, added into a vacuum degassing machine, and mixed at a speed of 500rpm for 10min to obtain a mixture; wherein the photosensitive resin is a mixture of 1,6-hexanediol diacrylate (HDDA) and trimethylolpropane triacrylate (TMPTA), and the weight ratio of 1,6-hexanediol diacrylate (HDDA) and trimethylolpropane triacrylate (TMPTA) in the mixture of 1,6-hexanediol diacrylate (HDDA) and trimethylolpropane triacrylate (TMPTA) is 3:1; the composite plasticizer is polypropylene glycol 400 (PPG40 0) and dibutyl phthalate (DBP), the weight ratio of polypropylene glycol 400 (PPG400) and dibutyl phthalate (DBP) in the mixture of polypropylene glycol 400 (PPG400) and dibutyl phthalate (DBP) is 2:1; the hydrogen abstraction type photoinitiator is a mixture of isopropylthioxanthone and 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, and the weight ratio of isopropylthioxanthone and 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone in the mixture of isopropylthioxanthone and 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone is 2:1; S2: adding the obtained mixture and 625 g of ZrO2 ceramic powder into a ball mill, and mixing at a speed of 100 rpm for 12 h to obtain a premixed slurry; S3 vacuum degasses the premixed slurry for 10 minutes to prepare high-precision ceramic 3D printing slurry.
[0041] The application of the prepared high-precision ceramic 3D printing slurry in 3D printing products includes the following steps: S401 uses a ceramic 3D printer to solidify high-precision ceramic 3D printing slurry layer by layer to form a ceramic green body; S402: placing the ceramic green body into a degreasing furnace, raising the degreasing temperature from room temperature to 200°C, and the degreasing rate is 0.1-0.5°C / min; S403 continues to heat up to the medium temperature range, the degreasing temperature rises from 200°C to 400°C, the degreasing rate is 0.3-1°C / min, and the holding time is maintained for at least 1 hour; S404 is heated from the medium temperature range to the high temperature range, the degreasing temperature is raised from 400°C to 600°C, and the temperature is kept for 4 to 6 hours. The degreasing rate is 0.1 to 0.5°C / min, and a ceramic matrix with higher purity is obtained.
[0042] Comparative Example 2 Comparative Example 2 provides a method for preparing a high-precision ceramic 3D printing slurry, comprising the following steps: S1 weighed 60g of photosensitive resin, 10g of dispersant BYK218, 1.3g of [2-hydroxy-4-(octyloxy)phenyl]phenyl ketone, 35g of composite plasticizer and 1.5g of hydrogen abstraction type photoinitiator, added them into a vacuum degassing machine, and mixed them at a speed of 2000rpm for 2min to obtain a mixture; wherein the photosensitive resin is a mixture of 1,6-hexanediol diacrylate (HDDA) and ethoxylated pentaerythritol tetraacrylate (PPTTA), and the 1,6-hexanediol diacrylate (HDDA) and ethoxylated pentaerythritol tetraacrylate (PPTTA) in the mixture are 1,6-hexanediol diacrylate (HDDA) and ethoxylated pentaerythritol tetraacrylate (PPTTA). The weight ratio of the ester (PPTTA) is 4:1; the composite plasticizer is a mixture of polypropylene glycol 400 (PPG400) and dioctyl phthalate (DOP), and the weight ratio of polypropylene glycol 400 (PPG400) and dioctyl phthalate (DOP) in the mixture of polypropylene glycol 400 (PPG400) and dioctyl phthalate (DOP) is 1:1; the hydrogen abstraction type photoinitiator is a mixture of isopropyl thioxanthone and 4-dimethylamino-ethyl benzoate, and the weight ratio of the hydrogen abstraction type photoinitiator is 2:1 for isopropyl thioxanthone and 4-dimethylamino-ethyl benzoate in the mixture of isopropyl thioxanthone and 4-dimethylamino-ethyl benzoate; S2: adding the obtained mixture and 400 g of Al2O3 ceramic powder into a ball mill, and mixing at 300 rpm for 5 h to obtain a premixed slurry; S3 vacuum degasses the premixed slurry for 30 minutes to prepare a high-precision ceramic 3D printing slurry; The application of the prepared high-precision ceramic 3D printing slurry in 3D printing products includes the following steps: S401 uses a ceramic 3D printer to solidify high-precision ceramic 3D printing slurry layer by layer to form a ceramic green body; S402: placing the ceramic green body into a degreasing furnace, raising the degreasing temperature from room temperature to 200°C, and the degreasing rate is 0.1-0.5°C / min; S403 continues to heat up to the medium temperature range, the degreasing temperature rises from 200°C to 400°C, the degreasing rate is 0.3-1°C / min, and the holding time is maintained for at least 1 hour; S404 is heated from the medium temperature range to the high temperature range, the degreasing temperature is raised from 400°C to 600°C, and the temperature is kept for 4 to 6 hours. The degreasing rate is 0.1 to 0.5°C / min, and a ceramic matrix with higher purity is obtained.
[0043] Comparative Example 3 Comparative Example 3 provides a method for preparing a high-precision ceramic 3D printing slurry, comprising the following steps: S1 weighed 52g of photosensitive resin, 9g of dispersant KOS110, 1g of ultraviolet absorber UV329, 9g of dioctyl phthalate, 0.8g of hydrogen abstraction type photoinitiator and 1g of triethylamine, added them into a vacuum degassing machine, and mixed them at a speed of 1500rpm for 2min to obtain a mixture; wherein the photosensitive resin is a mixture of 1,6-hexanediol diacrylate (HDDA), iminodiacetic acid (IDA) and trimethylolpropane triacrylate (TMPTA), 1,6-hexanediol diacrylate (HDDA), iminodiacetic acid (IDA) and trimethylolpropane triacrylate (TMPTA), The weight ratio of 1,6-hexanediol diacrylate (HDDA), iminodiacetic acid (IDA) and trimethylolpropane triacrylate (TMPTA) in the mixture of 1,6-hexanediol diacrylate (HDDA), iminodiacetic acid (IDA) and trimethylolpropane triacrylate (TMPTA) is 6:3:1; the hydrogen abstraction type photoinitiator is a mixture of benzophenone and 4,4'-bis(N,N-dimethylamino)benzophenone, and the weight ratio of benzophenone and 4,4'-bis(N,N-dimethylamino)benzophenone in the mixture of benzophenone and 4,4'-bis(N,N-dimethylamino)benzophenone is 1:1; S2: adding the obtained mixture and 420 g of zirconia toughened alumina ceramic powder into a ball mill, and mixing at a speed of 200 rpm for 10 h to obtain a premixed slurry; S3 vacuum degasses the premixed slurry for 30 minutes to obtain high-precision ceramic 3D printing slurry; The application of the prepared high-precision ceramic 3D printing slurry in 3D printing products includes the following steps: S401 uses a ceramic 3D printer to solidify high-precision ceramic 3D printing slurry layer by layer to form a ceramic green body; S402: placing the ceramic green body into a degreasing furnace, raising the degreasing temperature from room temperature to 200°C, and the degreasing rate is 0.1-0.5°C / min; S403 continues to heat up to the medium temperature range, the degreasing temperature rises from 200°C to 400°C, the degreasing rate is 0.3-1°C / min, and the holding time is maintained for at least 1 hour; S404 is heated from the medium temperature range to the high temperature range, the degreasing temperature is raised from 400°C to 600°C, and the temperature is kept for 4 to 6 hours. The degreasing rate is 0.1 to 0.5°C / min, and a ceramic matrix with higher purity is obtained.
[0044] Experimental means of experimental data testing The high-precision ceramic 3D printing slurries and 3D printing products prepared in Examples 1-3 and Comparative Examples 1-3 were measured by the following experimental means: The high-precision ceramic 3D printing slurry was tested for viscosity using a lamina viscometer. When testing the viscosity, the test conditions were set as follows: temperature was 25°C and revolutions per minute was 30RPM; 3D printed products, observe and evaluate the curing depth and curing width of the products as follows: The curing depth of the product was observed and evaluated by the following experimental means: a single-layer sample was printed in a suspended state according to fixed printing parameters, the uncured suspension was removed by washing with a mixed solution of 1,6-hexanediol diacrylate (HDDA) and ethanol, the thickness of each sample was tested by a micrometer, and the average value of 5 samples was taken for each group; The curing width of the product was observed and evaluated by the following experimental means: a single-line width sample was printed in a suspended state according to fixed printing parameters, the uncured suspension was removed by washing with a mixed solution of 1,6-hexanediol diacrylate (HDDA) and ethanol, and the cured width was measured by an optical automatic image measuring instrument. Five samples were measured in each group and the average value was taken. The experimental data of the three-point bending strength of 3D printed products after sintering was tested by a three-point mechanical testing machine; The experimental data of the high-precision ceramic 3D printing slurry and 3D printing product test prepared in Examples 1-3 and Comparative Examples 1-3 are as follows in Table 1: Table 1 Experimental data of high-precision ceramic 3D printing slurry and 3D printing product testing
[0045] From Table 1, we can observe that the formulation components of Comparative Example 1 do not add UV absorber compared to the formulation components of Example 1, resulting in an increase in the curing depth and curing width of the product provided by Comparative Example 1 compared to the product provided by Example 1, and a decrease in the precision of the 3D printed product provided by Comparative Example 1; Compared with the formula components of Example 2, the formula components of Comparative Example 2 do not add a curing accelerator. The curing depth of the product provided by Example 2 is 56 μm, and the curing depth of the product provided by Comparative Example 2 is reduced to 35 μm. The precision of the 3D printed product is reduced. The three-point bending strength of the product provided by Example 2 is 535 Mpa, and the three-point bending strength of the product provided by Comparative Example 2 is reduced to 347 Mpa. The printing strength and other properties of the product provided by Comparative Example 2 are poor, and the curing ability is weak; Compared with the formula components of Example 3, the formula components of Comparative Example 3 only select one plasticizer, and do not perform compounding and synergistic use of multiple plasticizers. The three-point bending strength of the product provided by Example 3 is 740 Mpa, and the slurry viscosity provided by Example 3 is 1983 mpas. The three-point bending strength of the product provided by Comparative Example 3 decreases to 435 Mpa, and the slurry viscosity provided by Example 3 increases to 3749 mpas. When only one plasticizer is selected in Comparative Example 3, multiple plasticizers are not compounded and synergized, resulting in increased viscosity of the product slurry, relatively poor fluidity, and reduced three-point bending strength of the product. The supporting effect is weak after degreasing and sintering, and the product is prone to cracking.
[0046] It is to be understood that the present invention is described by some embodiments, and it is known to those skilled in the art that various changes or equivalent substitutions may be made to these features and embodiments without departing from the spirit and scope of the present invention. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all various changes or equivalent substitutions falling within the scope of the claims of the present application are included. In addition, under the teachings of the present invention, these features and embodiments may be modified to adapt to specific circumstances and materials without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited by the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of the present application are within the scope protected by the present invention.
Claims
1. A high-precision ceramic 3D printing slurry, characterized in that: Includes the following components: Ceramic powder; Photosensitive resin; Dispersants; Ultraviolet absorbers, including any one or more of N-(2-ethoxyphenyl)-N'-(2-ethylphenyl)-oxalamide, 2-(2'-hydroxy-3', 5'-di-tert-butylphenyl)-5-chlorobenzotriazole), [2-hydroxy-4-(octyloxy)phenyl]phenyl ketone and benzotriazole ultraviolet absorbers; A composite plasticizer, wherein the composite plasticizer comprises any of polyethylene glycol 200, polyethylene glycol 400, polypropylene glycol 400, dibutyl phthalate and dioctyl phthalate; A hydrogen abstraction type photoinitiator, wherein the hydrogen abstraction type photoinitiator includes any one or more of benzophenone, 4,4'-bis(N,N-dimethylamino)benzophenone, isopropylthioxanthone, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone and 4-dimethylamino-ethyl benzoate; A curing accelerator, wherein the curing accelerator comprises any one or more of triethylamine, triethanolamine and organic tertiary amine compounds; The weight ratio of the ceramic powder, the photosensitive resin, the dispersant, the ultraviolet absorber, the composite plasticizer, the hydrogen abstraction type photoinitiator and the curing accelerator is (6.25-4): (0.6-0.5): (0.125-0.09): (0.013-0.008): (0.4-0.3): (0.015-0.008): (0.012-0.007).
2. The high-precision ceramic 3D printing slurry according to claim 1, characterized in that: The ceramic powder includes any one or more of zirconia, alumina, zirconia toughened alumina ceramics and alumina toughened zirconia ceramics.
3. The high-precision ceramic 3D printing slurry according to claim 1, characterized in that: The photosensitive resin includes any of isobornyl acrylate, 1,6-hexanediol diacrylate, iminodiacetic acid, trimethylolpropane triacrylate and ethoxylated pentaerythritol tetraacrylate.
4. The high-precision ceramic 3D printing slurry according to claim 1, characterized in that: The dispersant includes: any one or more of dispersant BYK110, dispersant BYK218, dispersant BYK111, and dispersant KOS110.
5. A method for preparing high-precision ceramic 3D printing slurry, characterized in that: The high-precision ceramic 3D printing slurry according to any one of claims 1 to 4 is prepared, comprising the following steps: S1: weighing a photosensitive resin, a dispersant, an ultraviolet absorber, a composite plasticizer, a hydrogen abstraction type photoinitiator and a curing accelerator according to a weight ratio, adding them into a vacuum degassing machine, and mixing them at a speed of 500 to 2000 rpm for 2 to 10 minutes to obtain a mixture; S2: adding the obtained mixture and the ceramic powder weighed according to the weight ratio into a ball mill, and mixing at a speed of 100 to 300 rpm for 5 to 12 hours to obtain a premixed slurry; S3 vacuum degasses the premixed slurry to obtain high-precision ceramic 3D printing slurry.
6. The method for preparing high-precision ceramic 3D printing slurry according to claim 5, characterized in that: The vacuum degassing time of the premixed slurry in step S3 is 10 to 30 minutes.
7. The use of the high-precision ceramic 3D printing slurry according to any one of claims 1 to 4 in 3D printing products, characterized in that: The high-precision ceramic 3D printing slurry is solidified layer by layer by a ceramic 3D printer to form a ceramic green body, and the ceramic green body is degreased in sections.
8. The use of the high-precision ceramic 3D printing slurry in 3D printing products according to claim 7, characterized in that: The temperature of the segmented degreasing is ≤600°C, and the rate of the segmented degreasing is 0.1-1°C / min.
Citation Information
Patent Citations
High-resolution light-cured 3D printing composite
CN110804276A
Silicon carbide ceramic slurry with high photosensitive activity and preparation method thereof
CN113429210A
Photocuring ceramic slurry for 3D printing and pretreatment method of formed green body
CN113603467A
Photo-cured calcium silicate / beta-tricalcium phosphate ceramic paste and preparation method of porous scaffold
CN113636836A
Porous ceramic matrix composition for electronic cigarette atomization core, porous ceramic matrix, preparation method of porous ceramic matrix and electronic cigarette atomization core
CN115043654A