Preparation method of slurry for improving thermal conductivity of silicon nitride ceramic chip
By adding reducing agent to the slurry of silicon nitride ceramic sheets and using spray atomization technology to prevent the oxidation of boron nitride, the problem of insufficient thermal conductivity of silicon nitride ceramic sheets is solved, and the thermal conductivity is improved and Improved surface quality.
Patent Information
- Application Number
- CN202410995101.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the sintering process, the surface heterogeneous phases are generated due to the oxidation of boron nitride, which affects the thermal conductivity. The prior art is difficult to effectively prevent oxidation, resulting in insufficient thermal conductivity.
Using the slurry preparation method with reducing agent added, the boron nitride powder is uniformly sprayed through spray atomization technology, and the reducing agent is used to decompose nitrogen, hydrogen or carbides at high temperatures to prevent boron nitride oxidation and improve silicon nitride ceramic sheets. thermal conductivity.
Through this method, the thermal conductivity of the silicon nitride ceramic sheet is significantly improved, reaching more than 90W/(m·K), reducing the generation of surface miscellaneous phases, and improving the thermal conductivity and surface smoothness of the ceramic sheet.
Smart Images

Figure CN118930319A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermally conductive ceramics, in particular to a method for preparing a slurry for improving the thermal conductivity of a silicon nitride ceramic sheet. Background Art
[0002] Silicon nitride ceramics have high thermal conductivity, high strength, high hardness, corrosion resistance, high modulus, low expansion coefficient, oxidation resistance, and good resistance to thermal shock and mechanical shock. They are considered by the material science community to be one of the ceramic materials with excellent comprehensive performance in the field of ceramics. The thermal conductivity of commercial high thermal conductivity silicon nitride ceramics is about 80W / (m·K), and the bending strength is 600-850MPa. When sintering silicon nitride ceramics, gas pressure liquid phase sintering technology is used. Therefore, the sheets need to be isolated by boron nitride with a higher sintering temperature, otherwise the sheets will sinter together and will not be easy to separate. Boron nitride coated on the surface of the ceramic is easily oxidized at high temperatures, and the oxidized substances will penetrate into the surface of the ceramic and form new impurities at high temperatures, thereby affecting the microscopic crystal structure and thermal conductivity of the surface of the ceramic.
[0003] The present invention adopts a powder coating slurry prepared by adding a reducing agent, and the slurry is evenly sprayed onto a green body by spray atomization, and then the green body is debinded and sintered. The reducing agent can decompose nitrogen, hydrogen or carbide at high temperature. These decomposed substances have reducing properties and can prevent boron nitride from being oxidized at high temperature, or reduce oxidized boron oxide to boron nitride, thereby greatly reducing the generation of impurities, and further increasing the thermal conductivity of the silicon nitride ceramic sheet by more than 10%, reaching more than 90W / (m·K). Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a slurry for improving the thermal conductivity of a silicon nitride ceramic tile, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A slurry for improving the thermal conductivity of silicon nitride ceramic sheets, wherein the slurry comprises, by mass percentage, 10-30% of boron nitride powder, 0.2-2% of a reducing agent, 0.5-2.5% of a binder, 0.2-1.5% of a plasticizer, 0.2-1.5% of a dispersant, and the remainder being a solvent.
[0007] The solvent is at least one of pure water, deionized water, isopropanol, ethylene glycol, and diethylene glycol; further set to pure water;
[0008] The binder is at least one of hydroxyethyl cellulose, acrylic resin, polyvinyl alcohol, and methyl cellulose; further configured as methyl cellulose;
[0009] The plasticizer is at least one of dodecyl alcohol ester, benzoic acid ester, dimethyl phthalate, and diethylene glycol butyl ether; further configured as benzoic acid ester;
[0010] The dispersant is at least one of polypropylene glycol, polyetheramines, and aqueous castor oil; and is further configured to be polypropylene glycol.
[0011] A method for preparing a slurry for improving the thermal conductivity of a silicon nitride ceramic tile, the specific preparation steps are as follows:
[0012] S1) glue preparation: mixing the solvent and the binder, heating and stirring at 60°C to 90°C, with a stirring speed of 20 to 120 rpm and a stirring time of 0.5 to 2 h to prepare the glue;
[0013] S2) solvent premixing: mixing the solvent, the glue prepared in S1, the dispersant, and the plasticizer at a stirring speed of 500 to 1500 rpm for 10 to 30 min to prepare a premixed solution;
[0014] S3) Dissolving the reducing agent: adding the reducing agent to the premixed solution, stirring at a constant temperature of 80° C. until the reducing agent is completely dissolved;
[0015] S4) preparing slurry and dispersing by emulsifier: adding boron nitride powder to the premixed liquid of the dissolved reducing agent prepared in S3, emulsifying and dispersing at a rotation speed of 3000 to 20000 rpm for a dispersion time of 2 to 6 hours to obtain slurry.
[0016] The reducing agent is at least one of melamine, urea, triethanolamine and acetanilide; further configured as melamine;
[0017] The invention discloses an application of a slurry for improving the thermal conductivity of silicon nitride ceramic sheets, and the specific steps are as follows: the prepared slurry is loaded into a spray powder coating machine with a spray pressure of 0.2-0.8 MPa, and sprayed on a silicon nitride green body to form a boron nitride coating with a thickness of 2-30 μm and a stacked particle diameter of 0.02-0.30 mm.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0019] 1) The method for preparing a slurry for improving the thermal conductivity of silicon nitride ceramic tiles of the present invention comprises selecting a soluble reducing agent, dispersing the slurry through an emulsifier, and the dissolved reducing agent can form a good wrapping and penetration of the boron nitride powder, and can be evenly dispersed on the surface of the boron nitride particles;
[0020] 2) The powder coating slurry of the present invention adopts a high-pressure spray powder coating method to form a coating with a thickness of 2 to 30 μm and a stacked particle diameter of 0.02 to 0.30 mm on the surface of the green body. The powder coating particles are uniform and the intercalation effect is good;
[0021] 3) The powder coating slurry of the present invention is evenly coated on the surface of the green body by adding a reducing agent. During the debinding and sintering process of the ceramic, the reducing agent can decompose nitrogen, hydrogen or carbide at a high temperature of 600-1000°C. These decomposition products can reduce the oxidation of boron nitride, or reduce the oxidized boron oxide, and reduce the generation of impurities on the surface of the ceramic piece, thereby increasing the thermal conductivity of the ceramic piece by more than 10%. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0023] Figure 1 This is a microscopic morphology of the surface of the green body after the powder is applied in Example 1, the microscope is magnified 30 times, and the scale is 1 mm;
[0024] Figure 2 Part (a) shows the microscopic state of the ceramic surface after sintering the green body of Comparative Example 1, magnified 75 times by a microscope; Part (b) shows the microscopic state of the ceramic surface after sintering the green body of Comparative Example 1, magnified 500 times by a metallographic microscope.
[0025] Figure 3 Part (a) shows the microscopic state of the surface of the ceramic piece after the green body of Example 3 is sintered, and the microscope magnification is 75 times; Part (b) shows the microscopic state of the surface of the ceramic piece after the green body of Example 3 is sintered, and the metallographic microscope magnification is 500 times. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] See also Figure 1-3 , the present invention provides a technical solution:
[0028] In the experiment, the methyl cellulose model is M450, and the viscosity is 350~550mpa · s, purchased from Tianjin Huasheng Chemical Reagent Co., Ltd.; polypropylene glycol model is PPG-200, molecular weight is 180-220, purchased from Shandong Huling New Materials Co., Ltd.
[0029] Embodiment 1: A method for preparing a slurry for improving the thermal conductivity of a silicon nitride ceramic tile, comprising the following steps:
[0030] S1) glue preparation: 90 g pure water and 10 g methyl cellulose were mixed, heated and stirred using a magnetic stirrer at a heating temperature of 70° C., a stirring speed of 60 rpm, and a stirring time of 1 h to prepare glue;
[0031] S2) solvent premixing: 200 g pure water, 20 g prepared glue, 2.5 g polypropylene glycol and 2 g benzoate were added to a beaker, stirred in a stirrer at a speed of 500 rpm for 15 min to prepare a premixed solution, and mixed evenly;
[0032] S3) Dissolving the reducing agent: adding 0.549 g (0.2 wt%) of melamine to the premixed solution, stirring at a constant temperature of 80° C. until the melamine is completely dissolved;
[0033] S4) Preparation of slurry and dispersion by emulsifier: Add 49.41 g of boron nitride powder (accounting for 18 wt%) into the premixed liquid containing melamine, and disperse it by emulsifier at a speed of 8000 rpm for 4 hours.
[0034] Example 2: Based on Example 1, the final composition ratio of boron nitride powder and reducing agent is changed to: 17.7wt% boron nitride, 0.5wt% melamine.
[0035] Example 3: Based on Example 1, the final composition ratio of boron nitride powder and reducing agent is changed to: 17.4wt% boron nitride, 0.8wt% melamine.
[0036] Example 4: Based on Example 1, the final composition ratio of boron nitride powder and reducing agent is changed to: 17.1wt% boron nitride, 1.1wt% melamine.
[0037] Comparative Example 1: Based on Example 1, the final composition ratio of boron nitride powder and reducing agent was changed to: 18.2 wt % of boron nitride and 0 wt % of melamine.
[0038] The slurries prepared in the above-mentioned Examples 1-4 and Comparative Example 1 were sprayed onto the surface of the silicon nitride green body by a spray powder coating machine at a spray pressure of 0.35 MPa to form a coating with a thickness of 10 μm on the green body. Figure 1 As shown, the green pieces are stacked to 6 layers for debinding. The debinding temperature is 500℃, and the temperature is kept for 4 hours. The ceramic pieces after debinding are placed in a graphite furnace and sintered under pressure in a nitrogen atmosphere at a sintering temperature of 1850℃ for 2 hours. The surface microscopic state and crystal phase structure of the ceramic pieces after sintering are observed by microscope and metallographic microscope, as shown in Figure 1. Figure 2 , 3 The roughness and thermal conductivity of the ceramic tile were tested. The test data are shown in Table 1.
[0039] Table 1 Effects of different slurry powder coating schemes on the performance of silicon nitride ceramics
[0040]
[0041] Conclusion: The slurries prepared in Examples 1-4 and Comparative Example 1 were sprayed on the surface of the silicon nitride green body. Figure 1 White powder particles can be seen in the figure; the processed green pieces are stacked, debinded and sintered to obtain thermal conductive ceramic sheets; Figure 2 The ceramic piece sintered from the slurry without adding reducing agent in Example 1. It can be seen from the figure that the white spots on the surface of the ceramic piece are serious. Through metallographic microscopic observation, it can be found that in the red circle area, there are many spherical impurities between the grains; the ceramic piece surface after sintering the slurry of Example 3 doped with reducing agent is as follows Figure 3 As shown, there are fewer white spots on the surface of the ceramic piece, and metallographic microscopic observation shows that there are almost no other impurities between the grains; the surface roughness and thermal conductivity of the ceramic pieces prepared by Examples 1-4 and Comparative Example 1 are measured. The thermal conductivity of Comparative Example 1 without reducing agent is significantly lower than that of other examples, and the surface of the ceramic piece is also rougher; Example 3 obtains relatively excellent thermal conductivity data among Examples 1-4, and the surface is also smoother and flatter.
[0042] Working principle of the present invention: In view of the problem that the existing conventional boron nitride powder coating technology is easy to oxidize during powder debinding and sintering, the purpose of the present invention is to add a reducing agent with nitriding reduction effect to the powder coating slurry, and adopt an emulsification dispersion process to evenly disperse the boron nitride powder and the reducing agent. A uniform coating is formed on the surface of the green body by high-pressure spray powder coating, the green body is stacked to debind, and pressurized and high-temperature sintered. The oxidized boron nitride at high temperature will be nitrided and reduced by the reducing agent, reducing its adverse effects on the surface of the ceramic tile, thereby improving the thermal conductivity of the ceramic tile.
[0043] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0044] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A slurry for improving the thermal conductivity of silicon nitride ceramics, characterized in that: The slurry comprises: by mass percentage, 10-30% of boron nitride powder, 0.2-2% of reducing agent, 0.5-2.5% of binder, 0.2-1.5% of plasticizer, 0.2-1.5% of dispersant, and the rest is solvent.
2. The slurry for improving the thermal conductivity of silicon nitride ceramic sheets according to claim 1, characterized in that: The solvent is at least one of pure water, deionized water, isopropanol, ethylene glycol and diethylene glycol.
3. The slurry for improving the thermal conductivity of silicon nitride ceramic sheets according to claim 1, characterized in that: The binder is at least one of hydroxyethyl cellulose, acrylic resin, polyvinyl alcohol and methyl cellulose.
4. The slurry for improving the thermal conductivity of silicon nitride ceramic sheets according to claim 1, characterized in that: The plasticizer is at least one of dodecyl alcohol ester, benzoic acid ester, dimethyl phthalate and diethylene glycol butyl ether.
5. The slurry for improving the thermal conductivity of silicon nitride ceramic sheets according to claim 1, characterized in that: The dispersant is at least one of polypropylene glycol, polyetheramines and aqueous castor oil.
6. A method for preparing a slurry for improving the thermal conductivity of silicon nitride ceramic tiles, characterized in that: The following steps are involved: S1) glue preparation: mixing the solvent and the binder, heating and stirring at 60°C to 90°C for 0.5 to 2 hours to prepare the glue; S2) solvent premixing: mixing the solvent, the glue prepared in S1, the dispersant, and the plasticizer for 10 to 30 minutes to prepare a premixed liquid; S3) Dissolving the reducing agent: adding the reducing agent to the premixed solution, stirring at a constant temperature of 80° C. until the reducing agent is completely dissolved; S4) preparing slurry and dispersing by emulsifier: adding boron nitride powder to the premixed liquid of the dissolved reducing agent prepared in S3, emulsifying and dispersing for 2 to 6 hours to obtain slurry.
7. The method for preparing a slurry for improving thermal conductivity of silicon nitride ceramic tiles according to claim 6, characterized in that: The stirring speed in S1) is 20-120 rpm; the stirring speed in S2) is 500-1500 rpm; the emulsification speed in S4) is 3000-20000 rpm.
8. The method for preparing a slurry for improving thermal conductivity of silicon nitride ceramic tiles according to claim 6, characterized in that: The reducing agent is at least one of melamine, urea, triethanolamine and acetanilide.
9. The use of a slurry for improving the thermal conductivity of silicon nitride ceramic sheets according to any one of claims 1 to 5, wherein The characteristic is that the slurry is sprayed onto the surface of the silicon nitride green body with a spray pressure of 0.2 to 0.8 MPa to form a 2 to 30 μm thick film on the green body. The coating has a particle diameter of 0.02 to 0.30 mm.
Citation Information
Patent Citations
Silicon nitride substrate and method for manufacturing silicon nitride substrate
CN103781742A
High-thermal-conductivity silicon nitride ceramic substrate and preparation method thereof
CN112159236A
Preparation method of boron nitride printing paste
CN116063084A
Si3N4 Sintered body with high thermal conductivity and method for producing the same
EP0940377A1
Production of planar sintered ceramics body
JP1989087574A
Cited By
Ceramic substrate blank powder coating and sintering process
CN119928059A
Method for preparing high-performance silicon nitride substrate based on direct nitriding method
CN122427028A