Curing agent and preparation method thereof

A new curing agent was prepared by performing carboxymethylation reaction of polyoxyethylene fatty alcohol ether with basic compounds and carboxymethylation reagents and mixing them with imidazole compounds, which solved the existing curing agent at room temperature. The problems of short storage time and high curing temperature achieve good compatibility with epoxy resin and fast curing at low temperatures, simplifying the steps of industrial application.

CN118930842APending Publication Date: 2024-11-12TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411236417.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing epoxy resin curing agent for electronic slurries has short storage time at room temperature and high curing temperature requirements, so the industrial application steps are complicated.

Method used

The obtained polyoxyethylene fatty alcohol ether, basic compound and carboxymethylation reagent are mixed to carry out carboxymethylation reaction, and the obtained polyoxyethylene fatty alcohol ether carboxylic acid and imidazole compounds are mixed at a temperature of 100 to 150°C to prepare A new curing agent is produced, which is liquid at room temperature and has a long room temperature storage time and good compatibility.

Benefits of technology

The curing agent is well compatible with epoxy resin at room temperature, can extend the storage time of a single component system, quickly cure under low temperature conditions, simplifies industrial application steps, and improves the ductility and conductivity of conductive pastes performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930842A_ABST
    Figure CN118930842A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of curing agents, particularly provides a curing agent and a curing agent preparation method, and aims to solve the problems of short storage time at room temperature, high curing temperature requirement and complex industrial application steps after an existing curing agent is mixed with epoxy resin. In order to achieve the purpose, the curing agent is a compound formed by an imidazole compound and polyoxyethylene fatty alcohol ether carboxylic acid, and the polyoxyethylene fatty alcohol ether carboxylic acid comprises a plurality of polyoxyethylene groups. The curing agent has the advantages of simple preparation method, mild conditions, cheap and easily available synthetic raw materials, long storage time when being mixed with resin at room temperature to form a single-component system, rapid curing at low temperature and the like. And meanwhile, the curing agent is in a liquid state at normal temperature and has good mixing compatibility with epoxy resin, so that the ductility of the slurry can be improved after the curing agent is prepared into the conductive slurry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of curing agents, and specifically provides a curing agent and a method for preparing the curing agent. Background Art

[0002] Existing epoxy resin curing agents for electronic pastes are often solid substances with poor compatibility with epoxy resins, and require additional diluents or organic solvents to ensure the curing effect. In addition, the storage time of the curing agent and epoxy resin at room temperature is short, the curing temperature requirement is high, and the industrial application steps are complicated. Summary of the invention

[0003] The present invention aims to solve the above technical problem, that is, to solve the problem that the existing curing agent has a short storage time at room temperature after being mixed with epoxy resin, has a high curing temperature requirement, and has complex industrial application steps.

[0004] In a first aspect, the present invention provides a curing agent, the molecular structure of which is as follows:

[0005]

[0006] Wherein, n is greater than or equal to 2, and R2 and R3 are each independently hydrogen or alkyl.

[0007] In some embodiments, R1 is one of hydrogen, an alkyl group, a stearyl alcohol group, or a sorbitan ester group.

[0008] In some embodiments, R2 is an alkyl group having a carbon number of 1 to 11 and R3 is hydrogen.

[0009] In some embodiments, R2 is methyl.

[0010] In some embodiments, 6<n<10.

[0011] In a second aspect, the present application provides a method for preparing a curing agent, the method being used to prepare any of the curing agents described above, the method comprising:

[0012] The polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent are mixed to perform a carboxymethylation reaction to obtain the polyoxyethylene fatty alcohol ether carboxylic acid; the chemical formula of the polyoxyethylene fatty alcohol ether is R1O-(CH2CH2O) n H;

[0013] The polyoxyethylene fatty alcohol ether carboxylic acid and the imidazole compound are mixed at a temperature of 100 to 150° C. to obtain a curing agent.

[0014] In some embodiments, the mixing of the polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent for the carboxymethylation reaction comprises:

[0015] At a temperature of 60 to 90° C., the polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent are mixed to carry out a carboxymethylation reaction, and the reaction time is 3 to 6 hours.

[0016] In some embodiments, before mixing the polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent for carboxymethylation reaction, the method further comprises:

[0017] A basic compound is added to the polyoxyethylene fatty alcohol ether to alkalize the polyoxyethylene fatty alcohol ether to obtain the alkalized polyoxyethylene fatty alcohol ether.

[0018] In some embodiments, after the polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent are mixed for carboxymethylation reaction, the method further comprises:

[0019] The solution obtained after the carboxymethylation reaction is compressed, distilled, filtered and dried to obtain the polyoxyethylene fatty alcohol ether carboxylic acid.

[0020] In some embodiments, before compressing, distilling, filtering and drying the solution obtained after the carboxymethylation reaction, the method further comprises:

[0021] The pH of the obtained solution is adjusted to a pH range of 5 to 6.

[0022] In some embodiments, the polyoxyethylene fatty alcohol ether includes Tween, polyethylene glycol or polyoxyethylene stearyl alcohol, wherein the molecular weight of the polyethylene glycol is 200-400.

[0023] In the case of adopting the above technical solution, the present invention can provide a curing agent, whose molecular structure is Wherein, n is greater than or equal to 2, and R2 and R3 are each independently hydrogen or alkyl. The curing agent can be obtained by mixing polyoxyethylene fatty alcohol ether, alkaline compound and carboxymethylation agent for carboxymethylation reaction, and, at a temperature of 100 to 150°C, mixing polyoxyethylene fatty alcohol ether carboxylic acid obtained after the carboxymethylation reaction with imidazole compounds. The preparation method is simple, the conditions are mild, the synthetic raw materials are cheap and easy to obtain, and the single-component system formed by mixing with resin at room temperature has a long storage time and has the advantages of rapid curing under low temperature conditions. At the same time, since the curing agent is liquid at room temperature, it has good compatibility with epoxy resin. After being made into a conductive paste, it helps to improve the ductility of the paste, can reduce the occurrence of defects such as broken grids, and is conducive to ensuring conductive performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings, in which:

[0025] Figure 1is the structural formula of multiple polyoxyethylene groups provided in the examples of the present application;

[0026] Figure 2 It is a schematic diagram of the structural formula of a curing agent obtained from a carboxymethylated derivative of Tween and 2-methylimidazole provided in an embodiment of the present application;

[0027] Figure 3 It is a schematic flow chart of the method for preparing a curing agent provided in an embodiment of the present application;

[0028] Figure 4 is a schematic flow chart of a method for preparing a curing agent provided in another embodiment of the present application;

[0029] Figure 5 is a schematic flow chart of a method for preparing a curing agent provided in another embodiment of the present application;

[0030] Figure 6 It is a schematic diagram of the alkalization process and carboxymethylation reaction process provided in the examples of the present application;

[0031] Figure 7 This is a schematic diagram of the process of obtaining a curing agent from a carboxymethylated derivative of Tween and 2-methylimidazole provided in an embodiment of the present application;

[0032] Figure 8 is a graph showing the relationship between viscosity and temperature of the curing agent provided in the embodiments of the present application;

[0033] Fig. 9 is a comparison chart of epoxy resin viscosity before and after application of a curing agent provided in an embodiment of the present application;

[0034] Fig.10 This is a schematic diagram of a DSC curve of the curing agent of the present application provided in the examples of the present application. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution of the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings of the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.

[0036] The present application provides a curing agent. In some embodiments, the curing agent provided by the present application can be applied to epoxy resin. The molecular structure of the curing agent is as follows:

[0037]

[0038] Wherein, n is greater than or equal to 2, and R2 and R3 are each independently hydrogen or alkyl.

[0039] In some embodiments, R1 is one of hydrogen, an alkyl group, a stearyl alcohol group, or a sorbitan ester group.

[0040] When R1 is a sorbitol ester group, the molecular structure formula of the curing agent is:

[0042] In some embodiments, R2 and R3 may be independently an alkyl group with a carbon number of 1 to 11; in other embodiments, R2 may be an alkyl group with a carbon number of 1 to 11, and R3 may be hydrogen, such as R2 is methyl and R3 is hydrogen, or R2 is ethyl and R3 is hydrogen. In other embodiments, R2 is hydrogen and R3 is hydrogen.

[0043] The curing agent obtained in the embodiment of the present application may include multiple polyoxyethylene groups. The multiple polyoxyethylene groups constitute a long chain, which can spatially wrap the imidazole compound, thereby inhibiting the activity of the imidazole compound. After the curing agent and the epoxy resin are mixed, it is beneficial to increase the storage time of the single-component system formed after the mixing, and the curing agent is liquid at room temperature, which is beneficial to improve its compatibility with the epoxy resin.

[0044] The structural formulas of multiple polyoxyethylene groups can be found in Figure 1 In some embodiments, 6<n<10. The activity of the imidazole compound can be suppressed, so that the single-component system formed by mixing the curing agent and the epoxy resin has a longer room temperature storage time.

[0045] The imidazole compound may be 2-methylimidazole or 2-ethylimidazole, see Figure 2 As shown, Figure 2 The present invention provides a schematic diagram of the structural formula of a curing agent obtained from a carboxymethylated derivative of Tween and 2-methylimidazole. In the embodiment of the present invention, a carboxyl group of the carboxymethylated derivative of Tween is bonded to a nitrogen atom on the imidazole ring of 2-methylimidazole through an ion bond, and an oxygen atom in the carboxymethylated derivative of Tween is bonded to an amine group in 2-methylimidazole through a hydrogen bond. In the carboxymethylated derivative of Tween, x+y+z+w=20.

[0046] In another aspect, the present application provides a method for preparing a curing agent, which is used to prepare the curing agent of any of the above embodiments. Figure 3 As shown, Figure 3 : is a schematic flow chart of a method for preparing a curing agent provided in an embodiment of the present application, which may include:

[0047] Step S31: mixing the polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent to perform a carboxymethylation reaction to obtain the polyoxyethylene fatty alcohol ether carboxylic acid;

[0048] Step S32: at a temperature of not less than 100° C. and not more than 150° C., polyoxyethylene fatty alcohol ether carboxylic acid and imidazole compound are mixed to obtain a curing agent.

[0049] Among them, the chemical formula of polyoxyethylene fatty alcohol ether is R1O-(CH2CH2O) n H, that is, the polyoxyethylene fatty alcohol ether may include multiple polyoxyethylene groups and at least one hydroxyl group; the polyoxyethylene fatty alcohol ether carboxylic acid includes multiple polyoxyethylene groups, and the structural formula of multiple polyoxyethylene groups can be found in Figure 1 As shown. Multiple polyoxyethylene groups form long chains, which can subsequently wrap the imidazole compounds in space, thereby inhibiting the activity of the imidazole compounds. After the curing agent and the epoxy resin are mixed, it is beneficial to increase the storage time of the single-component system formed after the mixture, and the curing agent is liquid at room temperature, which is beneficial to improve its compatibility with the epoxy resin.

[0050] In some embodiments, the polyoxyethylene fatty alcohol ether may include n polyoxyethylene groups, wherein 6<n<10. The activity of the imidazole compound can be inhibited, so that the single-component system formed by mixing the curing agent and the epoxy resin has a longer room temperature storage time.

[0051] In some embodiments, R1 can be one of hydrogen, alkyl, stearyl alcohol group or sorbitol ester group. When R1 is a sorbitol ester group, the polyoxyethylene fatty alcohol ether can be Tween, and its chemical formula is When R1 is hydrogen, the polyoxyethylene fatty alcohol ether can be a polyethylene glycol with a low molecular weight, wherein the polyethylene glycol with a low molecular weight refers to a polyethylene glycol with a molecular weight of 200 to 400. When the molecular weight is 200 to 400, the low molecular weight polyethylene glycol can ensure the long chain structure and inhibit the activity of imidazole compounds. At the same time, it has good water solubility and surface activity, which is conducive to good compatibility with epoxy resin in the future. When R1 is a stearyl alcohol group, the polyoxyethylene fatty alcohol ether can be polyoxyethylene stearyl alcohol.

[0052] In some embodiments, step S31 may be specifically as follows: sodium hydroxide (NaOH) and chloroacetic acid (ClCH2COOH) are added to the polyoxyethylene fatty alcohol ether to perform a carboxymethylation reaction on the polyoxyethylene fatty alcohol ether to obtain polyoxyethylene fatty alcohol ether carboxylic acid. Among them, sodium hydroxide is exemplarily shown as an alkaline compound to promote the progress of the carboxymethylation reaction, and chloroacetic acid is exemplarily shown as a carboxymethylation agent. There is no particular limitation on the alkaline compound and the carboxymethylation agent, and other types of alkaline compounds and carboxymethylation agents can be selected according to needs. In some embodiments, the molar ratio in the carboxymethylation reaction can be n (polyoxyethylene fatty alcohol ether): n (NaOH): n (ClCH2COOH) = (1 to 2): (4 to 6): (2 to 3).

[0053] In some embodiments, step 31 may also be specifically adding an alkaline compound and a carboxymethylation agent to the polyoxyethylene fatty alcohol ether, reacting at a first preset temperature for a first preset time to obtain the polyoxyethylene fatty alcohol ether carboxylic acid.

[0054] The chemical formula of the corresponding polyoxyethylene fatty alcohol ether carboxylic acid is: R1O-(CH2CH2O) n -CH2COOH.

[0055] When the polyoxyethylene fatty alcohol ether is Tween, the corresponding polyoxyethylene fatty alcohol ether carboxylic acid may be a carboxymethylated derivative of Tween.

[0056] The first preset temperature and the first preset time can be set according to the requirements. By setting the first preset temperature and the first preset time, the reaction is fully carried out to obtain polyoxyethylene fatty alcohol ether carboxylic acid.

[0057] In some embodiments, the first preset temperature may be 60 to 90° C., and the first preset time may be 3 to 6 hours.

[0058] In some embodiments, step S32 can be specifically adding an imidazole compound to polyoxyethylene fatty alcohol ether carboxylic acid at a second preset temperature for dissolution, stirring the current mixed solution at a third preset temperature for a third preset time after dissolving for a second preset time to obtain a curing agent. Wherein, the third preset temperature is greater than or equal to 100°C and less than or equal to 150°C, and the third temperature is greater than the second preset temperature, and the second preset time and the third preset time can be set as required. By adding an imidazole compound to polyoxyethylene fatty alcohol ether carboxylic acid and dissolving it for a second preset time at the second preset temperature, it is beneficial to fully dissolve the imidazole compound. After mixing, by stirring the mixed solution at a higher temperature, i.e., the third preset temperature, the polyoxyethylene fatty alcohol ether carboxylic acid and the imidazole compound are fully mixed and electrostatic interaction is formed to obtain a curing agent.

[0059] In some embodiments, the imidazole compound is 2-methylimidazole, and the molar ratio of polyoxyethylene fatty alcohol ether carboxylic acid to imidazole is 1:(2-3).

[0060] In some embodiments, the second preset temperature may be 90° C., and the second preset time may be 30 minutes.

[0061] In some embodiments, the third preset temperature may preferably be 130° C., and the third preset time may be 12 hours.

[0062] In some embodiments, polyoxyethylene fatty alcohol ether carboxylic acid and imidazole compounds form electrostatic interactions through ionic bonds and / or hydrogen bonds, which can inhibit the curing activity of imidazole or imidazole derivatives. After being applied to epoxy resin, it is beneficial to prolong the room temperature storage time of the single-component system formed by the curing agent and the epoxy resin.

[0063] When the polyoxyethylene fatty alcohol ether is Tween, a carboxymethylation reaction is performed through step S31 to obtain a carboxymethylated derivative of Tween, wherein the carboxyl group in the carboxymethylated derivative of Tween is bonded to the nitrogen atom in the imidazole compound through an ionic bond, and the oxygen atom in the carboxymethylated derivative of Tween is bonded to the amine group in the imidazole compound through a hydrogen bond.

[0064] See also Figure 4 As shown, Figure 4 : is a schematic flow chart of a method for preparing a curing agent provided by another embodiment of the present application, which may include:

[0065] Step S40: adding a basic compound to the polyoxyethylene fatty alcohol ether to alkalize the polyoxyethylene fatty alcohol ether to obtain the alkalized polyoxyethylene fatty alcohol ether;

[0066] Step S41: mixing the alkalized polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent to perform a carboxymethylation reaction to obtain polyoxyethylene fatty alcohol ether carboxylic acid;

[0067] Step S42: Mixing polyoxyethylene fatty alcohol ether carboxylic acid and imidazole compound at a temperature of 100° C. or more and 150° C. or less to obtain a curing agent.

[0068] Among them, step S41 can be implemented in the same manner as step S31 by adapting the polyoxyethylene fatty alcohol ether to the alkalized polyoxyethylene fatty alcohol ether, and step S42 can be implemented in the same manner as step S32. For the sake of brevity, the details are not repeated here, and please refer to the above description.

[0069] In some embodiments, step S40 may specifically include: adding sodium hydroxide to the polyoxyethylene fatty alcohol ether to alkalize the polyoxyethylene fatty alcohol ether to obtain the alkalized polyoxyethylene fatty alcohol ether. Here, the polyoxyethylene fatty alcohol ether is alkalized with sodium hydroxide, and in other examples, other alkaline compounds that do not interfere with subsequent reactions may be used to alkalize the polyoxyethylene fatty alcohol ether. By alkalizing the polyoxyethylene fatty alcohol ether, the terminal hydroxyl groups in the polyoxyethylene fatty alcohol ether can be converted into alcohol salt ions, thereby improving the selectivity and efficiency of the subsequent carboxymethylation reaction.

[0070] In some embodiments, the molar ratio of polyoxyethylene fatty alcohol ether to sodium hydroxide may be n(polyoxyethylene fatty alcohol ether):n(NaOH)=(1-2):(0.2-0.5).

[0071] In some embodiments, step S40 can also be specifically to maintain the fourth preset time at the fourth preset temperature to alkalize the polyoxyethylene fatty alcohol ether. The fourth preset temperature and the fourth preset time can be set according to demand to fully alkalize the polyoxyethylene fatty alcohol ether.

[0072] In some embodiments, the fourth preset temperature is 40-60° C., and the fourth preset time is 0.5-2 hours.

[0073] In some embodiments, the polyoxyethylene fatty alcohol ether can be dissolved in ethanol using an organic solvent such as ethanol as a reaction medium. Step S40 can specifically be alkalizing the ethanol solution of the polyoxyethylene fatty alcohol ether. Accordingly, the subsequent step S41 can also be performed in the alkalized ethanol solution of the polyoxyethylene fatty alcohol ether.

[0074] In other embodiments, before step S42, the pH of the solution after the carboxymethylation reaction can be adjusted to neutralize the remaining alkaline substances, so that the solution obtained after the carboxymethylation reaction is weakly acidic, thereby ensuring the stability of the subsequent final curing agent. It should be noted that this embodiment can be implemented based on any of the above method embodiments.

[0075] In other embodiments, after the carboxymethylation reaction, the current solution may be compressed, distilled, filtered, and dried to obtain polyoxyethylene fatty alcohol ether carboxylic acid; and / or, after the polyoxyethylene fatty alcohol ether carboxylic acid and the imidazole compound are mixed, the current mixed solution may be filtered and purified to obtain a curing agent. For details, please refer to the description of the following embodiments.

[0076] See also Figure 5 As shown, Figure 5 : is a schematic flow chart of a method for preparing a curing agent provided by another embodiment of the present application, which may include:

[0077] Step S50: adding a basic compound to the polyoxyethylene fatty alcohol ether to alkalize the polyoxyethylene fatty alcohol ether to obtain the alkalized polyoxyethylene fatty alcohol ether;

[0078] Step S51: mixing the alkalized polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent to perform a carboxymethylation reaction;

[0079] Step S52: adjusting the pH of the solution obtained after the carboxymethylation reaction;

[0080] Step S53: compressing, distilling, filtering and drying the solution after pH adjustment to obtain polyoxyethylene fatty alcohol ether carboxylic acid;

[0081] Step S54: mixing the polyoxyethylene fatty alcohol ether carboxylic acid and the imidazole compound at a temperature of greater than or equal to 100° C. and less than or equal to 150° C. to obtain a mixed solution;

[0082] Step S55: filtering and purifying the mixed solution to obtain a curing agent.

[0083] Among them, steps S50, S51 and S54 can be implemented in the same manner as steps S40, S41 and S42. For the sake of brevity, they are not repeated here. For details, please refer to the description above.

[0084] In some embodiments, step S52 may specifically be to adjust the pH of the solution obtained after the carboxymethylation reaction to neutralize the remaining alkaline substances, so that the obtained solution is weakly acidic, thereby ensuring the stability of the final product, i.e., the curing agent. In some embodiments, the pH range may be adjusted to 5-6.

[0085] In some embodiments, step S53 can be performed by compressing, distilling, filtering and drying the pH-adjusted solution to obtain polyoxyethylene fatty alcohol ether carboxylic acid with higher purity.

[0086] In some embodiments, step S55 may specifically include: filtering the current mixed solution using a filtration device to achieve solid-liquid separation; and purifying the current mixed solution to remove impurities to obtain the target product, namely, the curing agent.

[0087] As an example, based on polyoxyethylene fatty alcohol ether R1O-(CH2CH2O) n H and imidazole compounds, and the curing agent is obtained by the curing agent preparation method provided in the above embodiment of the present application. The reactant is alkalized with NaOH at 50°C for 2 hours; NaOH and ClCH2COOH are further added, and the reaction is maintained at 80°C for 5 hours for carboxymethylation to obtain an intermediate, namely polyoxyethylene fatty alcohol ether carboxylic acid; the intermediate R1O-(CH2CH2O) n-CH2COOH and imidazole compounds are stirred at 100-150°C to obtain a curing agent. The reaction process is as follows:

[0088]

[0089]

[0090] As an example, based on Tween and 2-methylimidazole, the curing agent preparation method provided in the above embodiment of the present application can be used to obtain Figure 2 The curing agent shown.

[0091] See also Figure 6 As shown, Figure 6 The present invention provides an alkalization process and a schematic diagram of a carboxymethylation reaction process, wherein the alkalization process includes using sodium hydroxide powder to maintain the ethanol solution of Tween at 50° C. for 2 hours to alkalize the ethanol solution of Tween. The carboxymethylation reaction includes adding an appropriate amount of NaOH and chloroacetic acid (ClCH2COOH) to the alkalized ethanol solution of Tween, maintaining the carboxymethylation reaction at 80° C. for 5 hours, and obtaining a solution of a carboxymethylated derivative of Tween. The obtained solution is PH-adjusted to a pH range of 5 to 6 to obtain a Tween carboxymethylated derivative solution under weakly acidic conditions.

[0092] The carboxymethylated derivative of Tween is compressed, distilled, filtered and dried under weakly acidic conditions to obtain the carboxymethylated derivative of Tween.

[0093] See also Figure 7 As shown, Figure 7 The process of obtaining a curing agent from a carboxymethylated derivative of Tween and 2-methylimidazole provided in the embodiment of the present application is schematic. The carboxymethylated derivative of Tween and 2-methylimidazole are dissolved at 90°C for 30 minutes, and then stirred at 130°C for 12 hours to obtain a mixed solution for generating a curing agent. Finally, the mixed solution can be filtered and purified to obtain Figure 2 The curing agent shown in FIG.

[0094] In some embodiments, the molar ratio of each reactant can be n(Tween):n(ClCH2COOH):n(NaOH):n(2-methylimidazole)=1:3:4:2.

[0095] In some specific examples, a curing agent can be obtained based on Tween and 2-methylimidazole by the following steps:

[0096] Weigh 0.01 mol of Tween, dissolve it in 40 mL of anhydrous ethanol, pour the dissolved solution into a 500 mL three-necked flask, add 0.01 mol of sodium hydroxide powder to the flask, and alkalize at 50°C for 2 hours. Subsequently, weigh 0.03 mol of sodium hydroxide and 0.03 mol of chloroacetic acid, and add them to the solution three times within 30 minutes. Then raise the reaction temperature of the system to 80°C and maintain it for 5 hours to achieve complete reaction. After the reaction is completed, filter out the solid matter and retain the filtrate. Use 3 mol / L hydrochloric acid to adjust the pH of the filtrate to between 5 and 6, distill under reduced pressure, filter, retain the filtrate, and record the intermediate product as TCm, which is the carboxymethylated derivative of Tween;

[0097] The intermediate product and 0.02 mol of 2-methylimidazole were placed in a 500 mL three-necked flask, the reaction temperature was controlled to be 90°C, and the mixture was stirred and dissolved for 30 minutes at this temperature, and then the reaction temperature of the system was raised to 130°C, and stirred at this temperature for 12 hours to obtain a brown mixed liquid. The obtained mixed liquid was purified and filtered using an acetone solution, the filtrate was retained, and the solvent in the system was removed by reduced pressure distillation to obtain the final product, i.e., the curing agent.

[0098] See also Figure 8 Shown and Fig. 9 As shown, Figure 8 is a graph showing the relationship between viscosity and temperature of the curing agent provided in the embodiments of the present application, Fig. 9 This is a comparison chart of the viscosity of epoxy resin before and after the application of curing agent provided in the embodiment of the present application. Among them, three types of curing agents are shown: TC20-2MI, TC60-2MI and TC80-2MI, TC represents Tween, MI represents methylimidazole, that is, the curing agent formed by Tween 20, Tween 60 and Tween 80 and 2-methylimidazole, and the epoxy resin is represented by E51. It can be seen from the above figure that the curing agent provided by the present application has a low viscosity at room temperature and can be in a liquid state. After mixing with the epoxy resin (E51), it can significantly reduce the viscosity of the system and has good compatibility.

[0099] See also Fig.10 As shown, Fig.10 The DSC (Differential Scanning Calorimetry) curve diagram provided in the embodiment of the present application is shown in the figure. Multiple curves obtained at different scanning rates such as 5°C / min, 10°C / min, etc. It can be seen from the figure that the curing agent provided by the present application is applied to the single-component system formed with E51, and the curing peak temperature is about 130-150°C, indicating that the curing agent has a long storage period after being mixed with epoxy resin at room temperature, and at the same time, the curing temperature is low, the curing speed is fast, and it is more convenient to use.

[0100] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. A curing agent, characterized in that The molecular structure is as follows: Wherein, n is greater than or equal to 2, and R2 and R3 are each independently hydrogen or alkyl.

2. The curing agent according to claim 1, characterized in that R1 is one of hydrogen, an alkyl group, a stearyl alcohol group or a sorbitan ester group.

3. The curing agent according to claim 1, characterized in that R2 is an alkyl group having 1 to 11 carbon atoms, and R3 is hydrogen.

4. The curing agent according to claim 3, characterized in that R2 is methyl.

5. The curing agent according to any one of claims 1 to 4, characterized in that 6<n<10。 6. A method for preparing a curing agent, characterized in that: The method is used to prepare the curing agent according to any one of claims 1 to 5, and the method comprises: The polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent are mixed to perform a carboxymethylation reaction to obtain the polyoxyethylene fatty alcohol ether carboxylic acid; the chemical formula of the polyoxyethylene fatty alcohol ether is R1O-(CH2CH2O) n H; The polyoxyethylene fatty alcohol ether carboxylic acid and the imidazole compound are mixed at a temperature of 100 to 150° C. to obtain a curing agent.

7. The method according to claim 6, characterized in that The method of mixing the polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent for the carboxymethylation reaction comprises: At a temperature of 60 to 90° C., the polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent are mixed to carry out a carboxymethylation reaction, and the reaction time is 3 to 6 hours.

8. The method according to claim 6, characterized in that Before mixing the polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent for carboxymethylation reaction, the method further comprises: A basic compound is added to the polyoxyethylene fatty alcohol ether to alkalize the polyoxyethylene fatty alcohol ether to obtain the alkalized polyoxyethylene fatty alcohol ether.

9. The method according to claim 6, characterized in that After the polyoxyethylene fatty alcohol ether, the alkaline compound and the carboxymethylation agent are mixed for carboxymethylation reaction, the method further comprises: The solution obtained after the carboxymethylation reaction is compressed, distilled, filtered and dried to obtain the polyoxyethylene fatty alcohol ether carboxylic acid.

10. The method according to claim 9, characterized in that Before compressing, distilling, filtering and drying the solution obtained after the carboxymethylation reaction, the method further comprises: The pH of the obtained solution is adjusted to a pH range of 5 to 6.

11. The method according to any one of claims 6 to 10, characterized in that The polyoxyethylene fatty alcohol ether includes Tween, polyethylene glycol or polyoxyethylene stearyl alcohol, wherein the molecular weight of the polyethylene glycol is 200-400.