Temperature-resistant and corrosion-resistant phenyl polysiloxane and preparation method thereof

By combining modified phenyl polysiloxane, graphite interlayer compounds, and glucomannan, a stable multilayer film structure is formed, which solves the problem of insufficient heat resistance and corrosion resistance of phenyl polysiloxane and achieves a significant improvement in heat resistance and corrosion resistance.

CN118931206AInactive Publication Date: 2024-11-12BENGBU AIYOU NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411271529.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing phenyl polysiloxane has an unstable film-forming interface, resulting in low heat resistance and corrosion resistance.

Method used

By adding modified phenyl polysiloxane, graphite interlayer compounds, glucomannan, and photoinitiators, a three-dimensional network structure and stable multilayer films are formed. The chemical bonds of diphenyl phosphite and naphthalimide are used to improve the degree of crosslinking. Combining the film-forming properties of glucomannan and the layered structure of graphite, the heat resistance and corrosion resistance are enhanced.

Benefits of technology

It significantly improves the heat resistance and corrosion resistance of phenyl polysiloxane, forms a stable three-layer structure, blocks heat transfer and prevents molecular intrusion, and enhances the adhesion of the film layer.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses temperature-resistant and corrosion-resistant phenyl polysiloxane, and relates to the technical field of polysiloxane, the temperature-resistant and corrosion-resistant phenyl polysiloxane comprises the following raw materials: modified phenyl polysiloxane, a graphite interlayer compound, glucomannan and a photoinitiator; the modified phenyl polysiloxane is prepared from the following raw materials: phenyl polysiloxane, diphenyl phosphite, naphthyl dialkenyl imide and a catalyst; the preparation method comprises the following steps: adding glucomannan and a graphite interlayer compound into tetrahydrofuran, and fully dissolving to form a solution M; adding modified polysiloxane into the solution M, and fully dissolving to form a solution N; filtering the solution N to obtain a filtrate, adding a photoinitiator, and uniformly stirring to form a solution L; a layer of the solution L is spread on a glass plate, UV irradiation is used for forming a first layer of thin film, a layer of the solution L is spread on the first layer of thin film, UV irradiation is used for forming a double-layer thin film, a layer of the solution L is spread on the second layer of thin film, and UV irradiation is used for obtaining the phenyl polysiloxane precursor which has excellent heat resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polysiloxanes, and in particular to a temperature-resistant and corrosion-resistant phenyl polysiloxane and a preparation method thereof. Background Art

[0002] Polysiloxane, also known as silicone oil, is generally a colorless (or light yellow), odorless, non-toxic, non-volatile liquid. Silicone oil is insoluble in water, methanol, ethylene glycol and 2-ethoxyethanol, but is miscible with benzene, dimethyl ether, methyl ethyl ketone, carbon tetrachloride or kerosene, slightly soluble in acetone, dioxane, ethanol and butanol, and easily soluble in benzene, toluene, xylene, ether and chloroalkanes. It has a very small vapor pressure, a high flash point and ignition point, a low freezing point, good thermal stability, and a gelation time of 1750h in hot air at 250°C. It also has good radiation resistance, extremely high oxidation stability, heat resistance, flame resistance, UV resistance and chemical resistance.

[0003] Phenyl silicone oil, i.e. phenyl polysiloxane, is the product in which part of the methyl groups in methyl polysiloxane are replaced by phenyl groups. It has a small coefficient of thermal expansion and can be prepared by polyolation reaction of the hydrolyzate of octamethylcyclotetrasiloxane, dimethyltetraphenyldisiloxane and methylphenyldiethoxysilane in the presence of a catalyst.

[0004] In the prior art, due to the good properties of phenyl polysiloxane, in addition to being used as a lubricating liquid or electrolyte, phenyl polysiloxane can also be compounded with other materials to form a coating or film layer. However, since the silicon-oxygen bonds in phenyl polysiloxane are very flexible, the film-forming interface of phenyl polysiloxane is unstable, which in turn leads to its low heat resistance and corrosion resistance. Summary of the invention

[0005] The purpose of the present invention is to provide a heat-resistant and corrosion-resistant phenyl polysiloxane and a preparation method thereof; to solve the following technical problems:

[0006] How to improve the heat resistance and corrosion resistance of polysiloxane?

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] In a first aspect, the present invention discloses a heat-resistant and corrosion-resistant phenyl polysiloxane, comprising the following raw materials in parts by weight: 35-50 parts of modified phenyl polysiloxane, 3-8 parts of graphite interlayer compound, 25-30 parts of glucomannan, and 0.1-1 parts of photoinitiator;

[0009] Preferably, the modified phenyl polysiloxane is 40-45 parts, the graphite interlayer compound is 5-7 parts, the glucomannan is 26-29 parts, and the photoinitiator is 0.2-0.8 parts; more preferably, the modified phenyl polysiloxane is 45 parts, the graphite interlayer compound is 6 parts, the glucomannan is 28 parts, and the photoinitiator is 0.5 parts.

[0010] The raw materials of the modified phenyl polysiloxane include phenyl polysiloxane, diphenyl phosphite, naphthyl diene imide and a catalyst, and the weight ratio of the four is (15:30): (5-10): (5-10): (0.2-1), preferably (20:25): (6-9): (6-9): (0.4-0.8), and more preferably 22:8:8:0.6.

[0011] In a further embodiment of the present invention, the preparation method of the modified phenyl polysiloxane is:

[0012] Step 1: dissolving phenyl polysiloxane, diphenyl phosphite and naphthalene diimide in toluene solvent in proportion, and stirring well to form a solution A with a mass fraction of 35-45%; the mass fraction is preferably 38-42%, and more preferably 40%;

[0013] Step 2: adding a catalyst to solution A, followed by stirring at 60-80° C. for 3-5 hours at a stirring rate of 500-600 rpm to obtain solution B; evaporating solution B to remove the solvent toluene to obtain modified phenyl polysiloxane.

[0014] In a further embodiment of the present invention: in the second step, the catalyst is a KARSTEDT catalyst or chloroplatinic acid, preferably a KARSTEDT catalyst.

[0015] In a further embodiment of the present invention: in the second step, solution B is evaporated by rotary evaporation.

[0016] In diphenyl phosphite, the phenyl group is connected to the phosphoryl group through an oxygen atom, and the oxygen atom in the phosphoryl group has the properties of hydroxyl oxygen. Since it forms a covalent bond with the phosphorus atom and has a certain reactivity in the molecule, it can be grafted onto the side chain of phenyl polysiloxane, thereby improving the heat resistance of phenyl polysiloxane and increasing the number of phenyl groups in phenyl polysiloxane; in naphthalene diimide, the naphthyl group is used as the core structure, and is connected to other groups such as imide group, carbonyl group and other substituents through chemical bonds. The naphthyl group is a rigid twisted group. After the introduction of phenyl polysiloxane, it is cross-linked with its side chain to form a three-dimensional network structure, which can inhibit the interchain stacking of the molecular chain, reduce the rotational fluidity around the flexible chain, and greatly increase its cross-linking degree, thereby improving its stability.

[0017] In a further embodiment of the present invention, the graphite interlayer compound is prepared by heating metallic potassium to above 760°C under the protection of an inert gas, such as argon, to form potassium vapor, exposing pure graphite powder to the potassium vapor and stirring it for 0.5-1h to obtain the graphite interlayer compound.

[0018] In a further embodiment of the present invention, the usage ratio of the metallic potassium to the graphite powder is 1 g:(1.8-2) g.

[0019] In a second aspect, the present invention further discloses a method for preparing the heat-resistant and corrosion-resistant phenyl polysiloxane as described above, comprising the following steps:

[0020] S1: Add glucomannan and graphite interlayer compound to tetrahydrofuran, stir at high speed until fully dissolved, and form solution M with a mass fraction of 15-20%; add modified polysiloxane to solution M in 2-3 times, stir ultrasonically until fully dissolved, and form solution N;

[0021] S2: Filtering solution N to obtain a filtrate, adding a photoinitiator to the filtrate and stirring evenly to form a solution L;

[0022] S3: prepare a glass plate, spread a layer of solution L on the glass plate, irradiate with UV for 0.5-1 min to form a first thin film, spread another layer of solution L on the first thin film, irradiate with UV at 80-100° C. for 0.5-1 min, spread another layer of solution L on the second thin film, irradiate with UV for 2-3 min, and obtain a phenyl polysiloxane precursor;

[0023] S4: vacuum drying the phenyl polysiloxane precursor to obtain heat-resistant and corrosion-resistant phenyl polysiloxane.

[0024] In a further embodiment of the present invention: in step S2, the photoinitiator is diphenylacetophenone or isopropylferrocenium hexafluorophosphate.

[0025] Glucomannan contains a large number of carboxyl groups, hydroxyl groups, and amine groups, and has excellent film-forming properties. After combining with modified phenyl polysiloxane, it can improve the film-forming properties of modified phenyl polysiloxane and reduce the influence of rigid groups in modified phenyl polysiloxane on film formation. At the same time, glucomannan also contains a large number of ether oxygen bonds, which have a strong affinity for carbon dioxide, so it can also improve heat resistance and flame retardancy. The graphite in the graphite interlayer compound has a layered structure, which is cross-linked with the phosphorus atoms in the modified polysiloxane to form a stable carbon layer, which can isolate the transfer of heat and the invasion of other substances. At the same time, when the multi-layer film is superimposed by UV irradiation, the epoxy groups in the film will produce secondary hydroxyl groups under the action of UV, which increases the polarity. At this time, superimposing the film upward can enhance the bonding force between the film layers and form a stable three-layer phenyl polysiloxane structure, which can not only block heat transfer, but also prevent other molecules from entering the film layer, thereby improving its corrosion resistance.

[0026] In a further embodiment of the present invention: in step S3, each layer of solution L is evenly spread using a wire rod, with a spreading thickness of 1-3 mm.

[0027] In a further embodiment of the present invention, the method for vacuum drying the phenyl polysiloxane precursor is as follows: placing the phenyl polysiloxane precursor in a vacuum oven at 30-40° C. and drying it for 40-48 hours.

[0028] Beneficial effects of the present invention:

[0029] (1) In the heat-resistant and corrosion-resistant phenyl polysiloxane of the present invention, diphenyl phosphite is added, and the phenyl group is connected to the phosphoryl group through an oxygen atom. The oxygen atom in the phosphoryl group has the properties of hydroxyl oxygen because it forms a covalent bond with the phosphorus atom and has a certain reactivity in the molecule. It can be grafted onto the side chain of phenyl polysiloxane, thereby improving the heat resistance of phenyl polysiloxane.

[0030] (2) In the heat-resistant and corrosion-resistant phenyl polysiloxane of the present invention, the added naphthalene diimide has a naphthyl group as the core structure and is connected to other groups, such as an imide group, a carbonyl group and other substituents, through chemical bonds. The naphthyl group is a rigid twisted group. After the phenyl polysiloxane is introduced, it is cross-linked with its side chains to form a three-dimensional network structure, which can inhibit the interchain stacking of the molecular chain, reduce the rotational fluidity around the flexible chain, and greatly improve its cross-linking degree, thereby improving its stability, heat resistance and corrosion resistance.

[0031] (3) In the heat-resistant and corrosion-resistant phenyl polysiloxane of the present invention, the added glucomannan contains a large amount of carboxyl groups, hydroxyl groups, and amine groups, and has excellent film-forming properties. After being combined with the modified phenyl polysiloxane, the film-forming properties of the modified phenyl polysiloxane can be improved, and the influence of the rigid groups in the modified phenyl polysiloxane on the film formation can be reduced; at the same time, glucomannan also contains a large amount of ether oxygen bonds, which have a strong affinity for carbon dioxide, and thus the heat resistance and flame retardancy can also be improved.

[0032] (4) In the heat-resistant and corrosion-resistant phenyl polysiloxane of the present invention, the graphite in the added graphite interlayer compound has a layered structure, which is cross-linked with the phosphorus atoms in the modified polysiloxane to form a stable carbon layer, which can isolate the transfer of heat and the intrusion of other substances.

[0033] (5) In the heat-resistant and corrosion-resistant phenyl polysiloxane of the present invention, when multiple layers of thin films are stacked and irradiated with UV, the epoxy groups in the thin films will produce secondary hydroxyl groups under the action of UV, thereby increasing the polarity. At this time, stacking the thin films upward can enhance the bonding force between the thin film layers, forming a stable three-layer phenyl polysiloxane structure, which can not only block heat transfer, but also prevent other molecules from entering the interior of the film layer, thereby improving its corrosion resistance. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.

[0035] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0036] Example 1

[0037] Preparation of modified phenyl polysiloxane:

[0038] 220 g of phenyl polysiloxane, 80 g of diphenyl phosphite and 80 g of naphthalene diimide were added to a stirring tank, and then 950 g of toluene was added, and stirred at 600 rpm for 30 min to form a solution A with a mass fraction of 40%; 6 g of KARSTEDT catalyst was added to solution A, and then stirred at 550 rpm for 4 h at 70°C to obtain solution B; solution B was rotary evaporated to remove toluene, and modified phenyl polysiloxane was obtained.

[0039] Example 2

[0040] Preparation of modified phenyl polysiloxane:

[0041] 220 g of phenyl polysiloxane and 80 g of diphenyl phosphite were added to an ultrasonic stirrer, and then 750 g of toluene was added, and the mixture was stirred at 600 rpm for 30 min to form a solution A with a mass fraction of 40%; 6 g of KARSTEDT catalyst was added to solution A, and then the mixture was stirred at 550 rpm for 4 h at 70° C. to obtain a solution B; solution B was rotary evaporated to remove toluene, thereby obtaining modified phenyl polysiloxane.

[0042] Example 3

[0043] 220 g of phenyl polysiloxane and 80 g of naphthalene diimide were added to an ultrasonic stirrer, and then 750 g of toluene was added, and the mixture was stirred at 600 rpm for 30 min to form a solution A with a mass fraction of 40%; 6 g of KARSTEDT catalyst was added to solution A, and then the mixture was stirred at 550 rpm for 4 h at 70°C to obtain a solution B; solution B was rotary evaporated to remove toluene, thereby obtaining modified phenyl polysiloxane.

[0044] Example 4

[0045] Preparation of graphite intercalation compounds

[0046] Under argon protection, 20 g of metallic potassium is heated to above 760° C. to form potassium vapor, and 38 g of pure graphite powder is exposed to the potassium vapor and stirred for 0.5-1 h to obtain a graphite interlayer compound.

[0047] Example 5

[0048] 186 g of tetrahydrofuran was added to an ultrasonic stirrer, and then 25 g of glucomannan and 3 g of the graphite interlayer compound obtained in Example 4 were added, and the mixture was stirred at 600 rpm for 20 min to form a solution M with a mass fraction of 15; then 35 g of the modified polysiloxane obtained in Example 1 was added to the solution M in two times, 20 g was added for the first time, and ultrasonic stirring was performed for 10 min, and then 15 g was added for the second time, and ultrasonic stirring was performed for 20 min to form a solution N; the solution N was filtered through a 1000 mesh sieve to obtain a filtrate, and 0.1 g of a photoinitiator was added to the filtrate and stirred evenly to form a solution L; Prepare a glass plate, use a wire rod to spread a layer of solution L on the glass plate with a thickness of 2 mm, use UV irradiation at 90°C for 1 min to form a first thin film, spread another layer of solution L on the first thin film, also with a thickness of 2 mm, use UV irradiation at 90°C for 1 min to form a double-layer thin film, spread another layer of solution L on the second thin film, use UV irradiation at 90°C for 3 min to obtain a phenyl polysiloxane precursor with a three-layer structure; place the phenyl polysiloxane precursor in a vacuum box at 30°C and dry it for 48 hours to obtain heat-resistant and corrosion-resistant phenyl polysiloxane.

[0049] Example 5

[0050] 186 g of tetrahydrofuran was added to an ultrasonic stirrer, and then 25 g of glucomannan and 3 g of the graphite interlayer compound obtained in Example 4 were added, and stirred at 600 rpm for 20 min to form a solution M with a mass fraction of 15%; then 35 g of the modified polysiloxane obtained in Example 1 was added to the solution M in two times, 20 g was added for the first time, and ultrasonic stirring was performed for 10 min, and then 15 g was added for the second time, and ultrasonic stirring was performed for 20 min to form a solution N; the solution N was filtered through a 1000 mesh sieve to obtain a filtrate, and 0.1 g of a photoinitiator was added to the filtrate and stirred evenly to form a solution L ; Prepare a glass plate, use a wire rod to spread a layer of solution L on the glass plate with a thickness of 2 mm, use UV irradiation at 90°C for 1 min to form a first thin film, spread another layer of solution L on the first thin film, also with a thickness of 2 mm, use UV irradiation at 90°C for 1 min to form a double-layer thin film, spread another layer of solution L on the second thin film, use UV irradiation at 90°C for 3 min to obtain a phenyl polysiloxane precursor with a three-layer structure; place the phenyl polysiloxane precursor in a vacuum box at 30°C and dry it for 48 hours to obtain heat-resistant and corrosion-resistant phenyl polysiloxane.

[0051] Example 6

[0052] 155 g of tetrahydrofuran was added to an ultrasonic stirrer, and then 26 g of glucomannan and 5 g of the graphite interlayer compound obtained in Example 4 were added, and the mixture was stirred at 600 rpm for 20 min to form a solution M with a mass fraction of 20%; then 40 g of the modified polysiloxane obtained in Example 1 was added to the solution M in three times, 10 g was added for the first time, and 15 g was added for the second time after ultrasonic stirring for 5 min, and 15 g was added for the third time after ultrasonic stirring for 10 min, and ultrasonic stirring was performed for 20 min to form a solution N; the solution N was filtered through a 1000 mesh sieve to obtain a filtrate, and 0.2 g of a photoinitiator was added to the filtrate and stirred. Stir evenly to form a solution L; prepare a glass plate, use a wire rod to spread a layer of solution L on the glass plate with a thickness of 2 mm, use UV irradiation at 90°C for 1 min to form a first thin film, spread another layer of solution L on the first thin film, and use UV irradiation at 90°C for 1 min to form a double-layer thin film, spread another layer of solution L on the second thin film, and use UV irradiation at 90°C for 3 min to obtain a phenyl polysiloxane precursor with a three-layer structure; place the phenyl polysiloxane precursor in a vacuum box at 35°C and dry it for 45 hours to obtain heat-resistant and corrosion-resistant phenyl polysiloxane.

[0053] Example 7

[0054] 170 g of tetrahydrofuran was added to an ultrasonic stirrer, and then 28 g of glucomannan and 6 g of the graphite interlayer compound obtained in Example 4 were added, and the mixture was stirred at 600 rpm for 20 min to form a solution M with a mass fraction of 20%; then 45 g of the modified polysiloxane obtained in Example 1 was added to the solution M in three times, 15 g was added for the first time, and ultrasonic stirring was performed for 5 min, and 15 g was added for the second time, and ultrasonic stirring was performed for 10 min, and 15 g was added for the third time, and ultrasonic stirring was performed for 20 min to form a solution N; the solution N was filtered through a 1000 mesh sieve to obtain a filtrate, and 0.5 g of a photoinitiator was added to the filtrate and stirred. Stir evenly to form a solution L; prepare a glass plate, use a wire rod to spread a layer of solution L on the glass plate with a thickness of 2 mm, use UV irradiation at 90°C for 1 min to form a first thin film, spread another layer of solution L on the first thin film, and use UV irradiation at 90°C for 1 min to form a double-layer thin film, spread another layer of solution L on the second thin film, and use UV irradiation at 90°C for 3 min to obtain a phenyl polysiloxane precursor with a three-layer structure; place the phenyl polysiloxane precursor in a vacuum box at 35°C and dry it for 45 hours to obtain heat-resistant and corrosion-resistant phenyl polysiloxane.

[0055] Example 8

[0056] 180 g of tetrahydrofuran was added to an ultrasonic stirrer, and then 29 g of glucomannan and 7 g of the graphite interlayer compound obtained in Example 4 were added, and the mixture was stirred at 600 rpm for 20 min to form a solution M with a mass fraction of 20%; then 45 g of the modified polysiloxane obtained in Example 1 was added to the solution M in three times, 15 g was added for the first time, and ultrasonic stirring was performed for 5 min, and 15 g was added for the second time, and ultrasonic stirring was performed for 10 min, and 15 g was added for the third time, and ultrasonic stirring was performed for 20 min to form a solution N; the solution N was filtered through a 1000 mesh sieve to obtain a filtrate, and 0.8 g of a photoinitiator was added to the filtrate and stirred. Stir evenly to form a solution L; prepare a glass plate, use a wire rod to spread a layer of solution L on the glass plate with a thickness of 2 mm, use UV irradiation at 90°C for 1 min to form a first thin film, spread another layer of solution L on the first thin film, and use UV irradiation at 90°C for 1 min to form a double-layer thin film, spread another layer of solution L on the second thin film, and use UV irradiation at 90°C for 3 min to obtain a phenyl polysiloxane precursor with a three-layer structure; place the phenyl polysiloxane precursor in a vacuum box at 35°C and dry it for 45 hours to obtain heat-resistant and corrosion-resistant phenyl polysiloxane.

[0057] Example 9

[0058] 152 g of tetrahydrofuran was added to an ultrasonic stirrer, followed by 30 g of glucomannan and 8 g of a graphite interlayer compound, and the mixture was stirred at 600 rpm for 20 min to form a solution M having a mass fraction of 25%; 50 g of the modified polysiloxane obtained in Example 1 was added to the solution M in three portions, 15 g was added for the first time, and ultrasonic stirring was performed for 5 min, followed by 15 g was added for the second time, and ultrasonic stirring was performed for 10 min, followed by 20 g was added for the third time, and ultrasonic stirring was performed for 20 min to form a solution N; the solution N was filtered using a 1000 mesh sieve to obtain a filtrate, 1 g of a photoinitiator was added to the filtrate, and the mixture was stirred evenly to form a solution N; A solution L is formed; a glass plate is prepared, and a wire rod is used to spread a layer of solution L on the glass plate with a thickness of 2 mm, and UV irradiation is performed at 90°C for 1 min to form a first thin film, and another layer of solution L is spread on the first thin film with a thickness of 2 mm, and UV irradiation is performed at 90°C for 1 min to form a double-layer thin film, and another layer of solution L is spread on the second thin film, and UV irradiation is performed at 90°C for 3 min to obtain a phenyl polysiloxane precursor with a three-layer structure; the phenyl polysiloxane precursor is placed in a vacuum box at 40°C and dried for 40 hours to obtain heat-resistant and corrosion-resistant phenyl polysiloxane.

[0059] Comparative Example 1

[0060] Compared with Example 7, the only difference is that the modified polysiloxane prepared in Example 1 is replaced by the modified polysiloxane prepared in Example 2.

[0061] Comparative Example 2

[0062] Compared with Example 7, the only difference is that the modified polysiloxane prepared in Example 1 is replaced by the modified polysiloxane prepared in Example 3.

[0063] Comparative Example 3

[0064] Compared with Example 7, the only difference is that no graphite interlayer compound is added.

[0065] Comparative Example 4

[0066] Compared with Example 7, the only difference is that the UV irradiation of each layer of the film is replaced by standing for 3 hours.

[0067] The phenyl polysiloxanes prepared in Examples 5-9 and Comparative Examples 1-4 were subjected to heat resistance and corrosion resistance tests. The test method was as follows: the phenyl polysiloxanes prepared in each example and comparative example were cut into two equal halves, which were generally used for heat resistance tests and corrosion resistance tests.

[0068] Heat resistance test: The prepared phenyl polysiloxane was subjected to the same high and low temperature cycle test, and its shrinkage rate was tested after the test.

[0069] Corrosion resistance test: The prepared phenyl polysiloxane was first immersed in a 75% hydrochloric acid solution for 12 hours, and then immersed in a 75% sodium hydroxide solution for 12 hours. After the immersion, the phenyl polysiloxane was taken out and observed to see if cracks, discoloration, or deformation occurred on the surface.

[0070] The test results are listed in Table 1, which is as follows:

[0071] Table 1

[0072] Shrinkage rate (%) Surface condition after acid and alkali immersion Example 5 0.95 No cracks, no discoloration, no deformation Example 6 0.82 No cracks, no discoloration, no deformation Example 7 0.66 No cracks, no discoloration, no deformation Example 8 0.72 No cracks, no discoloration, no deformation Example 9 0.89 No cracks, no discoloration, no deformation Comparative Example 1 2.23 A small amount of cracks, a large discoloration area, and no deformation Comparative Example 2 2.65 A small amount of cracks, a large discoloration area, and no deformation Comparative Example 3 3.12 A large number of cracks, large discoloration area, and severe deformation Comparative Example 4 3.23 A large number of cracks, large discoloration area, and severe deformation

[0073] By analyzing the data in Table 1, it can be seen that the heat-resistant and corrosion-resistant phenyl polysiloxanes obtained in Examples 5-9 have stronger heat resistance and corrosion resistance than those in Comparative Examples 1-4, which indicates that the phenyl polysiloxanes obtained in the present invention have stronger heat resistance and corrosion resistance.

[0074] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A heat-resistant and corrosion-resistant phenyl polysiloxane, characterized in that: The method comprises the following raw materials in parts by weight: 35-50 parts of modified phenyl polysiloxane, 3-8 parts of graphite interlayer compound, 45-60 parts of glucomannan, and 0.1-1 parts of photoinitiator; The raw materials of the modified phenyl polysiloxane include phenyl polysiloxane, diphenyl phosphite, naphthyl diene imide and a catalyst, and the weight ratio of the four is (15:30): (5-10): (5-10): (0.2-1).

2. The heat-resistant and corrosion-resistant phenyl polysiloxane according to claim 1, characterized in that: The preparation method of the modified phenyl polysiloxane is: The first step: dissolving phenyl polysiloxane, diphenyl phosphite and naphthalene diimide in toluene solvent in proportion to form a solution A with a mass fraction of 35-45%; Step 2: adding a catalyst to solution A, followed by stirring at 60-80° C. for 3-5 hours to obtain solution B; evaporating solution B to remove the solvent toluene to obtain modified phenyl polysiloxane.

3. The heat-resistant and corrosion-resistant phenyl polysiloxane according to claim 2, characterized in that: In the second step, the catalyst is KARSTEDT catalyst or chloroplatinic acid.

4. The heat-resistant and corrosion-resistant phenyl polysiloxane according to claim 2, characterized in that: In the second step, solution B was evaporated by rotary evaporation.

5. The heat-resistant and corrosion-resistant phenyl polysiloxane according to claim 1, characterized in that: The preparation method of the graphite interlayer compound is: Under the protection of inert gas, potassium metal is heated to above 760°C to form potassium vapor, and graphite powder is exposed to the potassium vapor and fully stirred for 0.5-1h to obtain a graphite interlayer compound.

6. The heat-resistant and corrosion-resistant phenyl polysiloxane according to claim 5, characterized in that: The usage ratio of the metallic potassium to the graphite powder is 1g:(1.8-2)g.

7. A method for preparing the heat-resistant and corrosion-resistant phenyl polysiloxane according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: Add glucomannan and graphite intercalation compound to tetrahydrofuran, stir at high speed until fully dissolved, and form a solution M with a mass fraction of 15-20%; Add the modified polysiloxane to solution M in 2-3 portions, and stir by ultrasonic until fully dissolved to form solution N; S2: Filtering solution N to obtain a filtrate, adding a photoinitiator to the filtrate and stirring evenly to form a solution L; S3: prepare a glass plate, spread a layer of solution L on the glass plate, irradiate with UV for 0.5-1 min to form a first thin film, spread another layer of solution L on the first thin film, irradiate with UV at 80-100° C. for 0.5-1 min, spread another layer of solution L on the second thin film, irradiate with UV for 2-3 min, and obtain a phenyl polysiloxane precursor; S4: vacuum drying the phenyl polysiloxane precursor to obtain heat-resistant and corrosion-resistant phenyl polysiloxane.

8. The method for preparing the heat-resistant and corrosion-resistant phenyl polysiloxane according to claim 7, characterized in that: In step S2, the photoinitiator is diphenylacetophenone or cumene ferrocenium hexafluorophosphate.

9. The method for preparing the heat-resistant and corrosion-resistant phenyl polysiloxane according to claim 7, characterized in that: In step S3, each layer of solution L is evenly spread using a wire rod, with a spreading thickness of 1-3 mm.

10. The method for preparing the heat-resistant and corrosion-resistant phenyl polysiloxane according to claim 7, characterized in that: The method for vacuum drying the phenyl polysiloxane precursor is as follows: placing the phenyl polysiloxane precursor in a vacuum box at 30-40° C. and drying it for 40-48 hours.