Liquid crystal polymer composite material as well as preparation method and application thereof

The preparation of liquid crystal polymer composite materials has solved the problem of static electricity accumulation in steel pipes during the transportation of flammable and explosive chemicals, providing excellent antistatic properties and stable mechanical properties, making it suitable for pipelines transporting flammable and explosive chemicals.

CN118931222AInactive Publication Date: 2024-11-12ZHEJIANG YUANBANG MATERIAL TECH

Patent Information

Application Number
CN202411436191.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118931222A_ABST
    Figure CN118931222A_ABST
Patent Text Reader

Abstract

The invention provides a liquid crystal polymer composite material as well as a preparation method and application thereof. The liquid crystal polymer composite material comprises the following raw material components in percentage by weight: 20-30% of a liquid crystal polymer; 50-75% of continuous glass fiber filaments modified by a coupling agent; 1-10% of a polymer alloy; 3-15% of stainless steel fiber modified by a coupling agent; the polymer alloy is selected from one or two of polyphenyl ether resin and polyaryletherketone resin. The liquid crystal polymer, the continuous glass fiber filaments, the polymer alloy and the stainless steel fibers are compounded, so that the liquid crystal polymer composite material has better mechanical properties, and is low in density, corrosion-resistant, antistatic and good in flame retardant property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymer composite materials, and in particular to a liquid crystal polymer composite material and a preparation method and application thereof. Background Art

[0002] Steel pipes, as a traditional piping material, play an important role in the transportation of flammable and explosive chemicals. They are well-known for their strong and durable characteristics, but they also face the challenge of static electricity accumulation.

[0003] Steel pipes themselves are not good antistatic materials because they are good conductors of electricity and can conduct static electricity. However, in the special environment of transporting flammable and explosive materials, static electricity accumulation may cause serious safety hazards. To reduce this risk, current technology reduces the generation and accumulation of static electricity by applying antistatic coatings. Nevertheless, this method still faces some potential problems:

[0004] (1) Adhesion problem: The coating must be tightly bonded to the steel pipe substrate to ensure stability under changing usage conditions. If the adhesion is insufficient, the coating may peel off prematurely, affecting its overall performance.

[0005] (2) Thickness uniformity: The thickness of the coating must be consistent to ensure uniform distribution of the antistatic effect. Uneven thickness may result in substandard antistatic performance in some areas.

[0006] Therefore, in order to improve safety and reliability, it is urgent to develop a new generation of pipes with excellent antistatic properties to meet the strict requirements of flammable and explosive chemical transportation. Summary of the invention

[0007] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a liquid crystal polymer composite material and a preparation method and use thereof, so as to solve the problems existing in the prior art.

[0008] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.

[0009] The present invention provides a liquid crystal polymer composite material, comprising the following raw material components in percentage by weight: Liquid crystal polymer 20~30%; Continuous glass fiber filaments treated with coupling agent 50~75%; Polymer alloy 1~10%; Stainless steel fiber treated with coupling agent 3~15%; The polymer alloy is one or two selected from polyphenylene ether resin and polyaryletherketone resin.

[0010] For example, the amount of liquid crystal polymer used can be 20~21.8%, 21.8~25%, 25~27%, 27~29%, or 29~30%.

[0011] For example, the dosage of continuous glass fiber filaments can be 50~55%, 55~56.3%, 56.3~60%, 60~66.2%, 66.2~70%, 70~72%, and 72~75%.

[0012] For example, the dosage of polymer alloy can be 1~1.4%, 1.4~2%, 2~3%, 3~4%, 4~5%, 5~6%, 6~7%, 7~8%, 8~9%, and 9~10%.

[0013] For example, the dosage of stainless steel fiber can be 3~3.2%, 3.2~5.4%, 5.4~6%, 6~7%, 7~8%, 8~9.7%, 9.7~10%, 10~11%, and 10~15%.

[0014] Preferably, the liquid crystal polymer composite material comprises the following raw material components in percentage by weight: Liquid crystal polymer 20~30%; Continuous glass fiber filament treated with coupling agent 55~75%; Polymer alloy 1~4%; The coupling agent is changed to 3~11% of stainless steel fiber after treatment.

[0015] More preferably, the liquid crystal polymer composite material comprises the following raw material components in percentage by weight: Liquid crystal polymer 25~30%; Continuous glass fiber filament treated with coupling agent 55~70%; Polymer alloy 1~4%; The coupling agent is changed to 3~11% of stainless steel fiber after treatment.

[0016] Preferably, the liquid crystal polymer composite material is a sheet obtained by impregnating a molten impregnant onto a plurality of rows of parallel continuous glass fiber filaments and then hot pressing the impregnated material to form the sheet.

[0017] More preferably, the liquid crystal polymer composite material comprises a plurality of stacked sheets. Further preferably, at least two layers of the liquid crystal polymer composite material have their continuous glass fiber filaments oriented in perpendicular directions.

[0018] Preferably, the melting temperature of the liquid crystal polymer is 280°C to 350°C.

[0019] Preferably, the liquid crystal polymer is a thermotropic liquid crystal polymer. More preferably, the liquid crystal polymer is Vectra A 950 from Celanese Corporation.

[0020] Preferably, the glass fibers in the continuous glass fiber filaments are S-1 type glass fibers.

[0021] Preferably, the linear density of the continuous glass fiber filaments is 1200-2400 tex.

[0022] Preferably, the breaking strength of the continuous glass fiber filaments is not less than 0.25 N / tex.

[0023] Preferably, the mass ratio of the polyphenylene ether resin to the polyaryletherketone resin is (1-1.5):1.

[0024] Preferably, the number average molecular weight of the polyphenylene ether resin is 25,000-35,000.

[0025] Preferably, the number average molecular weight of the polyaryletherketone resin is 25,000-35,000.

[0026] Preferably, the stainless steel fiber has a length of 3-6 mm and a diameter of 20-80 μm.

[0027] Preferably, the continuous glass fiber filaments modified by the coupling agent are modified by soaking the continuous glass fiber filaments in a coupling agent solution at 20-40° C. and pH 4-5 for 2-3 hours.

[0028] More preferably, the continuous glass fiber filaments are dried after the soaking treatment, the drying temperature is 110-120° C., and the drying time is 20-30 min.

[0029] Preferably, the stainless steel fiber modified by the coupling agent is modified by soaking the stainless steel fiber in a coupling agent solution at 20-40° C. and pH 4-5 for 2-3 hours.

[0030] More preferably, the stainless steel fiber is dried after the soaking treatment, the drying temperature is 110-120° C., and the drying time is 20-30 min.

[0031] More preferably, the mass fraction of the coupling agent in the coupling agent solution is 0.1-2.0%, such as 0.1-1.0%, 1.0-2.0%.

[0032] More preferably, the coupling agent is selected from one or more of dodecyltrimethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, mercaptopropyltrimethoxysilane and vinyltriethoxysilane.

[0033] More preferably, hydrochloric acid and / or acetic acid are used to adjust the pH of the coupling agent solution.

[0034] The liquid crystal polymer composite material includes one or more of the following features: a) Thickness is 3~3.5mm; b) Tensile strength is 100~150 MPa; c) Elongation at break is 2.0~3.0%; d) Flexural strength is 100~150 MPa; e) Flexural modulus is 6~8 GPa; f) Simply supported beam notched impact strength is 90~100KJ / m 2 ; g) compression strength is 100~140 MPa; h) surface resistance is 5×10 6 ~7.5×10 6 Ω; i) Volume resistivity 6.0×10 7 ~7.5×10 7 Ω·m; j) The flame retardant grade is UL94 V-0; k) After being immersed in 88℃, 50wt% sulfuric acid solution for 60 days, the corrosion resistance grade is A; after being immersed in 70℃, 50wt% sulfuric acid solution for 30 days, the corrosion resistance grade is A; l) After being immersed in 88℃, 37wt% sulfuric acid solution for 30 days, the corrosion resistance grade is A; after being immersed in 23℃, 10wt% sodium hydroxide solution for 30 days, the corrosion resistance grade is A.

[0035] The present invention also discloses a method for preparing the liquid crystal polymer composite material as described above, comprising the following steps:

[0036] The stainless steel fiber modified by the coupling agent, the polymer alloy and the liquid crystal polymer are mixed evenly, and then transported to a twin-screw extruder for extrusion and granulation. The granules are heated and melted, and then impregnated on the surface of a plurality of parallel continuous glass fiber filaments modified by the coupling agent. After impregnation and pressing, the unidirectional tape is cooled to obtain the unidirectional tape; the unidirectional tape is alternately stacked at 0° and 90°, and then hot-pressed. 0° is the moving direction of the unidirectional tape under the action of traction.

[0037] Preferably, the mixture is cooled to room temperature, which in this application is 20-25°C.

[0038] Preferably, the pressing pressure is 3-4 MPa / cm.

[0039] Preferably, the impregnation is performed by passing the continuous glass fiber filaments modified by the coupling agent through a flow channel of a melt impregnation tank for impregnation, and the flow channel width of the melt impregnation tank is 1-3 mm.

[0040] Preferably, the rotation speed of the twin-screw extruder is 80-120 r / min.

[0041] Preferably, the aspect ratio of the twin-screw extruder is 28-40.

[0042] Preferably, the temperature of zone 1 of the twin-screw extruder is 270-275°C, the temperature of zone 2 is 280-285°C, the temperature of zone 3 is 285-290°C, the temperature of zone 4 is 290-310°C, and the temperature of zone 5 is 310-330°C.

[0043] Preferably, the melt processing temperature is 20-50° C. higher than the melting temperature of the liquid crystal polymer.

[0044] Preferably, before cooling, an electric field adjustment process is performed, specifically: through a heating channel that applies an electric field, the direction of the electric field is perpendicular to the moving direction of the impregnated continuous glass fiber filaments.

[0045] More preferably, the temperature of the heating channel is 140-200°C.

[0046] More preferably, the electric field strength is 80-120 V / m, further preferably 100 V / m.

[0047] More preferably, the time for passing through the heating channel with the electric field applied is 1 to 3 minutes.

[0048] Preferably, the continuous glass fiber filaments are unwound, bundled, spread and preheated before impregnation.

[0049] More preferably, the unwinding is to place the fiber roll on an unwinding device to ensure that the continuous fiber filaments can be released smoothly and continuously.

[0050] More preferably, the bundling is a bundle formed by a plurality of fiber filaments being gathered together.

[0051] More preferably, the yarn spreading is to spread the bundled fiber bundle through a yarn spreading device to flatten the fiber bundle, reduce air and impurities between fibers, and facilitate subsequent impregnation.

[0052] More preferably, the preheating treatment is to heat the fiber bundle after the yarn is spread. More preferably, the preheating temperature is 180-200°C.

[0053] Preferably, the number of stacked layers is 5 to 15 layers, such as 5 to 10 layers, or 10 to 15 layers.

[0054] Preferably, the hot pressing pressure is 50-100 MPa and the temperature is 290-330°C.

[0055] The present invention also provides the use of the liquid crystal polymer composite material as a material for transporting pipelines for inflammable and explosive chemicals.

[0056] Preferably, the flammable and explosive chemicals include natural gas, hydrochloric acid, nitric acid, sulfuric acid and sodium hydroxide solution.

[0057] The invention discloses a liquid crystal polymer composite material and a preparation method and use thereof. Liquid crystal polymer, continuous glass fiber filaments, polymer alloy and stainless steel fiber are compounded to make the liquid crystal polymer composite material have good mechanical properties, corrosion resistance, antistatic and flame retardant properties, and improve the anisotropy caused by excessive differences in transverse and longitudinal properties during liquid crystal polymer processing, thereby reducing processing difficulty. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 Shown is a schematic diagram of the preparation process for unidirectional tape.

[0059] Figure 2 Schematic diagram showing unidirectional tape with 0º and 90º layup.

[0060] Figure 3 Schematic diagram of a unidirectional tape passing through an electric field under traction.

[0061] Description of reference numerals: Figure 1 In the figure, 1 represents a yarn frame, 2 represents a bundling device, 3 represents a yarn spreading device, 4 represents a melt impregnation tank, and 5 represents a cooling roller. DETAILED DESCRIPTION

[0062] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0063] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.

[0064] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.

[0065] The following examples of this application use the following raw materials:

[0066] The continuous glass fiber filament is a continuous glass fiber filament, the glass fiber is an S-1 type glass fiber, the linear density is 1200tex, and the breaking strength is not less than 0.25N / tex. The breaking strength is tested by GB / T7690.3-2013, and the linear density is tested by the single-filament linear density test in GB / T 14343-2008.

[0067] The polymer alloy is a composite system composed of polyphenylene ether resin and polyaryletherketone resin, wherein the mass ratio of the polyphenylene ether resin to the polyaryletherketone resin is 1.2:1, the number average molecular weights of the polyphenylene ether resin and the polyaryletherketone resin are 28000 and 28000 respectively, and the number average molecular weight is tested by GPC.

[0068] The coupling agent is dodecyltrimethoxysilane.

[0069] The grade of the liquid crystal polymer is Vectra A950 (manufacturer: Celanese Corporation), and the melting temperature is 280° C. The melting temperature is measured by DSC.

[0070] The stainless steel fibers were 5 mm in length and 30 µm in diameter.

[0071] The process for preparing unidirectional tape in the following examples and comparative examples of the present application is as follows: Figure 1 As shown, the fiber reel is placed on the yarn rack 1 and unwound under the traction of the drawing force, and then a plurality of fiber filaments are gathered together to form a bundle through the bundling device 2, and the bundled fiber bundle is unfolded through the yarn spreading device 3 to flatten the fiber bundle, and then the fiber bundle is impregnated and pressed through the melt impregnation tank 4, and after impregnation, it is cooled by the cooling roller 5 to obtain a unidirectional tape.

[0072] Example 1

[0073] This embodiment provides a specific liquid crystal polymer composite material, including the following raw material components in percentage by weight: Liquid crystal polymer 27% Continuous glass fiber filament treated with coupling agent 66.2% Polymer alloy 1.4% Stainless steel fiber treated with coupling agent: 5.4%.

[0074] The preparation method is as follows:

[0075] (1) Surface treatment of continuous glass fiber filaments: After washing and drying, the continuous glass fiber filaments were immersed in a 2.4 wt % dodecyltrimethoxysilane solution for 3 h, the pH was adjusted to 4, and dried at 120 ° C for 20 min;

[0076] Surface treatment of stainless steel fiber: After cleaning and drying, the stainless steel fiber was immersed in a 2.4 wt% dodecyltrimethoxysilane solution for 2 h, the pH was adjusted to 4, and dried at 110° C. for 30 min;

[0077] (2) unwinding, bundling, unwinding and preheating the surface treated continuous glass fiber filaments at a preheating temperature of 180°C;

[0078] (3) After the surface treated stainless steel fiber, polymer alloy and liquid crystal polymer are mixed evenly, they are transported to a twin-screw extruder for extrusion and granulation. The temperature of the first zone of the twin-screw extruder is 270°C, the temperature of the second zone is 280°C, the temperature of the third zone is 285°C, the temperature of the fourth zone is 300°C, and the temperature of the fifth zone is 320°C. The aspect ratio of the twin-screw extruder is 30, and the rotation speed is 100r / min. After the granules are heated and melted, they are passed into the flow channel of the melt impregnation tank 4. The flow channel width of the melt impregnation tank 4 is 1mm. The continuous glass fiber filaments are impregnated and pressed through the flow channel of the melt impregnation tank 4. The pressing pressure is 3MPa / cm;

[0079] (4) Under the action of the drawing force, the continuous glass fiber filament moves through the heating channel for 3 minutes. A flat plate capacitor is set on the heating channel. The direction of the electric field is perpendicular to the moving direction of the continuous glass fiber filament; the electric field strength is 100V / m;

[0080] (5) After cooling to room temperature, a unidirectional tape is obtained; the unidirectional tape is stacked 10 layers alternately at 0° and 90°, and then hot-pressed at 60 MPa and 300°C.

[0081] Embodiment 2-3

[0082] This embodiment provides a specific liquid crystal polymer composite material, the contents of its raw material components are shown in Table 1.

[0083] The preparation method is the same as that in Example 1.

[0084] Example 4

[0085] This embodiment provides a specific liquid crystal polymer composite material. The raw material composition of the liquid crystal polymer composite material is the same as that of Example 1, and the preparation method is different from that of Example 1. The only difference is that no electric field is applied to the heating channel. The rest of the preparation method is the same as that of Example 1.

[0086] Embodiment 5~7

[0087] This embodiment provides a specific liquid crystal polymer composite material, the raw material composition of the liquid crystal polymer composite material is basically the same as that of embodiment 1, the only difference is the selection of polymer alloy, specifically: the polymer alloy of embodiment 5 is polyphenylene ether resin; the polymer alloy of embodiment 6 is polyaryletherketone resin; the polymer alloy of embodiment 7 is a combination of polyphenylene ether resin and polyaryletherketone resin, and the mass ratio of polyphenylene ether resin to polyaryletherketone resin is 2.5:1. The content of the raw material components is shown in Table 1.

[0088] The preparation method is the same as that in Example 1.

[0089] Comparative Example 1

[0090] Comparative Example 1 is a comparative example of Example 1. The raw material component content of the liquid crystal polymer composite material is the same as that of Example 1. The only difference is that the stainless steel fiber and the continuous glass fiber filament are not treated with a coupling agent. Other preparation processes are the same as those of Example 1.

[0091] Comparative Examples 2 to 4

[0092] Comparative Examples 2 to 4 are comparative examples of Example 1, and the contents of the raw material components are shown in Table 1. The preparation method is the same as that of Example 1.

[0093] The thickness, density, tensile strength, elongation at break, flexural strength, flexural modulus, simply supported beam notched impact strength, compressive strength, surface resistance, volume resistivity, flame retardancy and corrosion resistance of the liquid crystal polymer composite materials prepared in test examples 1 to 7 and comparative examples 1 to 4 are shown in Tables 2 to 3, respectively. The test results are shown in Tables 2 to 3, and the test methods are shown as follows.

[0094] 1. Thickness: Use a micrometer to measure the thickness.

[0095] 2. Tensile strength: ISO 527-2, test speed 5mm / min;

[0096] 3. Elongation at break: ISO 527-2;

[0097] 4. Bending strength: ISO 178:2010, test speed is 2mm / min;

[0098] 5. Flexural modulus: using method A in ISO 178:2010, test speed is 2mm / min;

[0099] 6. Simply supported beam notched impact strength: using ISO 179-1:2010, the remaining width of the notch is 7.95mm;

[0100] 7. Compression strength: ASTM D3410-D3410M-16 (2016);

[0101] 8. Corrosion resistance test:

[0102] The samples were immersed in a 50wt% sulfuric acid solution at 88°C, and the change rates of tensile strength and weight dimensions of the samples were tested after immersion for 60 days.

[0103] The samples were immersed in 50wt% nitric acid at 70°C, and the change rates of tensile strength and weight dimensions of the samples were tested after immersion for 30 days.

[0104] The samples were immersed in 37wt% hydrochloric acid at 88°C, and the change rates of tensile strength and weight dimensions of the samples were tested after immersion for 30 days.

[0105] The samples were immersed in 10wt% sodium hydroxide solution at 23°C, and the change rates of tensile strength and weight dimensions of the samples were tested after immersion for 30 days.

[0106] If the reduction rate of tensile strength is not higher than 5%, and the weight and size change rate is not higher than 2%, it is grade A; if the reduction rate of tensile strength is higher than 5%, and the weight and size change rate is higher than 2%, it is grade B.

[0107] 9. UL94 flame retardant:

[0108] Sample preparation: Prepare samples with dimensions of 125 mm in length, 13.0 mm in width and 1.6 mm in thickness. If the test material has different thicknesses, samples of the minimum and maximum thicknesses need to be provided. If the test results of the two are inconsistent, samples of the intermediate thickness are also required.

[0109] Sample pretreatment: Before testing, the samples should be placed in an environment with a temperature of 23 ± 2℃ and a relative humidity of 50 ± 5% for at least 48 hours, then aged at 70 ± 1℃ for 168 hours, and then cooled at room temperature for at least 4 hours.

[0110] Test apparatus: Using a Bunsen burner as the ignition source, fix the sample vertically and place absorbent cotton under the sample to evaluate whether the molten material drips and ignites the cotton wool.

[0111] Vertical combustion test: Fix the sample vertically, place the Bunsen burner at the center point below the sample, and quickly remove the flame after it contacts the sample for 10 seconds. Record the spontaneous combustion time of the sample. After the spontaneous combustion stops, apply the flame again for 10 seconds and remove it. Record the second spontaneous combustion time and the red glow time after the flame is extinguished.

[0112] Test result recording: The test results need to record the burning duration of each sample, the total burning duration, the burning duration after the second flame application, and the glowing burning time.

[0113] Evaluation criteria: Evaluation is based on factors such as the burning time of the sample, whether there is molten material dripping, and whether the dripping material ignites the absorbent cotton underneath.

[0114] V-0 grade requirements: After the sample has been burned twice for 10 seconds, the flame must be extinguished within 30 seconds and no burning material can drip.

[0115] V-1: After the sample has been burned twice for 10 seconds, the flame shall be extinguished within 60 seconds, but no burning material shall drip and ignite the cotton wool below.

[0116] V-2: In the vertical burning test, after the sample has been burned twice for 10 seconds, the flame is extinguished within 60 seconds, and the burning material is allowed to drip, which can ignite the cotton wool 30 cm below.

[0117] 10. Surface resistance: The four-needle method is used for testing. Four conductive needles are inserted into the surface of the sample to be tested. The current is measured at a fixed voltage, and the surface resistance is calculated.

[0118] 11. Volume resistivity: tested by four-electrode method.

[0119] Table 1

[0120]

[0121] Table 2

[0122]

[0123] Table 3

[0124]

[0125] Since the continuous glass fiber filaments and the stainless steel fibers were not surface treated, the liquid crystal polymer composite material prepared in Comparative Example 1 had poor interface compatibility. After hot pressing, the product surface had defects and cracks visible to the naked eye.

[0126] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A liquid crystal polymer composite material, characterized in that: The raw material components include the following weight percentages: Liquid crystal polymer 20~30%; 50~75% of continuous glass fiber filaments modified by coupling agent; Polymer alloy 1~10%; Stainless steel fiber modified by coupling agent 3~15%; The polymer alloy is one or two selected from polyphenylene ether resin and polyaryletherketone resin.

2. The liquid crystal polymer composite material according to claim 1, characterized in that: The liquid crystal polymer composite material comprises the following raw material components in percentage by weight: Liquid crystal polymer 20~30%; Continuous glass fiber filaments modified with coupling agent 55~75%; Polymer alloy 1~4%; Stainless steel fiber modified by coupling agent 3~11%.

3. The liquid crystal polymer composite material according to claim 1, characterized in that: The melting temperature of the liquid crystal polymer is 280°C to 350°C; and / or, the liquid crystal polymer is a thermotropic liquid crystal polymer; and / or, the glass fibers in the continuous glass fiber filaments are S-1 type glass fibers; and / or, the linear density of the continuous glass fiber filament is 1200-2400tex; and / or the breaking strength of the continuous glass fiber filament is not less than 0.25 N / tex; And / or, the mass ratio of the polyphenylene ether resin to the polyaryletherketone resin is (1-1.5):1; And / or, the number average molecular weight of the polyphenylene ether resin is 25000-35000; And / or, the number average molecular weight of the polyaryletherketone resin is 25000-35000; and / or, the stainless steel fiber has a length of 3 to 6 mm and a diameter of 20 to 80 µm; And / or, the continuous glass fiber filaments modified by the coupling agent are modified by: immersing the continuous glass fiber filaments in a coupling agent solution at 20-40° C. and pH 4-5 for 2-3 hours; And / or, the stainless steel fiber modified by the coupling agent is modified by soaking the stainless steel fiber in a coupling agent solution at 20-40° C. and pH 4-5 for 2-3 hours.

4. The liquid crystal polymer composite material according to claim 3, characterized in that: The liquid crystal polymer is a Vectra A series liquid crystal polymer with a brand number of 950.

5. The liquid crystal polymer composite material according to claim 3, characterized in that: The mass fraction of the coupling agent in the coupling agent solution is 0.1-2.0%; And / or, the coupling agent is selected from one or more of dodecyltrimethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, mercaptopropyltrimethoxysilane and vinyltriethoxysilane.

6. The liquid crystal polymer composite material according to claim 1, characterized in that: Include one or more of the following characteristics: a) Thickness is 3~3.5mm; b) Tensile strength is 100~150 MPa; c) Elongation at break is 2.0~3.0%; d) Flexural strength is 100~150 MPa; e) Flexural modulus is 6~8 GPa; f) Simply supported beam notched impact strength is 90~100KJ / m 2 ; g) compression strength is 100~140 MPa; h) surface resistance is 5×10 6 ~7.5×10 6 Ω; i) Volume resistivity 6.0×10 7 ~7.5×10 7 Ω·m; j) The flame retardant grade is UL94 V-0; k) After being immersed in 88℃, 50wt% sulfuric acid solution for 60 days, the corrosion resistance grade is A; after being immersed in 70℃, 50wt% sulfuric acid solution for 30 days, the corrosion resistance grade is A; l) After being immersed in 88℃, 37wt% sulfuric acid solution for 30 days, the corrosion resistance grade is A; after being immersed in 23℃, 10wt% sodium hydroxide solution for 30 days, the corrosion resistance grade is A.

7. A method for preparing a liquid crystal polymer composite material according to any one of claims 1 to 6, characterized in that: The steps include: The stainless steel fiber modified by the coupling agent, the polymer alloy and the liquid crystal polymer are uniformly mixed and transported to a twin-screw extruder for extrusion and granulation. The granules are heated and melted, and impregnated on the surface of a plurality of parallel continuous glass fiber filaments modified by the coupling agent. After impregnation and pressing, the unidirectional tape is obtained by cooling. The unidirectional tape is alternately stacked at 0° and 90° and then hot-pressed.

8. The preparation method according to claim 7, characterized in that: The temperature of the first zone of the twin-screw extruder is 270-275°C, the temperature of the second zone is 280-285°C, the temperature of the third zone is 285-290°C, the temperature of the fourth zone is 290-310°C, and the temperature of the fifth zone is 310-330°C; And / or, the rotation speed of the twin-screw extruder is 80-120 r / min; And / or, the aspect ratio of the twin-screw extruder is 28 to 40; and / or, before cooling, undergoing an electric field adjustment step, specifically: applying an electric field through a heating channel, wherein the direction of the electric field is perpendicular to the moving direction of the impregnated continuous glass fiber filaments; and / or, the melt processing temperature is 20-50° C. higher than the melting temperature of the liquid crystal polymer; and / or, the pressing pressure is 3-4 MPa / cm; And / or, the impregnation is that the continuous glass fiber filaments after the coupling agent modification are passed through the flow channel of the melt impregnation tank (4) for impregnation, and the flow channel width of the melt impregnation tank (4) is 1-3 mm; And / or, the continuous glass fiber filaments are unwound, bundled, spread and preheated before impregnation; and / or, cooling to room temperature; and / or, the number of stacked layers is 5 to 15; and / or, the hot pressing pressure is 50-100 MPa; And / or, the temperature of hot pressing is 290-330°C.

9. The preparation method according to claim 8, characterized in that: The electric field strength is 80-120 V / m; and / or the preheating temperature is 180-200° C.; and / or the time of passing through the electric field is 1-3 min.

10. Use of the liquid crystal polymer composite material according to any one of claims 1 to 6 as a pipeline material for transporting flammable and explosive chemicals.

Citation Information

Patent Citations

  • Fibers sized with polyetherketoneketones

    CN102307920A

  • High heat-proof fiber-reinforced PBT plastic for automotive interior parts and preparation method thereof

    CN103834148A

  • Glass fiber reinforced PPS / PEEK (Polyphenylene Sulfide / Polyether-Ether-Ketone) alloy and preparation process thereof

    CN107778769A

  • Low-dielectric liquid crystal polyester composition and preparation method thereof

    CN111004519A

  • Continuous fiber reinforced crystalline polyaryletherketone resin-based one-way belt prepreg as well as preparation method and application of continuous fiber reinforced crystalline polyaryletherketone resin-based one-way belt prepreg

    CN112812351A

Cited By

  • Corrosion-resistant thin film, pipe and preparation method and application of corrosion-resistant thin film and pipe

    CN120464153A