Metal anticorrosive paint, preparation method thereof and metal anticorrosive coating
By copolymerizing reaction of components such as carboxyl monomers to form a high-adhesion coating, the problems of poor adhesion and weatherability of anti-corrosion coatings in steel structures are solved, and a safer and more environmentally friendly anti-corrosion effect of steel structures is achieved.
Patent Information
- Application Number
- CN202411015210.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The existing steel structures have insufficient adhesion and poor weather resistance, which leads to rust and breaking of steel structures under the erosion of air and water, and traditional organic solvents cause environmental pollution and health risks.
Metal anticorrosion coatings using carboxy monomers, epoxy group monomers, phosphate monomers, furfural methacrylate, soft monomers, hard monomers and ethyl orthosilicate, and form high bonding through copolymerization reaction The coating with abrasion resistance and aging resistance is used to improve the weather resistance of the coating by using the core-shell structure of silica particles.
It significantly improves the adhesion and weather resistance of metal anticorrosion coatings, reduces environmental pollution, provides safer construction conditions, and extends the service life of the coating.
Smart Images

Figure BDA0004965497880000061 
Figure BDA0004965497880000071 
Figure BDA0004965497880000072
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and in particular relates to a metal anticorrosion coating and a preparation method thereof, and a metal anticorrosion coating. Background Art
[0002] Anti-corrosion of steel structures is a global problem. Every year, hundreds of millions of tons of steel structure supports, water pipes, and ship hulls rust, break, and crack under the erosion of air and water, polluting the environment and posing safety hazards.
[0003] Traditional anti-corrosion paints use organic cracked petroleum as solvent. During production and construction, large amounts of it evaporate into the air, causing environmental pollution, fire hazards, and easily causing harm to the health of construction and user personnel.
[0004] With the improvement of social environmental protection requirements and the strengthening of supervision, the development of green, environmentally friendly, low-VOC water-based industrial paints has become an inevitable result of social choice. Water-based emulsions that are non-toxic, non-flammable, non-explosive, and safe to store and transport as the main material of water-based industrial paints have also attracted widespread attention.
[0005] The current water-based industrial paint emulsions are mainly traditional polyacrylic resins, which rely on a large amount of emulsifiers and carboxyl groups to disperse in water. They have poor water resistance and adhesion. They will be destroyed by air, water, and salt spray in the environment within two to three years and lose their protective function. Summary of the invention
[0006] In view of the problems of insufficient adhesion and poor weather resistance of existing anti-corrosion water-based coatings for steel structures, the present invention provides a metal anti-corrosion coating and a preparation method thereof, and a metal anti-corrosion coating.
[0007] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0008] In one aspect, the present invention provides a metal anticorrosion coating, the raw materials of which include the following components:
[0009] Solvents, emulsifiers, carboxyl monomers, epoxy monomers, phosphate monomers, furfural methacrylate, soft monomers, hard monomers, versatate and tetraethyl orthosilicate.
[0010] Optionally, the raw materials include the following weight components:
[0011] 420-530 parts of solvent, 10-30 parts of emulsifier, 5-20 parts of carboxyl monomer, 5-20 parts of epoxy group monomer, 5-35 parts of phosphate monomer, 3-8 parts of furfural methacrylate, 100-200 parts of soft monomer, 200-300 parts of hard monomer, 50-150 parts of versatate and 5-15 parts of tetraethyl orthosilicate.
[0012] Optionally, the emulsifier includes one or more of a nonionic emulsifier and an anionic emulsifier.
[0013] Optionally, the carboxyl monomer includes one or more of acrylic acid, methacrylic acid and itaconic acid, and / or
[0014] The epoxy group monomers include one or more of allyl glycidyl ether, glycidyl methacrylate, and / or
[0015] The phosphate monomer includes one or more of 2-hydroxyethyl methacrylate phosphate, acrylic acid phosphate, methacrylate phosphate and hydroxyethyl acrylic acid phosphate, and / or
[0016] The soft monomer includes one or more of ethyl acrylate, butyl acrylate and isooctyl acrylate, and the hard monomer includes one or more of methyl methacrylate, acrylonitrile, styrene, acrylamide, tert-butyl acrylate and tert-butyl methacrylate.
[0017] Optionally, the solvent is water.
[0018] Optionally, the raw materials of the metal anti-corrosion coating further include 1 to 6 parts by weight of a pH buffer, and the pH buffer includes one or more of sodium bicarbonate and ammonium bicarbonate.
[0019] Optionally, the raw materials of the metal anti-corrosion coating further include 0.5 to 15 parts by weight of an organic ammonia pH regulator, and the organic ammonia pH regulator includes one or more of triethylamine, N,N-dimethylethanolamine and AMP-95.
[0020] Optionally, the raw materials of the metal anti-corrosion coating further include 0.5 to 3.5 parts by weight of an initiator, and the initiator includes one or more of ammonium persulfate, sodium persulfate and potassium persulfate.
[0021] In another aspect, the present invention provides a metal anti-corrosion coating obtained by curing the metal anti-corrosion coating as described above.
[0022] In another aspect, the present invention provides a method for preparing the metal anticorrosive coating as described above, wherein an emulsifier is added to a solvent, and carboxyl monomer, epoxy monomer, phosphate monomer, furfural methacrylate, soft monomer, hard monomer and tert-butyl vinyl carbonate are added with stirring to obtain a pre-emulsion;
[0023] Adding a solvent, a pH buffer and an emulsifier into a reactor, raising the temperature to 80° C. to 85° C., adding an initiator, adding ethyl orthosilicate and a portion of the pre-emulsified liquid, and reacting to obtain a seed emulsion;
[0024] The remaining pre-emulsion was added dropwise to the reactor, and the initiator solution was added dropwise at the same time, and the temperature was maintained at 82°C to 88°C;
[0025] After the reaction is completed, an organic ammonia pH regulator is added to obtain a metal anti-corrosion coating.
[0026] According to the metal anticorrosion coating provided by the present invention, its preparation raw materials adopt carboxyl monomer, epoxy monomer, phosphate monomer, furfural methacrylate, soft monomer, hard monomer, tert-butyl vinyl carbonate and tetraethyl orthosilicate, wherein the polar group provided by the carboxyl monomer is conducive to improving the adhesion of the metal anticorrosion coating, and the epoxy group and phosphate group provided by the epoxy monomer and phosphate monomer are conducive to improving the bonding strength between the coating and the metal interface; more importantly, in order to meet the requirements of wear resistance and aging resistance of metal anticorrosion, furfural methacrylate and tetraethyl orthosilicate are added to the metal anticorrosion coating, furfural methacrylate participates in the monomer copolymerization reaction, and the formed copolymer chain contains furfural ester groups. These groups can form additional crosslinking points between molecules, thereby improving the rigidity and hardness of the polymer. In addition, due to the special structure of the furfural ester group, it can also give the material a certain chemical resistance and heat resistance, thereby improving the overall weather resistance of the coating; tetraethyl orthosilicate is used for hydrolysis and condensation to form silica particles. Since the silica particles are formed in situ by tetraethyl orthosilicate in the emulsion, they have good dispersibility, and the formed silica particles serve as seeds for the polymerization of other monomers, so that the acrylic copolymer obtained by the polymerization is coated on the surface of the silica particles to form a core-shell structure, which ultimately effectively improves the heat resistance and weather resistance of the coating. DETAILED DESCRIPTION
[0027] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0028] In the description of the present invention, the term "monomer" refers to the raw material participating in the polymerization process of the coating. Specifically, "carboxyl monomer, epoxy monomer, phosphate monomer, furfural methacrylate, soft monomer, hard monomer, versatate vinyl ester" in the present invention can all be classified as "monomers".
[0029] An embodiment of the present invention provides a metal anti-corrosion coating, the raw materials of which include the following components:
[0030] Solvents, emulsifiers, carboxyl monomers, epoxy monomers, phosphate monomers, furfural methacrylate, soft monomers, hard monomers, versatate and tetraethyl orthosilicate.
[0031] Among them, the homopolymer glass transition temperature of the soft monomer is relatively low, which gives the adhesive a certain flexibility and extensibility, while the homopolymer glass transition temperature of the hard monomer is relatively high, which can improve the hardness and tensile strength of the adhesive.
[0032] The polar groups provided by the carboxyl monomers are conducive to improving the adhesion of the metal anticorrosion coating. The epoxy groups provided by the epoxy monomers can open the ring and cross-link during the reaction process, thereby improving the hardness of the coating and connecting with the hydroxyl groups on the metal surface. The phosphate groups provided by the phosphate monomers can form stable chemical bonds with the metal surface, thereby improving the adhesion strength of the coating and the metal interface.
[0033] More importantly, in order to meet the requirements of wear resistance and aging resistance of metal corrosion protection, furfural methacrylate and ethyl orthosilicate are added to the metal corrosion protection coating.
[0034] Furfural methacrylate participates in the monomer copolymerization reaction, and the copolymer chain formed contains furfural ester groups. These groups can form additional cross-linking points between molecules, thereby improving the rigidity and hardness of the polymer. In addition, due to the special structure of the furfural ester group, it can also give the material a certain chemical resistance and heat resistance, thereby improving the weather resistance of the coating as a whole.
[0035] Tetraethyl orthosilicate is used for hydrolysis and condensation to form silica particles. Since the silica particles are formed in situ from tetraethyl orthosilicate in the emulsion, they have good dispersibility, and the formed silica particles serve as seeds for the polymerization of other monomers, so that the acrylic copolymer obtained by polymerization is coated on the surface of the silica particles to form a core-shell structure, which ultimately effectively improves the heat resistance and weather resistance of the coating.
[0036] In some embodiments, the raw materials include the following components by weight:
[0037] 420-530 parts of solvent, 10-30 parts of emulsifier, 5-20 parts of carboxyl monomer, 5-20 parts of epoxy group monomer, 5-35 parts of phosphate monomer, 3-8 parts of furfural methacrylate, 100-200 parts of soft monomer, 200-300 parts of hard monomer, 50-150 parts of versatate and 5-15 parts of tetraethyl orthosilicate.
[0038] In a specific embodiment, the weight parts of the solvent can be 420 parts, 430 parts, 440 parts, 450 parts, 460 parts, 470 parts, 480 parts, 490 parts, 500 parts, 510 parts, 520 parts or 530 parts; the weight parts of the emulsifier can be 10 parts, 12 parts, 15 parts, 17 parts, 18 parts, 20 parts, 22 parts, 25 parts, 27 parts, 28 parts or 30 parts; the weight parts of the carboxyl monomer can be 5 parts, 7 parts, 8 parts, 10 parts, 12 parts, 15 parts, 17 parts, 18 parts or 20 parts; the weight parts of the epoxy group monomer can be 5 parts, 7 parts, 8 parts, 10 parts, 12 parts, 15 parts, 17 parts, 18 parts or 20 parts; the weight parts of the phosphate monomer can be 5 parts, 7 parts, 8 parts, 10 parts, 12 parts, The weight proportion of the furfural methacrylate can be 3 parts, 4 parts, 5 parts, 6 parts, 7 parts or 8 parts; the weight proportion of the soft monomer can be 100 parts, 120 parts, 130 parts, 140 parts, 150 parts, 160 parts, 180 parts or 200 parts; the weight proportion of the hard monomer can be 200 parts, 220 parts, 230 parts, 240 parts, 250 parts, 260 parts, 280 parts or 300 parts; the weight proportion of the versatate can be 50 parts, 60 parts, 80 parts, 100 parts, 120 parts, 130 parts, 140 parts or 150 parts; the weight proportion of the tetraethyl orthosilicate can be 5 parts, 7 parts, 8 parts, 10 parts, 12 parts or 15 parts.
[0039] In some embodiments, the emulsifier includes one or more of a nonionic emulsifier and an anionic emulsifier.
[0040] The anionic emulsifier includes one or more of sodium methyl allyl sulfonate, sodium dodecyl sulfate, sodium dodecyl sulfonate and sodium dodecylbenzene sulfonate; the nonionic emulsifier includes one or more of allyl polyoxyethylene ether, fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether.
[0041] The emulsifier is used to disperse the monomer and ethyl orthosilicate, and prevent the acrylic ester particles after polymerization from agglomerating with each other, so that the metal anticorrosive coating obtained after polymerization is in an emulsion state, which is convenient for construction operation.
[0042] In some embodiments, the carboxyl monomer includes one or more of acrylic acid, methacrylic acid, and itaconic acid.
[0043] In some embodiments, the epoxy group monomer includes one or more of allyl glycidyl ether and glycidyl methacrylate.
[0044] In some embodiments, the phosphate monomer includes one or more of 2-hydroxyethyl methacrylate phosphate, acrylic acid phosphate, methacrylate phosphate, and hydroxyethyl acrylic acid phosphate.
[0045] In some embodiments, the soft monomer includes one or more of ethyl acrylate, butyl acrylate, and isooctyl acrylate, and the hard monomer includes one or more of methyl methacrylate, acrylonitrile, styrene, acrylamide, t-butyl acrylate, and t-butyl methacrylate.
[0046] In some embodiments, the solvent is water.
[0047] Compared with organic solvents, using water as an organic solvent has the characteristics of being environmentally friendly and having low toxicity.
[0048] In some embodiments, the raw materials of the metal anti-corrosion coating further include 1 to 6 parts by weight of a pH buffer, and the pH buffer includes one or more of sodium bicarbonate and ammonium bicarbonate.
[0049] The pH buffer is used to maintain the stability of the pH value of the system during the polymerization process, ensure the polymerization speed of the monomer, and obtain a uniform and controllable polymer.
[0050] In some embodiments, the raw materials of the metal anti-corrosion coating further include 0.5 to 15 parts by weight of an organic ammonia pH regulator, and the organic ammonia pH regulator includes one or more of triethylamine, N,N-dimethylethanolamine and AMP-95.
[0051] Since the carboxyl monomer contained in the monomer has a certain acidity, the metal anti-corrosion coating obtained after the polymerization reaction also has a certain acidity, so when used in the field of metal coatings, it is easy to corrode the metal. The addition of organic ammonia pH adjuster to the metal anti-corrosion coating can be used to adjust the pH value to 7.5-8.5, thereby avoiding corrosion to metal materials.
[0052] In some embodiments, the raw materials of the metal anti-corrosion coating further include 0.5 to 3.5 parts by weight of an initiator, and the initiator includes one or more of ammonium persulfate, sodium persulfate, and potassium persulfate.
[0053] The initiator is used to initiate the polymerization reaction of the monomers.
[0054] In some embodiments, the metal anti-corrosion coating has a core-shell structure, the core of the core-shell structure is silica particles obtained by hydrolysis and condensation of the tetraethyl orthosilicate, and the shell of the core-shell structure is a polyacrylate copolymer layer obtained by polymerization of the carboxyl monomer, the epoxy group monomer, the phosphate monomer, the methacrylate furfural ester, the soft monomer and the hard monomer; because the silica particles serve as the core to form a good support for the polyacrylate copolymer layer, the weather resistance and salt spray resistance of the coating formed by the metal anti-corrosion coating can be effectively improved.
[0055] Another embodiment of the present invention provides a metal anti-corrosion coating, which is obtained by curing the metal anti-corrosion coating as described above.
[0056] Another embodiment of the present invention provides a method for preparing the metal anticorrosive coating as described above, wherein an emulsifier is added to a solvent, and carboxyl monomer, epoxy monomer, phosphate monomer, furfural methacrylate, soft monomer, hard monomer and tert-butyl vinyl carbonate are added with stirring to obtain a pre-emulsion;
[0057] Adding a solvent, a pH buffer and an emulsifier into a reactor, raising the temperature to 80° C. to 85° C., adding an initiator, adding ethyl orthosilicate and a portion of the pre-emulsified liquid, and reacting to obtain a seed emulsion;
[0058] The remaining pre-emulsion was added dropwise to the reactor, and the initiator solution was added dropwise at the same time, and the temperature was maintained at 82°C to 88°C;
[0059] After the reaction is completed, an organic ammonia pH regulator is added to obtain a metal anti-corrosion coating.
[0060] In the preparation method provided by the present invention, tetraethyl orthosilicate and part of the pre-emulsion are first placed in a solvent at 80°C to 85°C. Under this condition, tetraethyl orthosilicate undergoes a hydrolysis and condensation reaction to form silica particles. At the same time, carboxyl monomers, epoxy group monomers, phosphate monomers, furfural methacrylate, soft monomers and hard monomers in the pre-emulsion are preliminarily polymerized and in-situ polymerized on the surface of the silica particles to form coated particles as a seed emulsion. The remaining pre-emulsion and an initiator are then added dropwise to further grow the coated particles with silica as the core, and finally a metal anticorrosive coating with a core-shell structure is obtained.
[0061] In some embodiments, after adding ethyl orthosilicate and a portion of the pre-emulsion, the temperature is maintained at 80° C. to 85° C. for 15 to 30 minutes.
[0062] In some embodiments, the remaining pre-emulsion is added dropwise to the reactor for 180 to 240 minutes, the initiator solution is added dropwise for 210 to 270 minutes, and the mixture is kept at 82 to 88° C. for 1 to 3 hours.
[0063] In some embodiments, after adding the organic ammonia pH regulator, the pH value of the system is controlled at 7.5 to 8.5. The present invention is further described below through examples.
[0064] Example 1
[0065] This example is used to illustrate the metal anticorrosion coating disclosed in the present invention, and its raw materials include the following components in parts by weight:
[0066]
[0067]
[0068] The preparation method of the metal anticorrosion coating comprises the following steps:
[0069] 1: Add 40% deionized water and 80% emulsifier into the pre-emulsification kettle, add all monomers while stirring, stir for 20 minutes to obtain a pre-emulsion.
[0070] All the ammonium persulfate was dissolved in 3% deionized water to obtain an initiator solution.
[0071] All N,N-dimethylethanolamine was diluted with 2% deionized water to obtain an N,N-dimethylethanolamine solution.
[0072] 2: Add 35% deionized water, all the sodium bicarbonate, and 20% emulsifier to the reactor, raise the temperature to 82°C, add 20% initiator solution after the temperature stabilizes, add all the ethyl orthosilicate and 5% pre-emulsion, react for 20 minutes, and obtain the seed emulsion.
[0073] 3: Add the remaining pre-emulsion evenly into the reactor within 200 minutes, and at the same time, add the initiator solution evenly within 230 minutes. After the pre-emulsion is added, keep warm at 85°C for 2 hours.
[0074] 4: Lower the reaction system to below 55°C, add N,M-dimethylethanolamine solution, stir for 20 minutes, control the pH to 7.5-8.5, and filter to obtain the metal anti-corrosion coating.
[0075] Example 2
[0076] This example is used to illustrate the metal anticorrosion coating disclosed in the present invention, and its raw materials include the following components in parts by weight:
[0077]
[0078]
[0079] The preparation method of the metal anticorrosion coating comprises the following steps:
[0080] 1: Add 35% deionized water and 75% emulsifier into the pre-emulsification kettle, add all monomers while stirring, stir for 20 minutes to obtain a pre-emulsion.
[0081] All potassium persulfate was dissolved in 5% deionized water to obtain an initiator solution.
[0082] All triethylamine was diluted with 3% deionized water to obtain a triethylamine solution.
[0083] 2: Add 57% deionized water, all the ammonium bicarbonate, and 25% emulsifier to the reactor, heat it to 84°C, add 15% initiator after the temperature is constant, add all the ethyl orthosilicate and 3% pre-emulsion, and react for 20 minutes to obtain the seed emulsion.
[0084] 3: Evenly add the remaining pre-emulsion to the reactor, and at the same time, add the initiator solution. The total addition time of the pre-emulsion is controlled to be 220 minutes, and the addition time of the initiator solution is 250 minutes. After the pre-emulsion is added, keep it warm at 86°C for 2 hours.
[0085] 4: Lower the reaction system to below 55°C, add triethylamine solution, stir for 20 minutes, control the pH to 7.5-8.5, and filter to obtain the metal anti-corrosion coating.
[0086] Example 3
[0087] This example is used to illustrate the metal anticorrosion coating disclosed in the present invention, and its raw materials include the following components in parts by weight:
[0088]
[0089]
[0090] The preparation method of the metal anticorrosion coating comprises the following steps:
[0091] 1: Add 45% deionized water and 70% emulsifier into the pre-emulsification kettle, add all monomers while stirring, stir for 20 minutes to obtain a pre-emulsified liquid.
[0092] All of the sodium persulfate was dissolved in 2% deionized water to obtain an initiator solution.
[0093] All AMP-95 was diluted with 3% deionized water to obtain AMP-95 solution.
[0094] 2: Add 50% deionized water, all the sodium bicarbonate, and 30% emulsifier to the reactor, raise the temperature to 83°C, add 30% initiator solution after the temperature stabilizes, add all the ethyl orthosilicate and 7% pre-emulsion, and react for 20 minutes to obtain the seed emulsion.
[0095] 3: Add the remaining pre-emulsion evenly into the reactor within 230 minutes, and at the same time, add the initiator solution evenly within 260 minutes. After the pre-emulsion is added, keep warm at 86°C for 2 hours.
[0096] 4: Cool the reaction system to below 55°C, add AMP-95 solution, stir for 20 minutes, control the pH at 7.5-8.5, and filter to obtain an industrial paint emulsion with excellent adhesion.
[0097] Example 4
[0098] This example is used to illustrate the metal anticorrosion coating disclosed in the present invention. Its raw material composition is the same as that of Example 1, except that:
[0099] The preparation method of the metal anticorrosion coating comprises the following steps:
[0100] 1: Add 40% deionized water and 80% emulsifier into the pre-emulsification kettle, add all monomers while stirring, stir for 20 minutes to obtain a pre-emulsion.
[0101] All the ammonium persulfate was dissolved in 3% deionized water to obtain an initiator solution.
[0102] All N,N-dimethylethanolamine was diluted with 2% deionized water to obtain an N,N-dimethylethanolamine solution.
[0103] 2: Add 35% deionized water, all sodium bicarbonate, and 20% emulsifier to the reactor, heat to 82°C, add 20% initiator solution after the temperature stabilizes, and add 5% pre-emulsion, react for 20 minutes to obtain seed emulsion.
[0104] 3: Add the remaining pre-emulsion evenly into the reactor within 200 minutes, and at the same time, evenly add the initiator solution evenly within 230 minutes. After the pre-emulsion is added, add all the ethyl orthosilicate and keep warm at 85°C for 2 hours.
[0105] 4: Lower the reaction system to below 55°C, add N,M-dimethylethanolamine solution, stir for 20 minutes, control the pH to 7.5-8.5, and filter to obtain the metal anti-corrosion coating.
[0106] Comparative Example 1
[0107] This comparative example is used to compare and illustrate the metal anticorrosion coating disclosed in the present invention. Its raw materials include most of the components and operating steps in Example 1, and the difference is that:
[0108] Excludes furfural methacrylate.
[0109] Comparative Example 2
[0110] This comparative example is used to compare and illustrate the metal anticorrosion coating disclosed in the present invention. Its raw materials include most of the components and operating steps in Example 1, and the difference is that:
[0111] Does not include tetraethyl orthosilicate.
[0112] Comparative Example 3
[0113] This comparative example is used to compare and illustrate the metal anticorrosion coating disclosed in the present invention. Its raw materials include most of the components and operating steps in Example 1, and the difference is that:
[0114] Does not include versatate VV-10.
[0115] Comparative Example 4
[0116] This comparative example is used to compare and illustrate the metal anticorrosion coating disclosed in the present invention. Its raw materials include most of the components and operating steps in Example 1, and the difference is that:
[0117] Excluding phosphate ester PM-1500
[0118] Performance Testing
[0119] The metal anti-corrosion coating prepared above was subjected to the following performance tests:
[0120] 1. Adhesion test
[0121] The metal anti-corrosion coating is applied to the tinplate and cured to obtain the tinplate coated with the metal anti-corrosion coating. A grid cutter is used to cut in two mutually perpendicular directions in the test area to form a grid. When cutting, the blade penetrates the coating until it contacts the substrate to ensure the effectiveness of the test. The test tape is used to cover the cut grid, ensuring that the tape is completely adhered to the coating. The tape is quickly torn off in the vertical direction (90° angle), and the peeling of the coating is checked. The degree of peeling of the coating is observed and recorded. The rating is from 0 to 5, 0 represents the best adhesion, 5 represents the worst adhesion,
[0122] 2. Salt spray resistance test
[0123] The metal anti-corrosion coating is applied to the tinplate and cured to obtain the tinplate coated with the metal anti-corrosion coating, and the tinplate is placed in a salt spray test chamber, and a 5% salt water solution is prepared using pure water and analytically pure sodium chloride (NaCl). The pH value of the solution is adjusted to between 6.5 and 7.2, and a neutral salt spray test (NSS) is performed to analyze the corrosion phenomenon and determine the corrosion resistance time of the coating.
[0124] The test results obtained are entered in Table 1.
[0125] Table 1
[0126] sample Adhesion test Salt spray resistance test Example 1 Level 0 758h Example 2 Level 0 694h Example 3 Level 0 907h Example 4 Level 1 416h Comparative Example 1 Level 2 124h Comparative Example 2 Level 3 98h Comparative Example 3 Level 2 176h Comparative Example 4 Level 3 73h
[0127] It can be seen from the test results of Table 1 that the metal anti-corrosion coating prepared by the metal anti-corrosion coating provided by the present invention has a high adhesion to the metal material, and can better prevent the coating from falling off from the metal surface under impact or use. On the other hand, the metal anti-corrosion coating provided by the present invention has good salt spray resistance, indicating that it has good weather resistance and can be suitable for use in outdoor environments. Specifically, it can be seen from the test results of Examples 1 to 3 and Example 4 that in the coating preparation process, the order of adding tetraethyl orthosilicate has a greater influence on the weather resistance of the coating.
[0128] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A metal anticorrosion coating, characterized in that: Its raw materials Includes the following components: Solvents, emulsifiers, carboxyl monomers, epoxy monomers, phosphate monomers, furfural methacrylate, soft monomers, hard monomers, versatate and tetraethyl orthosilicate.
2. The metal anticorrosion coating according to claim 1, characterized in that: Its raw materials include the following weight components: 420-530 parts of solvent, 10-30 parts of emulsifier, 5-20 parts of carboxyl monomer, 5-20 parts of epoxy group monomer, 5-35 parts of phosphate monomer, 3-8 parts of furfural methacrylate, 100-200 parts of soft monomer, 200-300 parts of hard monomer, 50-150 parts of versatate and 5-15 parts of tetraethyl orthosilicate.
3. The metal anticorrosion coating according to claim 1, characterized in that: The emulsifier includes one or more of a nonionic emulsifier and an anionic emulsifier.
4. The metal anticorrosion coating according to claim 1, characterized in that: The carboxyl monomer includes one or more of acrylic acid, methacrylic acid and itaconic acid, and / or The epoxy group monomers include one or more of allyl glycidyl ether, glycidyl methacrylate, and / or The phosphate monomer includes one or more of 2-hydroxyethyl methacrylate phosphate, acrylic acid phosphate, methacrylate phosphate and hydroxyethyl acrylic acid phosphate, and / or The soft monomer includes one or more of ethyl acrylate, butyl acrylate and isooctyl acrylate, and the hard monomer includes one or more of methyl methacrylate, acrylonitrile, styrene, acrylamide, tert-butyl acrylate and tert-butyl methacrylate.
5. The metal anticorrosion coating according to claim 1, characterized in that: The solvent is water.
6. The metal anticorrosion coating according to claim 2, characterized in that: The raw materials of the metal anticorrosion coating also include 1 to 6 parts by weight of a pH buffer, and the pH buffer includes one or more of sodium bicarbonate and ammonium bicarbonate.
7. The metal anticorrosion coating according to claim 2, characterized in that: The raw materials of the metal anticorrosion coating also include 0.5 to 15 parts by weight of an organic ammonia pH regulator, and the organic ammonia pH regulator includes one or more of triethylamine, N,N-dimethylethanolamine and AMP-95.
8. The metal anticorrosion coating according to claim 2, characterized in that: The raw materials of the metal anti-corrosion coating also include 0.5 to 3.5 parts by weight of an initiator, and the initiator includes one or more of ammonium persulfate, sodium persulfate and potassium persulfate.
9. A metal anticorrosion coating, characterized in that: The metal anticorrosion coating is obtained by curing the metal anticorrosion coating according to any one of claims 1 to 8.
10. The method for preparing a metal anticorrosion coating according to any one of claims 1 to 8, characterized in that: The following operations are included: Adding an emulsifier to the solvent, stirring and adding a carboxyl monomer, an epoxy monomer, a phosphate monomer, furfural methacrylate, a soft monomer, a hard monomer and tert-butyl vinyl carbonate to obtain a pre-emulsified liquid; Adding a solvent, a pH buffer and an emulsifier into a reactor, raising the temperature to 80° C. to 85° C., adding an initiator, adding ethyl orthosilicate and a portion of the pre-emulsified liquid, and reacting to obtain a seed emulsion; The remaining pre-emulsion was added dropwise to the reactor, and the initiator solution was added dropwise at the same time, and the temperature was maintained at 82°C to 88°C; After the reaction is completed, an organic ammonia pH regulator is added to obtain a metal anti-corrosion coating.
Citation Information
Patent Citations
Method for preparing nano silicon / polyacrylate composite emulsion
CN102030873A
Preparation method for anti-rust soap-free acrylate emulsion
CN102115517A
Cited By
Method for fluorinating inside equipment to form film
CN119663164A
Water-based steel structure fireproof coating and preparation method thereof
CN120865760A
Aqueous fireproofing coating for steel structure and preparation method thereof
CN120865760B