Anti-corrosion conductive coating for high-speed rail electric contact network parts and preparation method of anti-corrosion conductive coating

By combining graphene oxide with multi-wall carbon nanotubes and combined with epoxy resin and aqueous polyurethane, anti-corrosion conductive coatings for high-speed rail power contact network components are prepared, solving the problems of unstable conductivity and environmental pollution. The coating is achieved with high conductivity, weather resistance and long life.

CN118931364APending Publication Date: 2024-11-12SHENZHEN JIADA ENERGY SAVING & ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411239676.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing anti-corrosion coatings for high-speed rail power contact network components have problems such as unstable conductivity, environmental pollution and high production costs, and traditional coatings have shortcomings in corrosion resistance and weather resistance.

Method used

Graphene oxide is used to combine with multi-wall carbon nanotubes, and to form a composite through the connection of para-phenylenediamine, and combine it with epoxy resin and aqueous polyurethane. Add nano-silicon dioxide and other materials to prepare a high-speed iron power contact network zero The anti-corrosion conductive coating of the component improves the conductivity and stability through the reduction of hydrazine hydrate and the action of initiator.

Benefits of technology

The conductive performance of high-speed rail power contact network components has been improved, and the flexibility, adhesion and impact resistance of the coating have been significantly improved. At the same time, it has good water, acid, alkali and salt spray resistance, which has extended its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005028854880000141
    Figure BDA0005028854880000141
  • Figure BDA0005028854880000151
    Figure BDA0005028854880000151
Patent Text Reader

Abstract

The invention provides an anti-corrosion conductive coating for parts of a high-speed rail electric contact network and a preparation method of the anti-corrosion conductive coating, and belongs to the technical field of coatings. The preparation method comprises the following steps: reacting graphene oxide with p-phenylenediamine to form a compound, then reacting with acid-treated multi-walled carbon nanotubes, reducing, polymerizing, adding into epoxy resin together with nano silicon dioxide to prepare modified epoxy resin, and uniformly mixing with water-based polyurethane modified by resveratrol to prepare the water-based polyurethane coating. Adding a pH value regulator, a dispersing agent, a defoaming agent, water, pigment, talcum powder and a thickening agent, uniformly mixing, filtering, and coating on the surface of the high-speed rail electric contact network part to prepare the anti-corrosion conductive coating for the high-speed rail electric contact network part. The coating prepared by the invention is uniformly coated on the surfaces of the parts of the high-speed rail electric contact network to prepare an anti-corrosion conductive coating, the anti-corrosion conductive coating has better conductivity and remarkable anti-corrosion and anti-rust effects, the flexibility and adhesive force of the coating are high, the impact resistance is good, and the performances of water resistance, acid and alkali resistance, salt spray resistance and the like are obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, and in particular to an anti-corrosion conductive coating for high-speed railway electric contact network components and a preparation method thereof. Background Art

[0002] The high-speed railway power contact network is an important part of the high-speed railway traction power supply system, which provides the required electricity for high-speed trains. The power supply system of high-speed railway mainly includes traction substations, contact networks, return lines and high-speed trains themselves. The operating speed and stability of high-speed railways are closely related to the power quality of the power grid. The components of the high-speed railway power contact network are easily corroded due to long-term exposure to the outdoors and the influence of various environmental factors such as rain, moisture, salt spray, industrial pollution, etc. In order to prevent corrosion, anti-corrosion conductive coatings are usually applied to the contact network components. These coatings can not only provide anti-corrosion protection, but also maintain or enhance the conductive properties of the components.

[0003] At present, the most effective way to prevent metal corrosion is to isolate the protected metal from the corrosive medium. Anti-corrosion coatings usually serve as a functional barrier to block substances such as water and oxygen. Heavy metals such as lead and chromium or volatile organic solvents such as xylene contained in traditional anti-corrosion coatings are prone to pollution, which not only affects health but also causes environmental pollution. Therefore, the research and development of water-based anti-corrosion coatings with strong corrosion resistance and green environmental protection has become an urgent problem to be solved.

[0004] Conductive coatings are functional coatings that give objects the ability to conduct electricity and eliminate accumulated static charges. Due to their special functions, they can be used in the fields of eliminating static electricity and electromagnetic shielding. In recent years, both at home and abroad, efforts have been made to develop composite conductive fillers, which are obtained by using cheap and lightweight materials such as glass, mica, graphite, etc. as substrates or core materials, and coating their surfaces with conductive materials such as silver, nickel, copper, etc. At present, this type of powder is called composite conductive powder, which has been widely used in conductive and anti-corrosion coatings. However, the conductive substances added to the coating often cause the conductive properties of the conductive coating to fail due to their stability; and some conductive substances with high stability have a high unit price, resulting in a large increase in production costs; some conductive substances with low unit prices have the problem of poor conductivity; in addition, directly adding composite conductive powders to the coating system also has the problem of poor conductivity. Summary of the invention

[0005] The purpose of the present invention is to propose an anti-corrosion conductive coating for high-speed railway power contact network components and a preparation method thereof. The prepared coating is evenly coated on the surface of the high-speed railway power contact network components and cured to obtain an anti-corrosion conductive coating. While having good conductivity, the coating has significant anti-corrosion and anti-rust effects. The coating has high flexibility and adhesion, good impact resistance, and significantly improved water resistance, acid and alkali resistance, and salt spray resistance, and has good application prospects.

[0006] The technical solution of the present invention is achieved in this way:

[0007] The invention provides a method for preparing an anti-corrosion conductive coating for high-speed railway electric contact network parts. The method comprises the following steps: reacting graphene oxide with p-phenylenediamine to form a composite, then reacting the composite with acid-treated multi-walled carbon nanotubes, reducing the composite with hydrazine hydrate, polymerizing the composite to obtain a graphene-poly-p-phenylenediamine-multi-walled carbon nanotube composite, adding the composite together with nano-silicon dioxide into epoxy resin to obtain a modified epoxy resin, uniformly mixing the composite with water-based polyurethane modified with resveratrol, adding a pH regulator, a dispersant, a defoamer, water, a pigment, talcum powder and a thickener, mixing the composite and stirring the composite, filtering the composite, uniformly coating the composite on the surface of the high-speed railway electric contact network parts, and curing the composite to obtain the anti-corrosion conductive coating for the high-speed railway electric contact network parts.

[0008] As a further improvement of the present invention, the following steps are included:

[0009] S1. Preparation of graphene oxide-p-phenylenediamine complex: dispersing graphene oxide in water, adding p-phenylenediamine and ammonia water, heating and stirring under reflux reaction, filtering, washing, and drying to obtain a graphene oxide-p-phenylenediamine complex;

[0010] S2. Preparation of graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite: adding multi-walled carbon nanotubes to nitric acid, heating, filtering, washing, and drying to obtain acid-treated multi-walled carbon nanotubes, adding to hydrochloric acid, adding graphene oxide-p-phenylenediamine composite and sodium nitrite, heating to reflux reaction, filtering, washing, and drying to obtain graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite;

[0011] S3. Preparation of graphene-p-phenylenediamine-multi-walled carbon nanotubes: reducing the graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite with hydrazine hydrate vapor to obtain a graphene-p-phenylenediamine-multi-walled carbon nanotube composite;

[0012] S4. Preparation of graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes: adding a graphene-p-phenylenediamine-multi-walled carbon nanotube complex to hydrochloric acid, dropping an initiator solution, stirring to react, filtering, washing, and drying to obtain graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes;

[0013] S5. Preparation of modified epoxy resin: polyethylene glycol and multifunctional epoxy resin are mixed, boron trifluoride ether is added, heated and stirred to react, and an emulsifier is prepared, the emulsifier and epoxy resin are added to water, heated and stirred to react, and then nano-silica and graphene-poly-p-phenylenediamine-multi-walled carbon nanotubes are added, stirred to react, and colloid milled to prepare a modified epoxy resin emulsion;

[0014] S6. Preparation of modified waterborne polyurethane: adding polytetrahydrofuran diol to acetone, heating, adding isocyanate dropwise, stirring to react, adding catalyst, dimethylol propionic acid, 1,4-butanediol and resveratrol dropwise, continuing to stir to react, cooling to room temperature, adding triethylamine, stirring to react, adding deionized water, emulsifying, and removing acetone under reduced pressure to obtain modified waterborne polyurethane;

[0015] S7. Preparation of anti-corrosion conductive coating for high-speed railway power contact network components: Stir and mix modified water-based polyurethane, modified epoxy resin emulsion, pH adjuster, dispersant, defoaming agent and water evenly, add pigment and talcum powder, colloid mill, add thickener, stir evenly, filter, and evenly apply on the surface of high-speed railway power contact network components, and cure to obtain anti-corrosion conductive coating for high-speed railway power contact network components.

[0016] As a further improvement of the present invention, in step S1, the mass ratio of graphene oxide, p-phenylenediamine and ammonia water is 1:1-2:3-4, the time of the heating, stirring and reflux reaction is 4-6 hours, and the filtration is carried out by 0.22 μm microporous membrane filtration.

[0017] As a further improvement of the present invention, the solid-liquid ratio of the multi-walled carbon nanotubes and nitric acid in step S2 is 1:30-50 g / mL, the concentration of the nitric acid is 2-3 mol / L, the temperature of the heating treatment is 50-70°C, the time is 1-2 h, the mass ratio of the acid-treated multi-walled carbon nanotubes, graphene oxide-p-phenylenediamine complex and sodium nitrite is 10:12-15:4-6, the concentration of the hydrochloric acid is 35-45wt%, the heating reflux reaction time is 3-5 h, and the filtration is carried out using a 0.22 μm microporous membrane.

[0018] As a further improvement of the present invention, the reduction time in step S3 is 10-12 hours.

[0019] As a further improvement of the present invention, in step S4, the mass ratio of the graphene-p-phenylenediamine-multi-walled carbon nanotube composite and the initiator is 100:0.5-1, the concentration of the hydrochloric acid is 20-30wt%, the initiator is selected from at least one of potassium persulfate, sodium persulfate, and ammonium persulfate, and the stirring reaction time is 3-5h.

[0020] As a further improvement of the present invention, the mass ratio of the polyethylene glycol, the multifunctional epoxy resin, and the boron trifluoride ether in step S5 is 3-5:4-7:0.5-1, the multifunctional epoxy resin is the epoxy resin DEN-425, the mass ratio of the emulsifier, the epoxy resin, the nano-silica, and the graphene-polyparaphenylenediamine-multi-walled carbon nanotubes is 2-4:60-80:1-2:3-5, the rotation speed of the colloid mill is 10000-12000r / min, the time is 1-3h, and the epoxy resin is bisphenol A or bisphenol F type epoxy resin.

[0021] As a further improvement of the present invention, the mass ratio of the polytetrahydrofuran diol, isocyanate, catalyst, dimethylol propionic acid, 1,4-butanediol, modifier and triethylamine in step S6 is 10: 5-7: 0.01-0.02: 1-2: 0.2-0.4: 2-4: 0.5-1.5, the heating temperature is 55-65°C, the isocyanate is selected from at least one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate and lysine diisocyanate, the catalyst is dibutyltin dilaurate or stannous octoate, and the emulsification time is 20-30 min.

[0022] As a further improvement of the present invention, the mass ratio of the modified waterborne polyurethane, modified epoxy resin emulsion, pH regulator, dispersant, defoamer, water, pigment, talcum powder and thickener in step S7 is 25-35:7-9:1-2:0.2-0.4:0.1-0.2:20-40:1-3:1-2:0.5-1, the pH regulator is N,N-dimethylethanol, the dispersant is 104BC, the defoamer is BYK-024, the pigment is carbon black, and the thickener is polyurethane RM-8W.

[0023] The present invention further protects an anti-corrosion conductive coating for high-speed railway power contact network components prepared by the above-mentioned preparation method.

[0024] The present invention has the following beneficial effects:

[0025] Compared with traditional solvent-based polyurethane coatings, water-based polyurethane coatings are insufficient in water resistance, chemical resistance, heat resistance and fullness. The present invention uses resveratrol, which has both conjugated double bonds and hydroxyl structures, as an internal cross-linking modifier, which can react with isocyanate to form polyurethane segments with branches, playing the role of an internal cross-linking agent. At the same time, the conjugated double bonds can be oxidized and cross-linked to form a film, thereby improving the film-forming property of the water-based emulsion. After the water-based polyurethane anti-corrosion coating film is formed, the water resistance, acid and alkali resistance, and salt spray resistance and other properties are significantly improved.

[0026] Epoxy resin has excellent anti-corrosion protection, but it is insufficient in toughness and impact resistance. Graphene is an emerging two-dimensional nanomaterial. Graphene is the thinnest (0.34nm) and hardest nanomaterial. The theoretical resistivity of a graphene single layer is about 10 -6 Ω·cm, is the material with the lowest resistivity at present, and like graphite, has excellent chemical resistance. Compared with metal fillers with high density, graphene is not easy to sink in the coating, and the coating has stable conductivity, temperature resistance and non-oxidation. However, the easy agglomeration of graphene makes it difficult to disperse evenly in epoxy resin emulsion.

[0027] Graphene and carbon nanotubes can greatly improve the coating's aging resistance, anti-leakage, and scrub resistance, while also extending the coating's service life. The conductivity of the composite conductive filler prepared from graphene and carbon nanotubes is better than the performance of each filler alone.

[0028] Therefore, the present invention forms a composite of graphene oxide and carbon nanotubes through the connecting effect of p-phenylenediamine, the grafted structure is conducive to the dispersion of carbon nanotubes and graphene, and the support effect of the carbon nanotubes also prevents the restacking of graphene oxide sheets, thereby increasing the conductivity, and further under the reduction effect of hydrazine hydrate vapor, a graphene-p-phenylenediamine-multi-walled carbon nanotube composite with better conductivity is prepared.

[0029] In addition, the graphene-p-phenylenediamine-multi-walled carbon nanotube composite can be polymerized to form polyp-phenylenediamine under the action of an initiator. The raw materials are easily available, the synthesis method is simple, pollution-free, and the composite has the advantages of light weight, high chemical stability, good environmental stability, structural diversity, unique doping mechanism, high conductivity, and reversible redox characteristics, which further improve the conductivity of the prepared coating.

[0030] The present invention improves the dispersibility of the composite by allowing the residual amino groups of the graphene-poly-p-phenylenediamine-multi-walled carbon nanotubes to react with the residual epoxy groups of the epoxy resin, solves the agglomeration problem easily generated by physical blending and adding composites, and achieves a strong physical shielding effect and conductive properties of the coating with a small amount of composites, and also greatly improves the flexibility and impact resistance of the coating. The addition of nano-silicon dioxide can improve the adhesion of the coating through inorganic-inorganic interaction, and also improves the mechanical properties of the coating.

[0031] The coating prepared by the present invention is evenly coated on the surface of high-speed railway power contact network components and cured to obtain an anti-corrosion conductive coating. While having good conductivity, the coating has significant anti-corrosion and anti-rust effects. The coating has high flexibility and adhesion, good impact resistance, and significantly improved water resistance, acid and alkali resistance, and salt spray resistance, and has good application prospects. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The dispersant 104BC is Korean KS Rheorlow DW-104BC dispersant.

[0034] Polyurethane RM-8W is Rohm and Haas thickener RM8W.

[0035] Epoxy resin DEN-425 is Dow phenolic epoxy resin DEN 425.

[0036] Nano-silicon dioxide, with an average particle size of 100-200 nm, was purchased from Hubei Huifu Nanomaterials Co., Ltd.

[0037] Example 1

[0038] This embodiment provides a method for preparing an anti-corrosion conductive coating for high-speed railway power contact network components, comprising the following steps:

[0039] S1. Preparation of graphene oxide-p-phenylenediamine complex: 1 g of graphene oxide was dispersed in 100 mL of water, 1 g of p-phenylenediamine and 2 g of aqueous ammonia were added, the mixture was heated and stirred under reflux for 4 h, filtered through a 0.22 μm microporous membrane, washed, and dried to obtain a graphene oxide-p-phenylenediamine complex;

[0040] S2. Preparation of graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite: 1 g of multi-walled carbon nanotubes was added to 30 mL of 2 mol / L nitric acid, heated to 50° C., treated for 1 h, filtered, washed, and dried to obtain acid-treated multi-walled carbon nanotubes; 1 g of acid-treated multi-walled carbon nanotubes was added to 35 wt % hydrochloric acid, 1.2 g of graphene oxide-p-phenylenediamine composite and 0.4 g of sodium nitrite were added, heated to reflux for 3 h, filtered with a 0.22 μm microporous membrane, washed, and dried to obtain graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite;

[0041] S3. Preparation of graphene-p-phenylenediamine-multi-walled carbon nanotubes: The graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite was reduced with hydrazine hydrate vapor for 10 h to obtain a graphene-p-phenylenediamine-multi-walled carbon nanotube composite;

[0042] S4. Preparation of graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes: 1 g of graphene-p-phenylenediamine-multi-walled carbon nanotube composite was added to 100 mL of 20 wt% hydrochloric acid, and an aqueous solution containing 0.05 g of sodium persulfate was added dropwise, and the mixture was stirred for 3 h, filtered, washed, and dried to obtain graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes;

[0043] S5. Preparation of modified epoxy resin: 3 g of polyethylene glycol 1000 and 4 g of epoxy resin DEN-425 were mixed, 0.5 g of boron trifluoride ether was added, the mixture was heated to 85 ° C, stirred and reacted for 3 h to obtain an emulsifier, 2 g of the emulsifier and 60 g of bisphenol F epoxy resin were added to 500 mL of water, heated to 70 ° C, stirred and reacted for 1 h, and then 1 g of nano-silica and 3 g of graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes were added, the mixture was stirred and reacted for 1 h, and the mixture was colloid milled at 10000 r / min for 1 h to obtain a modified epoxy resin emulsion;

[0044] S6. Preparation of modified waterborne polyurethane: 10 g of polytetrahydrofuran diol 2000 was added to 50 mL of acetone, heated to 55 ° C, 5 g of toluene diisocyanate was added dropwise, stirred for 1 h, 0.01 g of dibutyltin dilaurate, 1 g of dimethylolpropionic acid, 0.2 g of 1,4-butanediol and 2 g of resveratrol were added, and the reaction was continued with stirring for 4 h, cooled to room temperature, 0.5 g of triethylamine was added, stirred for 30 min, 30 mL of deionized water was added, emulsified for 20 min, and acetone was removed under reduced pressure to obtain a modified waterborne polyurethane;

[0045] S7. Preparation of anti-corrosion conductive coating for high-speed railway power contact network components: stir and mix 25g modified waterborne polyurethane, 7g modified epoxy resin emulsion, 1g N,N-dimethylethanol, 0.2g dispersant 104BC, 0.1g defoamer BYK-024 and 20mL water for 20min, add 1g carbon black and 1g talcum powder, 10000r / min colloid mill for 1h, add 0.5g polyurethane RM-8W, stir and mix for 20min, filter, evenly apply on the surface of high-speed railway power contact network components, and cure to obtain anti-corrosion conductive coating for high-speed railway power contact network components.

[0046] Example 2

[0047] This embodiment provides a method for preparing an anti-corrosion conductive coating for high-speed railway power contact network components, comprising the following steps:

[0048] S1. Preparation of graphene oxide-p-phenylenediamine complex: 1 g of graphene oxide was dispersed in 100 mL of water, 2 g of p-phenylenediamine and 4 g of aqueous ammonia were added, the mixture was heated and stirred under reflux for 6 h, filtered through a 0.22 μm microporous membrane, washed, and dried to obtain a graphene oxide-p-phenylenediamine complex;

[0049] S2. Preparation of graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite: 1 g of multi-walled carbon nanotubes was added to 50 mL of 3 mol / L nitric acid, heated to 70° C., treated for 2 h, filtered, washed, and dried to obtain acid-treated multi-walled carbon nanotubes; 1 g of acid-treated multi-walled carbon nanotubes was added to 45 wt % hydrochloric acid, 1.5 g of graphene oxide-p-phenylenediamine composite and 0.6 g of sodium nitrite were added, heated to reflux for 5 h, filtered with a 0.22 μm microporous membrane, washed, and dried to obtain graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite;

[0050] S3. Preparation of graphene-p-phenylenediamine-multi-walled carbon nanotubes: The graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite was reduced with hydrazine hydrate vapor for 12 hours to obtain a graphene-p-phenylenediamine-multi-walled carbon nanotube composite;

[0051] S4. Preparation of graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes: 1 g of graphene-p-phenylenediamine-multi-walled carbon nanotube composite was added to 100 mL of 30 wt% hydrochloric acid, and an aqueous solution containing 0.1 g of potassium persulfate was added dropwise, and the mixture was stirred for 5 h, filtered, washed, and dried to obtain graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes;

[0052] S5. Preparation of modified epoxy resin: 5 g of polyethylene glycol 1000 and 7 g of epoxy resin DEN-425 were mixed, 1 g of boron trifluoride ether was added, the mixture was heated to 95 ° C, stirred and reacted for 5 h to obtain an emulsifier, 4 g of the emulsifier and 80 g of bisphenol F epoxy resin were added to 500 mL of water, heated to 80 ° C, stirred and reacted for 2 h, and then 2 g of nano-silica and 5 g of graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes were added, the mixture was stirred and reacted for 2 h, and the mixture was colloid milled at 12000 r / min for 3 h to obtain a modified epoxy resin emulsion;

[0053] S6. Preparation of modified waterborne polyurethane: 10 g of polytetrahydrofuran diol 2000 was added to 50 mL of acetone, heated to 65 ° C, 7 g of toluene diisocyanate was added dropwise, stirred for 3 h, 0.02 g of dibutyltin dilaurate, 2 g of dimethylolpropionic acid, 0.4 g of 1,4-butanediol and 4 g of resveratrol were added, and the reaction was continued with stirring for 6 h, cooled to room temperature, 1.5 g of triethylamine was added, stirred for 50 min, 50 mL of deionized water was added, emulsified for 30 min, and acetone was removed under reduced pressure to obtain a modified waterborne polyurethane;

[0054] S7. Preparation of anti-corrosion conductive coating for high-speed railway power contact network components: stir and mix 35g modified waterborne polyurethane, 9g modified epoxy resin emulsion, 2g N,N-dimethylethanol, 0.4g dispersant 104BC, 0.2g defoamer BYK-024 and 40mL water for 20min, add 3g carbon black and 2g talcum powder, colloid mill at 12000r / min for 3h, add 1g polyurethane RM-8W, stir and mix for 20min, filter, evenly apply on the surface of high-speed railway power contact network components, and cure to obtain the anti-corrosion conductive coating for high-speed railway power contact network components.

[0055] Example 3

[0056] This embodiment provides a method for preparing an anti-corrosion conductive coating for high-speed railway power contact network components, comprising the following steps:

[0057] S1. Preparation of graphene oxide-p-phenylenediamine complex: 1 g of graphene oxide was dispersed in 100 mL of water, 1.5 g of p-phenylenediamine and 3 g of aqueous ammonia were added, the mixture was heated and stirred under reflux for 5 h, filtered through a 0.22 μm microporous membrane, washed, and dried to obtain a graphene oxide-p-phenylenediamine complex;

[0058] S2. Preparation of graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite: 1 g of multi-walled carbon nanotubes was added to 40 mL of 2.5 mol / L nitric acid, heated to 60 ° C, treated for 1.5 h, filtered, washed, and dried to obtain acid-treated multi-walled carbon nanotubes, 1 g of acid-treated multi-walled carbon nanotubes was added to 40 wt% hydrochloric acid, 1.35 g of graphene oxide-p-phenylenediamine composite and 0.5 g of sodium nitrite were added, heated to reflux for 4 h, filtered with a 0.22 μm microporous membrane, washed, and dried to obtain graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite;

[0059] S3. Preparation of graphene-p-phenylenediamine-multi-walled carbon nanotubes: The graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite was reduced with hydrazine hydrate vapor for 11 hours to obtain a graphene-p-phenylenediamine-multi-walled carbon nanotube composite;

[0060] S4. Preparation of graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes: 1 g of graphene-p-phenylenediamine-multi-walled carbon nanotube composite was added to 100 mL of 25 wt% hydrochloric acid, and an aqueous solution containing 0.07 g of ammonium persulfate was added dropwise, and the mixture was stirred for 4 h, filtered, washed, and dried to obtain graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes;

[0061] S5. Preparation of modified epoxy resin: 4 g of polyethylene glycol 1000 and 5.5 g of epoxy resin DEN-425 were mixed, 0.7 g of boron trifluoride ether was added, heated to 90 ° C, stirred for 4 h, and an emulsifier was prepared. 3 g of emulsifier and 70 g of bisphenol F epoxy resin were added to 500 mL of water, heated to 75 ° C, stirred for 1.5 h, and then 1.5 g of nano-silica and 4 g of graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes were added, stirred for 1.5 h, and 11000 r / min colloid mill was used for 2 h to obtain a modified epoxy resin emulsion;

[0062] S6. Preparation of modified waterborne polyurethane: 10 g of polytetrahydrofuran diol 2000 was added to 50 mL of acetone, heated to 60 ° C, 6 g of toluene diisocyanate was added dropwise, stirred for 2 h, 0.015 g of dibutyltin dilaurate, 1.5 g of dimethylolpropionic acid, 0.3 g of 1,4-butanediol and 3 g of resveratrol were added, and the reaction was continued with stirring for 5 h, cooled to room temperature, 1 g of triethylamine was added, stirred for 40 min, 40 mL of deionized water was added, emulsified for 25 min, and acetone was removed under reduced pressure to obtain a modified waterborne polyurethane;

[0063] S7. Preparation of anti-corrosion conductive coating for high-speed railway power contact network components: 30g modified waterborne polyurethane, 8g modified epoxy resin emulsion, 1.5g N,N-dimethylethanol, 0.3g dispersant 104BC, 0.15g defoamer BYK-024 and 30mL water were stirred and mixed for 20min, 2g carbon black and 1.5g talcum powder were added, 11000r / min colloid mill was used for 2h, 0.7g polyurethane RM-8W was added, stirred and mixed for 20min, filtered, and evenly coated on the surface of high-speed railway power contact network components, and cured to obtain the anti-corrosion conductive coating for high-speed railway power contact network components.

[0064] Comparative Example 1

[0065] Compared with Example 3, the difference is that step S3 is not performed.

[0066] The details are as follows:

[0067] S1. Preparation of graphene oxide-p-phenylenediamine complex: 1 g of graphene oxide was dispersed in 100 mL of water, 1.5 g of p-phenylenediamine and 3 g of aqueous ammonia were added, the mixture was heated and stirred under reflux for 5 h, filtered through a 0.22 μm microporous membrane, washed, and dried to obtain a graphene oxide-p-phenylenediamine complex;

[0068] S2. Preparation of graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite: 1 g of multi-walled carbon nanotubes was added to 40 mL of 2.5 mol / L nitric acid, heated to 60 ° C, treated for 1.5 h, filtered, washed, and dried to obtain acid-treated multi-walled carbon nanotubes, 1 g of acid-treated multi-walled carbon nanotubes was added to 40 wt% hydrochloric acid, 1.35 g of graphene oxide-p-phenylenediamine composite and 0.5 g of sodium nitrite were added, heated to reflux for 4 h, filtered with a 0.22 μm microporous membrane, washed, and dried to obtain graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite;

[0069] S3. Preparation of graphene oxide-poly(p-phenylenediamine)-multi-walled carbon nanotubes: 1 g of graphene oxide-p-phenylenediamine-multi-walled carbon nanotubes composite was added to 100 mL of 25 wt% hydrochloric acid, and an aqueous solution containing 0.07 g of ammonium persulfate was added dropwise, and the mixture was stirred for 4 h, filtered, washed, and dried to obtain graphene oxide-poly(p-phenylenediamine)-multi-walled carbon nanotubes;

[0070] S4. Preparation of modified epoxy resin: 4 g of polyethylene glycol 1000 and 5.5 g of epoxy resin DEN-425 were mixed, 0.7 g of boron trifluoride ether was added, the mixture was heated to 90 ° C, stirred and reacted for 4 h to obtain an emulsifier, 3 g of the emulsifier and 70 g of bisphenol F epoxy resin were added to 500 mL of water, heated to 75 ° C, stirred and reacted for 1.5 h, and then 1.5 g of nano-silicon dioxide and 4 g of graphene oxide-poly(p-phenylenediamine)-multi-walled carbon nanotubes were added, the mixture was stirred and reacted for 1.5 h, and the mixture was colloid milled at 11000 r / min for 2 h to obtain a modified epoxy resin emulsion;

[0071] S5. Preparation of modified waterborne polyurethane: 10 g of polytetrahydrofuran diol 2000 was added to 50 mL of acetone, heated to 60 ° C, 6 g of toluene diisocyanate was added dropwise, stirred for 2 h, 0.015 g of dibutyltin dilaurate, 1.5 g of dimethylolpropionic acid, 0.3 g of 1,4-butanediol and 3 g of resveratrol were added, and the reaction was continued with stirring for 5 h, cooled to room temperature, 1 g of triethylamine was added, stirred for 40 min, 40 mL of deionized water was added, emulsified for 25 min, and acetone was removed under reduced pressure to obtain a modified waterborne polyurethane;

[0072] S6. Preparation of anti-corrosion conductive coating for high-speed railway power contact network components: 30g modified waterborne polyurethane, 8g modified epoxy resin emulsion, 1.5g N,N-dimethylethanol, 0.3g dispersant 104BC, 0.15g defoamer BYK-024 and 30mL water were stirred and mixed for 20min, 2g carbon black and 1.5g talcum powder were added, 11000r / min colloid mill was used for 2h, 0.7g polyurethane RM-8W was added, stirred and mixed for 20min, filtered, and evenly coated on the surface of high-speed railway power contact network components, and cured to obtain the anti-corrosion conductive coating for high-speed railway power contact network components.

[0073] Comparative Example 2

[0074] Compared with Example 3, the difference is that step S4 is not performed.

[0075] The details are as follows:

[0076] S1. Preparation of graphene oxide-p-phenylenediamine complex: 1 g of graphene oxide was dispersed in 100 mL of water, 1.5 g of p-phenylenediamine and 3 g of aqueous ammonia were added, the mixture was heated and stirred under reflux for 5 h, filtered through a 0.22 μm microporous membrane, washed, and dried to obtain a graphene oxide-p-phenylenediamine complex;

[0077] S2. Preparation of graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite: 1 g of multi-walled carbon nanotubes was added to 40 mL of 2.5 mol / L nitric acid, heated to 60 ° C, treated for 1.5 h, filtered, washed, and dried to obtain acid-treated multi-walled carbon nanotubes, 1 g of acid-treated multi-walled carbon nanotubes was added to 40 wt% hydrochloric acid, 1.35 g of graphene oxide-p-phenylenediamine composite and 0.5 g of sodium nitrite were added, heated to reflux for 4 h, filtered with a 0.22 μm microporous membrane, washed, and dried to obtain graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite;

[0078] S3. Preparation of graphene-p-phenylenediamine-multi-walled carbon nanotubes: The graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite was reduced with hydrazine hydrate vapor for 11 hours to obtain a graphene-p-phenylenediamine-multi-walled carbon nanotube composite;

[0079] S4. Preparation of modified epoxy resin: 4 g of polyethylene glycol 1000 and 5.5 g of epoxy resin DEN-425 were mixed, 0.7 g of boron trifluoride ether was added, the mixture was heated to 90 ° C, stirred and reacted for 4 h to obtain an emulsifier, 3 g of the emulsifier and 70 g of bisphenol F epoxy resin were added to 500 mL of water, heated to 75 ° C, stirred and reacted for 1.5 h, and then 1.5 g of nano-silica and 4 g of graphene-p-phenylenediamine-multi-walled carbon nanotube composite were added, stirred and reacted for 1.5 h, and 11000 r / min colloid mill was used for 2 h to obtain a modified epoxy resin emulsion;

[0080] S5. Preparation of modified waterborne polyurethane: 10 g of polytetrahydrofuran diol 2000 was added to 50 mL of acetone, heated to 60 ° C, 6 g of toluene diisocyanate was added dropwise, stirred for 2 h, 0.015 g of dibutyltin dilaurate, 1.5 g of dimethylolpropionic acid, 0.3 g of 1,4-butanediol and 3 g of resveratrol were added, and the reaction was continued with stirring for 5 h, cooled to room temperature, 1 g of triethylamine was added, stirred for 40 min, 40 mL of deionized water was added, emulsified for 25 min, and acetone was removed under reduced pressure to obtain a modified waterborne polyurethane;

[0081] S6. Preparation of anti-corrosion conductive coating for high-speed railway power contact network components: 30g modified waterborne polyurethane, 8g modified epoxy resin emulsion, 1.5g N,N-dimethylethanol, 0.3g dispersant 104BC, 0.15g defoamer BYK-024 and 30mL water were stirred and mixed for 20min, 2g carbon black and 1.5g talcum powder were added, 11000r / min colloid mill was used for 2h, 0.7g polyurethane RM-8W was added, stirred and mixed for 20min, filtered, and evenly coated on the surface of high-speed railway power contact network components, and cured to obtain the anti-corrosion conductive coating for high-speed railway power contact network components.

[0082] Comparative Example 3

[0083] Compared with Example 3, the difference is that in step S5, graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes are replaced by a mixture of equal masses of graphene, poly(p-phenylenediamine) and multi-walled carbon nanotubes in a mass ratio of 0.54:0.81:1.

[0084] The details are as follows:

[0085] S5. Preparation of modified epoxy resin: Mix 4g polyethylene glycol 1000 and 5.5g epoxy resin DEN-425, add 0.7g boron trifluoride etherate, heat to 90°C, stir and react for 4h to obtain an emulsifier, add 3g emulsifier and 70g bisphenol F epoxy resin into 500mL water, heat to 75°C, stir and react for 1.5h, then add 1.5g nano-silica and 4g composite (a mixture of graphene, polyparaphenylenediamine, and multi-walled carbon nanotubes in a mass ratio of 0.54:0.81:1), stir and react for 1.5h, and colloid mill at 11000r / min for 2h to obtain a modified epoxy resin emulsion.

[0086] Comparative Example 4

[0087] Compared with Example 3, the difference is that graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes are not added in step S5.

[0088] The details are as follows:

[0089] S5. Preparation of modified epoxy resin: Mix 4g polyethylene glycol 1000 and 5.5g epoxy resin DEN-425, add 0.7g boron trifluoride etherate, heat to 90°C, stir and react for 4h to obtain an emulsifier, add 3g emulsifier and 70g bisphenol F epoxy resin into 500mL water, heat to 75°C, stir and react for 1.5h, add 1.5g nano-silica, stir and react for 1.5h, and colloid mill at 11000r / min for 2h to obtain a modified epoxy resin emulsion.

[0090] Comparative Example 5

[0091] Compared with Example 3, the difference is that resveratrol is not added in step S6.

[0092] The details are as follows:

[0093] S6. Preparation of waterborne polyurethane: Add 10g of polytetrahydrofuran diol 2000 to 50mL of acetone, heat to 60°C, add 6g of toluene diisocyanate dropwise, stir and react for 2h, add 0.015g of dibutyltin dilaurate, 1.5g of dihydroxymethylpropionic acid, and 0.3g of 1,4-butanediol, continue to stir and react for 5h, cool to room temperature, add 1g of triethylamine, stir and react for 40min, add 40mL of deionized water, emulsify for 25min, remove acetone under reduced pressure, and obtain waterborne polyurethane.

[0094] Test Example 1

[0095] The anti-corrosion conductive coatings of high-speed railway power contact network components prepared in Examples 1-3 and Comparative Examples 1-5 were tested as follows:

[0096] Adhesion test: The adhesion is tested according to GB / T5210-2006 coating adhesion test method (pull-off method).

[0097] The pencil hardness test refers to GB / T6739-2006 method.

[0098] The flexibility test refers to the GB / T1731-2020 method.

[0099] Impact resistance test: refer to GB / T1732-2020 method, the mass of the weight is (1000±1)g, magnify 4 times to observe whether the paint film is damaged, and the maximum weight drop height when there is no damage is the measurement result.

[0100] Volume resistivity test: The volume resistivity of the coating was measured in accordance with GB / T2439-2001.

[0101] The results are shown in Table 1.

[0102] Table 1

[0103]

[0104] It can be seen from the above table that the layers prepared in Examples 1-3 of the present invention have higher adhesion, greater hardness, better flexibility, better impact resistance, and better electrical conductivity.

[0105] Test Example 2

[0106] The anti-corrosion conductive coatings of high-speed railway power contact network components prepared in Examples 1-3 and Comparative Examples 1-5 were tested as follows:

[0107] The neutral salt spray resistance test was carried out in accordance with the provisions of GB / T1771-2007 "Determination of neutral salt spray resistance of paints and varnishes" on a JD-120 (600L) salt spray tester. The mass concentration of the sodium chloride solution was (50±5) g / L and the pH was 6.5-7.0.

[0108] The acid resistance is tested according to the immersion method specified in GB / T9274-1988 "Determination of resistance of paints and varnishes to liquid media", with a sulfuric acid mass fraction of 5%. Defects are observed after immersion for 24 hours.

[0109] The organic solvent resistance test is carried out according to the manual wiping method specified in GB / T23989-2009 "Determination of Solvent Resistance of Coatings by Wiping". Wipe back and forth 25 times with a finger wrapped in absorbent cotton to observe whether it is damaged and the base material is exposed.

[0110] The water resistance test refers to GB / T1733-1993, the test temperature is 40℃, and the test time is 24h.

[0111] The results are shown in Table 2.

[0112] Table 2

[0113]

[0114]

[0115] It can be seen from the above table that the coatings prepared in Examples 1-3 of the present invention have good acid resistance, water resistance, salt spray resistance, and organic solvent resistance.

[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an anti-corrosion conductive coating for high-speed railway power contact network components, characterized in that: Graphene oxide is reacted with p-phenylenediamine to form a complex, which is then reacted with acid-treated multi-walled carbon nanotubes. After reduction with hydrazine hydrate, the complex is polymerized to obtain a graphene-polyp-phenylenediamine-multi-walled carbon nanotube complex, which is added into epoxy resin together with nano-silicon dioxide to obtain a modified epoxy resin, which is evenly mixed with water-based polyurethane modified with resveratrol, a pH regulator, a dispersant, a defoamer, water, a pigment, talcum powder, and a thickener, and the mixture is evenly stirred. The mixture is filtered and evenly coated on the surface of high-speed railway power contact network components, and cured to obtain an anti-corrosion conductive coating for high-speed railway power contact network components.

2. The preparation method according to claim 1, characterized in that: The following steps are involved: S1. Preparation of graphene oxide-p-phenylenediamine complex: dispersing graphene oxide in water, adding p-phenylenediamine and ammonia water, heating and stirring under reflux reaction, filtering, washing, and drying to obtain a graphene oxide-p-phenylenediamine complex; S2. Preparation of graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite: adding multi-walled carbon nanotubes to nitric acid, heating, filtering, washing, and drying to obtain acid-treated multi-walled carbon nanotubes, adding to hydrochloric acid, adding graphene oxide-p-phenylenediamine composite and sodium nitrite, heating to reflux reaction, filtering, washing, and drying to obtain graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite; S3. Preparation of graphene-p-phenylenediamine-multi-walled carbon nanotubes: reducing the graphene oxide-p-phenylenediamine-multi-walled carbon nanotube composite with hydrazine hydrate vapor to obtain a graphene-p-phenylenediamine-multi-walled carbon nanotube composite; S4. Preparation of graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes: adding a graphene-p-phenylenediamine-multi-walled carbon nanotube complex to hydrochloric acid, dropping an initiator solution, stirring to react, filtering, washing, and drying to obtain graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes; S5. Preparation of modified epoxy resin: polyethylene glycol and multifunctional epoxy resin are mixed, boron trifluoride ether is added, heated and stirred to react, and an emulsifier is prepared, the emulsifier and epoxy resin are added to water, heated and stirred to react, and then nano-silica and graphene-poly-p-phenylenediamine-multi-walled carbon nanotubes are added, stirred to react, and colloid milled to prepare a modified epoxy resin emulsion; S6. Preparation of modified waterborne polyurethane: adding polytetrahydrofuran diol to acetone, heating, adding isocyanate dropwise, stirring to react, adding catalyst, dimethylol propionic acid, 1,4-butanediol and resveratrol dropwise, continuing to stir to react, cooling to room temperature, adding triethylamine, stirring to react, adding deionized water, emulsifying, and removing acetone under reduced pressure to obtain modified waterborne polyurethane; S7. Preparation of anti-corrosion conductive coating for high-speed railway power contact network components: Stir and mix modified water-based polyurethane, modified epoxy resin emulsion, pH adjuster, dispersant, defoaming agent and water evenly, add pigment and talcum powder, colloid mill, add thickener, stir evenly, filter, and evenly apply on the surface of high-speed railway power contact network components, and cure to obtain anti-corrosion conductive coating for high-speed railway power contact network components.

3. The preparation method according to claim 2, characterized in that: In step S1, the mass ratio of graphene oxide, p-phenylenediamine and ammonia water is 1:1-2:3-4, the time of the heating, stirring and reflux reaction is 4-6 hours, and the filtration is carried out by 0.22 μm microporous filter membrane.

4. The preparation method according to claim 2, characterized in that: In step S2, the solid-liquid ratio of the multi-walled carbon nanotubes and nitric acid is 1:30-50 g / mL, the concentration of the nitric acid is 2-3 mol / L, the temperature of the heating treatment is 50-70°C, the time is 1-2 h, the mass ratio of the acid-treated multi-walled carbon nanotubes, graphene oxide-p-phenylenediamine complex and sodium nitrite is 10:12-15:4-6, the concentration of the hydrochloric acid is 35-45 wt%, the heating reflux reaction time is 3-5 h, and the filtration is performed using a 0.22 μm microporous membrane.

5. The preparation method according to claim 2, characterized in that: The reduction time in step S3 is 10-12 hours.

6. The preparation method according to claim 2, characterized in that: In step S4, the mass ratio of the graphene-p-phenylenediamine-multi-walled carbon nanotube composite and the initiator is 100:0.5-1, the concentration of the hydrochloric acid is 20-30wt%, the initiator is selected from at least one of potassium persulfate, sodium persulfate, and ammonium persulfate, and the stirring reaction time is 3-5h.

7. The preparation method according to claim 2, characterized in that: In step S5, the mass ratio of polyethylene glycol, multifunctional epoxy resin and boron trifluoride ether is 3-5:4-7:0.5-1, the multifunctional epoxy resin is epoxy resin DEN-425, the mass ratio of the emulsifier, epoxy resin, nano-silica and graphene-poly(p-phenylenediamine)-multi-walled carbon nanotubes is 2-4:60-80:1-2:3-5, the rotation speed of the colloid mill is 10000-12000 r / min, the time is 1-3h, and the epoxy resin is bisphenol A or bisphenol F epoxy resin.

8. The preparation method according to claim 2, characterized in that: The mass ratio of the polytetrahydrofuran diol, isocyanate, catalyst, dimethylol propionic acid, 1,4-butanediol, modifier and triethylamine in step S6 is 10: 5-7: 0.01-0.02: 1-2: 0.2-0.4: 2-4: 0.5-1.5, the heating temperature is 55-65° C., the isocyanate is selected from at least one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate and lysine diisocyanate, the catalyst is dibutyltin dilaurate or stannous octoate, and the emulsification time is 20-30 min.

9. The preparation method according to claim 2, characterized in that: The mass ratio of the modified waterborne polyurethane, modified epoxy resin emulsion, pH regulator, dispersant, defoamer, water, pigment, talcum powder and thickener in step S7 is 25-35:7-9:1-2:0.2-0.4:0.1-0.2:20-40:1-3:1-2:0.5-1, the pH regulator is N,N-dimethylethanol, the dispersant is 104BC, the defoamer is BYK-024, the pigment is carbon black, and the thickener is polyurethane RM-8W.

10. An anti-corrosion conductive coating for high-speed railway power contact network components prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of light-resistant and waterproof waterborne polyurethane paint

    CN104893540A

  • Graphene modified epoxy resin heavy duty anticorrosion paint, and preparation method thereof

    CN109957309A

  • Graphene conductive anticorrosive coating for grounding grid and preparation method thereof

    CN110713743A

  • High-solid-content water-based graphene anticorrosive paint as well as preparation method and application thereof

    CN114752279A

  • High-strength stainless steel band

    CN118440584A