Antibacterial cleaning agent for glass cleaning machine and preparation method of antibacterial cleaning agent

Through the combination of modified zinc oxide nanoparticles and oil removal agent, a high-volatile antibacterial cleaning agent is formed, which solves the problem of poor oil and antibacterial effects in glass cleaning machines, and achieves efficient cleaning and long-term antibacterial effects, protects the Clean and safe glass surfaces.

CN118931665AInactive Publication Date: 2024-11-12FOSHAN YICHUAN GLASS MASCH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410981273.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The cleaning agents used in existing glass cleaning machines are not effective in removing oil stains and antibacterials, resulting in accumulation of dirt and grease on the surface of the glass, increasing the risk of cross-contamination, and affecting the cleaning effect and hygiene and safety.

Method used

Modified zinc oxide nanoparticles and oil removal agents are used to modify zinc oxide nanoparticles through fluorosiloxane, and combined with anhydrous ethanol to form a highly volatile antibacterial cleaning agent, and the fluorosiloxane modification layer is used. Improve antibacterial properties and wear resistance, and combine cyclohexanone mannitol to improve oil removal ability.

Benefits of technology

It achieves efficient removal of oil stains and antibacterials, improves cleaning efficiency and antibacterial durability, protects the hygiene of the glass surface and prevents wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956133930000031
    Figure BDA0004956133930000031
  • Figure BDA0004956133930000032
    Figure BDA0004956133930000032
  • Figure BDA0004956133930000051
    Figure BDA0004956133930000051
Patent Text Reader

Abstract

The invention discloses an antibacterial cleaning agent for a glass cleaning machine and a preparation method of the antibacterial cleaning agent. The preparation method of the antibacterial cleaning agent for the glass cleaning machine comprises the following steps: (1) preparing zinc oxide nanoparticles by using zinc acetate dihydrate and citric acid as raw materials, and then modifying the zinc oxide nanoparticles by using fluorosiloxane to obtain modified zinc oxide nanoparticles; (2) dispersing the modified zinc oxide nanoparticles and a degreaser into absolute ethyl alcohol to obtain the antibacterial cleaning agent. The zinc oxide nanoparticles are modified to obtain the antibacterial, hydrophilic, wear-resistant and anti-aging modified zinc oxide nanoparticles, the detergent has a better cleaning effect due to the addition of the degreaser, the detergent has good volatility due to the existence of absolute ethyl alcohol, and the cleaning efficiency of the detergent is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cleaning agents, and in particular relates to an antibacterial cleaning agent for a glass cleaning machine and a preparation method thereof. Background Art

[0002] Glass cleaning machines are increasingly used in the glass industry. They are mainly used to clean various types of glass products, such as flat glass, glass tubes, glass instruments, glassware, optical glass, etc. Glass cleaning machines can effectively remove dirt and grease on the glass surface without causing any damage to the glass surface, avoiding surface wear and deformation that may be caused by mechanical cleaning methods. At the same time, they can also clean subtle corners that are difficult to reach. If the glass cleaning machine is not cleaned regularly, the dirt and grease on the glass surface will accumulate in the glass cleaning machine, leading to the growth of bacteria and microorganisms, increasing the risk of cross-contamination during the glass cleaning process, and affecting the cleaning effect and sanitary safety; glass cleaning machines that are not cleaned for a long time will produce odors, affecting the user experience and working environment, and will also cause problems such as blockage and scaling inside the glass cleaning machine, increasing the risk of equipment failure and affecting the normal operation and life of the equipment.

[0003] Patent CN 107012018 A discloses an antibacterial cleaning agent for toilets, which comprises the following components in parts by weight: 6 parts of sodium secondary alkyl sulfonate, 10 parts of oleamide, 15 parts of concentrated hydrochloric acid (37%), 5 parts of sodium xylene sulfonate, 2 parts of sodium sulfate, 5 parts of fatty alcohol polyoxyethylene ether, 6 parts of sodium fatty acid, and 5 parts of sodium tripolyphosphate. The prepared antibacterial cleaning agent is mainly used for cleaning surface dirt of toilet facilities, tiles, floors and other equipment, and has a good cleaning effect. However, the cleaning agent still has room for improvement in removing oil stains and inhibiting bacteria. Summary of the invention

[0004] The object of the present invention is to provide an antibacterial cleaning agent for a glass cleaning machine and a preparation method thereof, so as to solve the technical problem that the cleaning agent in the prior art has poor effects in removing oil stains and inhibiting bacteria.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides an antibacterial cleaning agent for a glass cleaning machine and a preparation method thereof, comprising the following steps:

[0007] Step (1) using zinc acetate dihydrate, citric acid and ethylene glycol as raw materials to prepare zinc oxide nanoparticles, and then modifying the zinc oxide nanoparticles with fluorosilicone to obtain modified zinc oxide nanoparticles;

[0008] Step (2) dispersing the modified zinc oxide nanoparticles and the degreasing agent in anhydrous ethanol to obtain an antibacterial cleaning agent.

[0009] In the above process, the modified zinc oxide nanoparticles and the degreasing agent are dispersed in anhydrous ethanol. Since the anhydrous ethanol molecules mainly interact with each other through the van der Waals force, the force is relatively weak, so the attraction between the molecules is relatively small; the anhydrous ethanol molecules contain hydrogen bond donors and acceptor groups, but since there are no water molecules in the anhydrous ethanol, a hydrogen bond network cannot be formed, which reduces the attraction between the molecules, making the interaction between the anhydrous ethanol molecules weaker and having high volatility, which makes the antibacterial cleaning agent also highly volatile. The highly volatile cleaning agent can remove stains and grease from the glass surface and improve the cleaning efficiency; the cleaning agent evaporates quickly and the required contact time is short, which helps to reduce contact wear during the cleaning process and protect the glass surface from damage. In addition, anhydrous ethanol also has a bactericidal effect, which can provide additional antibacterial protection and protect the hygiene of the glass surface.

[0010] Preferably, the method for preparing the modified zinc oxide nanoparticles comprises the following steps:

[0011] P1: Dissolve zinc acetate dihydrate and citric acid in deionized water, heat and stir in a water bath, then add ethylene glycol to the mixed solution, adjust the pH of the mixed solution with ammonia water, continue heating and stirring to obtain a precursor solution; dry the precursor solution in an oven to obtain a precursor gel, place the precursor gel in a tubular furnace, and sinter at high temperature to obtain zinc oxide nanoparticles;

[0012] In the above process, citric acid is used as a catalyst to promote the hydrolysis reaction of zinc acetate dihydrate. The reaction process is as follows:

[0013]

[0014] According to mass spectrometry analysis, the m / z of zinc acetate dihydrate is: 217.98 (100.0%), 219.97 (57.4%), 221.97 (38.6%), 220.97 (8.4%), 218.98 (4.7%), 220.98 (2.7%), 222.98 (1.9%), 219.98 (1.3%), 223.97 (1.3%) ), 221.98 (1.2%); m / z of citric acid: 192.03 (100.0%), 193.03 (6.8%), 194.03 (1.6%); m / z of zinc oxide: 79.92 (100.0%), 81.92 (57.4%), 83.92 (38.6%), 82.92 (8.4%), 85.92 (1.4%).

[0015] P2: Dissolve chloroplatinic acid in isopropanol, stir to dissolve, and allow to stand to obtain a Sperier catalyst. Then add tetrafluoropropyl allyl ether, toluene, and a Sperier catalyst into a three-necked flask, heat and stir, increase the temperature, dropwise add tetramethyltetrahydrocyclotetrasiloxane, and after the addition is complete, increase the temperature to react. After the temperature reaction is complete, stop heating, add activated carbon, stir, filter, and rotary evaporate to obtain fluorosilicone;

[0016] In the above process, the synthesis mechanism of fluorosilicone is as follows:

[0017]

[0018] According to mass spectrometry analysis, the m / z of fluorosilicone is: 928.22 (100.0%), 929.22 (51.5%), 930.22 (14.0%), 930.21 (13.4%), 931.22 (6.5%), 931.21 (2.0%), 932.22 (1.7%).

[0019] P3: Add the obtained zinc oxide nanoparticles to anhydrous ethanol, stir magnetically, and pour into a three-necked flask after ultrasonic dispersion. Then add fluorosilicone to the three-necked flask, heat and stir the mixed solution containing fluorosilicone in a water bath under condensation reflux conditions. After the reaction is completed, the mixed solution is centrifuged and washed, and the precipitate after centrifugation is vacuum dried to obtain modified zinc oxide nanoparticles.

[0020] In the above process, fluorosilicone reacts chemically with the surface of zinc oxide to form a fluorosilicone modified layer, which forms a hydrophilic modified layer on the surface of zinc oxide. This modified layer makes it difficult for bacteria to adhere to the surface of the particles, thereby inhibiting the growth and reproduction of bacteria. The fluorine functional group of the fluorosilicone modified layer gives it a lower surface energy and high hydrophilicity, making it easier for water molecules to expand on the surface, thereby achieving hydrophilic properties. Fluorosilicone modification can form a protective layer on the surface of zinc oxide nanoparticles, thereby increasing the hardness and wear resistance of the particles and reducing wear and friction between the particles. The modified layer adheres to the surface of zinc oxide nanoparticles, blocking the entry of oxygen and moisture, reducing the progress of oxidation reactions, and delaying the aging process of the particles, so that the cleaning agent has a lasting antibacterial effect.

[0021] Preferably, in step P1, the volume ratio of zinc acetate dihydrate to citric acid is 1:(0.8-1.2); the concentration of zinc acetate dihydrate is 0.05 mol / L, the concentration of citric acid is 0.075 mol / L, the water bath heating temperature is 60-70°C, the stirring time is 1-2h, the volume ratio of ethylene glycol to citric acid is 1:(2.8-3.4), the volume fraction of ethylene glycol is 96vt%, pH=7, the continued heating and stirring time is 0.3-0.8h, the drying temperature is 90-100°C, the drying time is 4-7h, the high temperature sintering temperature is 500-600°C, and the high temperature sintering time is 1-3h.

[0022] Preferably, in step P2, the dosage ratio of chloroplatinic acid to isopropanol is 1 g:(90-110) mL, the stirring temperature is 20-30° C., the standing time is 40-50 h, the three-necked flask contains a thermometer, a magnet, a reflux condenser with a CaCl2 drying tube at the upper end, and a constant pressure dropping funnel, the volume ratio of tetrafluoropropyl allyl ether to tetramethyltetrahydrocyclotetrasiloxane is 1:(0.2-0.3), the concentration of the Sperier catalyst is 6 ppm, the heating temperature is 40-50° C., the stirring time is 1-2 h, the heating temperature is 70-80° C., the temperature of the heating reaction is 80-85° C., the reaction time is 8-10 h, and the stirring time is 5-7 h.

[0023] Preferably, in step P3, the magnetic stirring time is 10-14 min, the ultrasonic dispersion time is 20-24 min, the mass ratio of zinc oxide nanoparticles to fluorosilicone is 1:(0.05-0.1), the water bath heating temperature is 50-80°C, the stirring time is 2-3h, the centrifugal washing is 3-5 times, the washing solvent is anhydrous ethanol, the vacuum drying temperature is 50-70°C, and the vacuum drying time is 12-20h.

[0024] Preferably, the method for preparing the degreasing agent comprises the following steps:

[0025] S1: molecular sieves, p-toluenesulfonic acid and mannitol were added to a three-necked flask, and then cyclohexanone was added, and the mixture was heated and stirred for reaction. After the reaction was completed, the mixture was cooled and triethylamine was added for neutralization;

[0026] S2: extracting the product with ethyl acetate, filtering under reduced pressure, washing with deionized water, drying with magnesium sulfate, filtering, rotary evaporation, and concentrating to obtain a crude product;

[0027] S3: Purify the crude product through a chromatographic column to obtain a degreasing agent.

[0028] In the above process, p-toluenesulfonic acid is used as a catalyst, mannitol and cyclohexanone are used as substrates, and the degreasing agent, cyclohexanone mannide, is prepared through a ketal reaction. The generated product can interact with oil molecules, destroy the aggregation structure of oils, and make them agglomerate into agglomerates to achieve the degreasing effect. The molecular structure of cyclohexanone mannide enables it to reduce the surface tension between oils and other substances, further promoting the dispersion and removal of oils. The synthesis process of the degreasing agent is as follows:

[0029]

[0030] According to mass spectrometry analysis, the m / z of the degreasing agent is: 342.20 (100.0%), 343.21 (20.0%), 344.21 (3.1%).

[0031] Preferably, the molecular sieve and cyclohexanone in S1 are used in a ratio of 1 g: (0.8-1.2) mL, the heating temperature is 50-60°C, the reaction time is 2-4 h, and the mixture is cooled to room temperature; in S3, during the column purification process, the eluent is a mixture of petroleum ether and ethyl acetate, and the ratio of petroleum ether to ethyl acetate is 2:1, and the eluent is rotary evaporated at 80-90°C.

[0032] The antibacterial cleaning agent for a glass cleaning machine is prepared by the method for preparing the antibacterial cleaning agent for a glass cleaning machine.

[0033] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0034] 1. In the present invention, modified zinc oxide nanoparticles are used as the main antibacterial substance. The zinc oxide nanoparticles are modified by using fluorosilicone so that the modified zinc oxide nanoparticles have hydrophilic, wear-resistant and anti-aging properties. At the same time, a degreasing agent prepared by ketal reaction of mannitol and cyclohexanone is added to anhydrous ethanol to obtain a cleaning agent with grease removal performance. Since the main solvent of the cleaning agent is anhydrous ethanol, it has good volatility and improves the cleaning efficiency.

[0035] 2. In the present invention, fluorosilicone is used to modify zinc oxide, so that a fluorosilicone modification layer is formed on the surface of zinc oxide. The modification layer makes it difficult for bacteria to adhere to the surface of the particles, thereby inhibiting the growth and reproduction of bacteria. The presence of the fluorine functional group makes the modified zinc oxide nanoparticles have low surface energy and high hydrophilicity, making it easier for water molecules to expand on the surface, thereby achieving hydrophilic properties. At the same time, fluorosilicone can also increase the hardness and wear resistance of the particles, reduce wear and friction between the particles, and the attachment of the modified layer can also reduce the oxidation reaction, delay the aging process of the particles, and make the antibacterial cleaning agent have excellent antibacterial durability.

[0036] 3. In the present invention, mannitol and cyclohexanone are used as raw materials, p-toluenesulfonic acid is used as a catalyst, and cyclohexanone mannide is generated through a ketal reaction. Cyclohexanone mannide can react with oil molecules to achieve a degreasing effect, and the molecular structure of cyclohexanone mannide enables it to reduce the surface tension between oil and other substances, thereby promoting the dispersion and removal of oil. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] This embodiment discloses a method for preparing modified zinc oxide nanoparticles, comprising the following steps:

[0040] P1: Dissolve 10 mL of 0.05 mol / L zinc acetate dihydrate and 10 mL of 0.075 mol / L citric acid in deionized water, heat and stir in a 60°C water bath for 2 h, then add 3.2 mL of 96 vt% ethylene glycol to the mixed solution, adjust the pH of the mixed solution to 7 with ammonia water, continue heating and stirring for 0.5 h, and obtain a precursor solution; place the precursor solution in a 90°C oven and dry for 6 h to obtain a precursor gel, place the precursor gel in a tubular furnace, and sinter at 550°C for 3 h to obtain zinc oxide nanoparticles;

[0041] P2: Take 1g of chloroplatinic acid and dissolve it in 100mL of isopropanol, stir and dissolve it at 25℃, and place it for 48h to obtain Sperier catalyst. Then, add 10mL of tetrafluoropropyl allyl ether, toluene, and Sperier catalyst with a concentration of 6ppm to a three-necked flask containing a thermometer, a magnet, a reflux condenser with a CaCl2 drying tube at the upper end, and a constant pressure dropping funnel. Heat to 50℃ and stir for 1h, then heat to 75℃, drop 2.5mL of tetramethyltetrahydrocyclotetrasiloxane, and after the addition is complete, heat to 80℃ and react for 10h. After the temperature reaction is completed, stop heating, add activated carbon, stir for 6h, filter, and rotary evaporate to obtain fluorosilicone;

[0042] P3: Add 10g of the obtained zinc oxide nanoparticles to anhydrous ethanol, stir magnetically for 12min, and ultrasonically disperse for 22min, then pour into a three-necked flask, then add 0.75g of fluorosilicone to the three-necked flask, heat the mixed solution containing fluorosilicone in a 60°C water bath and stir for 2h under condensation reflux conditions. After the reaction is completed, the mixed solution is centrifuged and washed 5 times with anhydrous ethanol as the washing solvent. The precipitate after centrifugation is vacuum dried at 60°C for 15h to obtain modified zinc oxide nanoparticles.

[0043] This embodiment discloses a method for preparing a degreasing agent, comprising the following steps:

[0044] S1: Add 1 g of molecular sieve, p-toluenesulfonic acid and mannitol into a three-necked flask, then add 1 mL of cyclohexanone, heat the mixture to 60 °C and stir for 3 h. After the reaction is completed, cool to room temperature and add triethylamine for neutralization;

[0045] S2: extracting the product with ethyl acetate, filtering under reduced pressure, washing with deionized water, drying with magnesium sulfate, filtering, rotary evaporation, and concentrating to obtain a crude product;

[0046] S3: The crude product is purified by a chromatographic column. During the purification process, the eluent is a mixture of petroleum ether and ethyl acetate, and the petroleum ether:ethyl acetate=2:1. The eluent is rotary evaporated at 80°C to obtain a degreasing agent.

[0047] This embodiment discloses a method for preparing an antibacterial cleaning agent for a glass cleaning machine, comprising the following steps:

[0048] Step (1) using zinc acetate dihydrate, citric acid and ethylene glycol as raw materials to prepare zinc oxide nanoparticles, and then modifying the zinc oxide nanoparticles with fluorosilicone to obtain modified zinc oxide nanoparticles;

[0049] Step (2) dispersing the modified zinc oxide nanoparticles and the degreasing agent in anhydrous ethanol to obtain an antibacterial cleaning agent.

[0050] Example 2

[0051] This embodiment discloses a method for preparing modified zinc oxide nanoparticles, comprising the following steps:

[0052] P1: Dissolve 10 mL of 0.05 mol / L zinc acetate dihydrate and 12 mL of 0.075 mol / L citric acid in deionized water, heat and stir in a 60°C water bath for 2 h, then add 4 mL of 96 vt% ethylene glycol to the mixed solution, adjust the pH of the mixed solution to 7 with ammonia water, continue heating and stirring for 0.5 h to obtain a precursor solution; place the precursor solution in a 90°C oven and dry for 6 h to obtain a precursor gel, place the precursor gel in a tubular furnace, and sinter at 550°C for 3 h to obtain zinc oxide nanoparticles;

[0053] P2: Take 1g of chloroplatinic acid and dissolve it in 110mL of isopropanol, stir and dissolve it at 25℃, and place it for 48h to obtain Sperier catalyst. Then, add 10mL of tetrafluoropropyl allyl ether, toluene, and Sperier catalyst with a concentration of 6ppm to a three-necked flask containing a thermometer, a magnet, a reflux condenser with a CaCl2 drying tube at the upper end, and a constant pressure dropping funnel. Heat to 50℃ and stir for 1h, then heat to 75℃, drop 3mL of tetramethyltetrahydrocyclotetrasiloxane, and after the addition is complete, heat to 80℃ and react for 10h. After the temperature reaction is completed, stop heating, add activated carbon, stir for 6h, filter, and rotary evaporate to obtain fluorosilicone;

[0054] P3: Add 10g of the obtained zinc oxide nanoparticles to anhydrous ethanol, stir magnetically for 12min, and ultrasonically disperse for 22min, then pour into a three-necked flask, then add 1g of fluorosilicone to the three-necked flask, heat the mixed solution containing fluorosilicone in a 60°C water bath and stir for 2h under condensation reflux conditions. After the reaction is completed, the mixed solution is centrifuged and washed 5 times with anhydrous ethanol as the washing solvent. The precipitate after centrifugation is vacuum dried at 60°C for 15h to obtain modified zinc oxide nanoparticles.

[0055] This embodiment discloses a method for preparing a degreasing agent, comprising the following steps:

[0056] S1: Add 1 g molecular sieve, p-toluenesulfonic acid and mannitol into a three-necked flask, then add 1.2 mL cyclohexanone, heat the mixture to 60 °C and stir for 3 h. After the reaction is completed, cool to room temperature and add triethylamine for neutralization;

[0057] S2: extracting the product with ethyl acetate, filtering under reduced pressure, washing with deionized water, drying with magnesium sulfate, filtering, rotary evaporation, and concentrating to obtain a crude product;

[0058] S3: The crude product is purified by a chromatographic column. During the purification process, the eluent is a mixture of petroleum ether and ethyl acetate, and the petroleum ether:ethyl acetate=2:1. The eluent is rotary evaporated at 80°C to obtain a degreasing agent.

[0059] This embodiment discloses a method for preparing an antibacterial cleaning agent for a glass cleaning machine, comprising the following steps:

[0060] Step (1) using zinc acetate dihydrate, citric acid and ethylene glycol as raw materials to prepare zinc oxide nanoparticles, and then modifying the zinc oxide nanoparticles with fluorosilicone to obtain modified zinc oxide nanoparticles;

[0061] Step (2) dispersing the modified zinc oxide nanoparticles and the degreasing agent in anhydrous ethanol to obtain an antibacterial cleaning agent.

[0062] Example 3

[0063] This embodiment discloses a method for preparing modified zinc oxide nanoparticles, comprising the following steps:

[0064] P1: Dissolve 10 mL of 0.05 mol / L zinc acetate dihydrate and 8 mL of 0.075 mol / L citric acid in deionized water, heat and stir in a 60°C water bath for 2 h, then add 2.7 mL of 96 vt% ethylene glycol to the mixed solution, adjust the pH of the mixed solution to 7 with ammonia water, continue heating and stirring for 0.5 h, and obtain a precursor solution; place the precursor solution in a 90°C oven and dry for 6 h to obtain a precursor gel, place the precursor gel in a tubular furnace, and sinter at 550°C for 3 h to obtain zinc oxide nanoparticles;

[0065] P2: Take 1g of chloroplatinic acid and dissolve it in 90mL of isopropanol, stir and dissolve it at 25℃, and place it for 48h to obtain Sperier catalyst. Then, add 10mL of tetrafluoropropyl allyl ether, toluene, and Sperier catalyst with a concentration of 6ppm to a three-necked flask containing a thermometer, a magnet, a reflux condenser with a CaCl2 drying tube at the upper end, and a constant pressure dropping funnel. Heat to 50℃ and stir for 1h, then heat to 75℃, drop 2mL of tetramethyltetrahydrocyclotetrasiloxane, and after the addition is complete, heat to 80℃ and react for 10h. After the temperature reaction is completed, stop heating, add activated carbon, stir for 6h, filter, and rotary evaporate to obtain fluorosilicone;

[0066] P3: Add 10g of the obtained zinc oxide nanoparticles to anhydrous ethanol, stir magnetically for 12min, and ultrasonically disperse for 22min, then pour into a three-necked flask, then add 0.5g of fluorosilicone to the three-necked flask, heat the mixed solution containing fluorosilicone in a water bath at 60°C and stir for 2h under condensation reflux conditions. After the reaction is completed, the mixed solution is centrifuged and washed 5 times with anhydrous ethanol as the washing solvent. The precipitate after centrifugation is vacuum dried at 60°C for 15h to obtain modified zinc oxide nanoparticles.

[0067] This embodiment discloses a method for preparing a degreasing agent, comprising the following steps:

[0068] S1: Add 1 g molecular sieve, p-toluenesulfonic acid and mannitol into a three-necked flask, then add 0.8 mL cyclohexanone, heat the mixture to 60 °C and stir for 3 h. After the reaction is completed, cool to room temperature and add triethylamine for neutralization;

[0069] S2: extracting the product with ethyl acetate, filtering under reduced pressure, washing with deionized water, drying with magnesium sulfate, filtering, rotary evaporation, and concentrating to obtain a crude product;

[0070] S3: The crude product is purified by a chromatographic column. During the purification process, the eluent is a mixture of petroleum ether and ethyl acetate, and the petroleum ether:ethyl acetate=2:1. The eluent is rotary evaporated at 80°C to obtain a degreasing agent.

[0071] This embodiment discloses a method for preparing an antibacterial cleaning agent for a glass cleaning machine, comprising the following steps:

[0072] Step (1) using zinc acetate dihydrate, citric acid and ethylene glycol as raw materials to prepare zinc oxide nanoparticles, and then modifying the zinc oxide nanoparticles with fluorosilicone to obtain modified zinc oxide nanoparticles;

[0073] Step (2) dispersing the modified zinc oxide nanoparticles and the degreasing agent in anhydrous ethanol to obtain an antibacterial cleaning agent.

[0074] Example 4

[0075] This embodiment discloses a method for preparing modified zinc oxide nanoparticles, comprising the following steps:

[0076] P1: Dissolve 10 mL of 0.05 mol / L zinc acetate dihydrate and 9 mL of 0.075 mol / L citric acid in deionized water, heat and stir in a 60°C water bath for 2 h, then add 3 mL of 96 vt% ethylene glycol to the mixed solution, adjust the pH of the mixed solution to 7 with ammonia water, continue heating and stirring for 0.5 h to obtain a precursor solution; place the precursor solution in a 90°C oven and dry for 6 h to obtain a precursor gel, place the precursor gel in a tubular furnace, and sinter at 550°C for 3 h to obtain zinc oxide nanoparticles;

[0077] P2: Take 1g of chloroplatinic acid and dissolve it in 96mL of isopropanol, stir and dissolve it at 25℃, and place it for 48h to obtain Sperier catalyst. Then, add 10mL of tetrafluoropropyl allyl ether, toluene, and Sperier catalyst with a concentration of 6ppm to a three-necked flask containing a thermometer, a magnet, a reflux condenser with a CaCl2 drying tube at the upper end, and a constant pressure dropping funnel. Heat to 50℃ and stir for 1h, then heat to 75℃, drop 2.8mL of tetramethyltetrahydrocyclotetrasiloxane, and after the addition is complete, heat to 80℃ and react for 10h. After the temperature reaction is completed, stop heating, add activated carbon, stir for 6h, filter, and rotary evaporate to obtain fluorosilicone;

[0078] P3: Add 10g of the obtained zinc oxide nanoparticles to anhydrous ethanol, stir magnetically for 12min, and ultrasonically disperse for 22min, then pour into a three-necked flask, then add 0.6g of fluorosilicone to the three-necked flask, heat the mixed solution containing fluorosilicone in a 60°C water bath and stir for 2h under condensation reflux conditions. After the reaction is completed, the mixed solution is centrifuged and washed 5 times with anhydrous ethanol as the washing solvent. The precipitate after centrifugation is vacuum dried at 60°C for 15h to obtain modified zinc oxide nanoparticles.

[0079] This embodiment discloses a method for preparing a degreasing agent, comprising the following steps:

[0080] S1: Add 1 g molecular sieve, p-toluenesulfonic acid and mannitol into a three-necked flask, then add 1.1 mL cyclohexanone, heat the mixture to 60 °C and stir for 3 h. After the reaction is completed, cool to room temperature and add triethylamine for neutralization;

[0081] S2: extracting the product with ethyl acetate, filtering under reduced pressure, washing with deionized water, drying with magnesium sulfate, filtering, rotary evaporation, and concentrating to obtain a crude product;

[0082] S3: The crude product is purified by a chromatographic column. During the purification process, the eluent is a mixture of petroleum ether and ethyl acetate, and the petroleum ether:ethyl acetate=2:1. The eluent is rotary evaporated at 80°C to obtain a degreasing agent.

[0083] This embodiment discloses a method for preparing an antibacterial cleaning agent for a glass cleaning machine, comprising the following steps:

[0084] Step (1) using zinc acetate dihydrate, citric acid and ethylene glycol as raw materials to prepare zinc oxide nanoparticles, and then modifying the zinc oxide nanoparticles with fluorosilicone to obtain modified zinc oxide nanoparticles;

[0085] Step (2) dispersing the modified zinc oxide nanoparticles and the degreasing agent in anhydrous ethanol to obtain an antibacterial cleaning agent.

[0086] Comparative Example 1

[0087] Comparative Example 1 Compared with Example 1, in the preparation process of zinc oxide nanoparticles in Comparative Example 1, no fluorosilicone was added for modification, and other conditions remained unchanged.

[0088] Comparative Example 2

[0089] Comparative Example 2 Compared with Example 1, no degreasing agent was added to the antibacterial cleaning agent in Comparative Example 2, and other conditions remained unchanged.

[0090] Experimental example

[0091] The antibacterial cleaning agents for glass cleaning machines prepared in Examples 1-4 and Comparative Examples 1-2 were tested for their antibacterial, hydrophilic, antibacterial durability and degreasing properties.

[0092] 1. Antibacterial performance test

[0093] According to GB / T 21510-2008, a certain amount of bacterial suspension was added to a conical flask, and then an antibacterial cleaning agent was added, a blank group was set, and the mixed solution was placed in a constant temperature shaker with an oscillation frequency of 150 rpm and a temperature of 37°C. After culturing for 1 hour, 1 mL of liquid was taken from the conical flask and dripped into a culture dish containing solid culture medium, and then cultured at 37°C for 48 hours before being taken out and the number of colonies on the plate was counted. The antibacterial rate was calculated according to the antibacterial rate = (the number of colonies in the blank group - the number of colonies in the antibacterial cleaning agent group) / the number of colonies in the blank group. The results are shown in the following table:

[0094] Table 1

[0095] Group Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Antibacterial rate% 98.98 96.67 96.41 95.39 88.35 86.63

[0096] From the test results in Table 1, it can be seen that the antibacterial cleaning agents for glass cleaning machines prepared in Examples 1-4 of the present invention have excellent antibacterial properties. From the comparison between Comparative Example 1 and Examples 1-4, it can be seen that the antibacterial properties of the antibacterial cleaning agents for glass cleaning machines can be improved by adding fluorosilicone for modification; from the comparison between Comparative Example 2 and Examples 1-4, it can be seen that the antibacterial properties of the antibacterial cleaning agents for glass cleaning machines can be improved by adding a degreasing agent.

[0097] 2. Hydrophilic performance test

[0098] The antibacterial cleaning agent was evenly coated on the glass surface, and then the contact angle of the droplet on the glass surface was measured using a contact angle meter (OCA50, Beijing Audlino Instrument Co., Ltd.). The test results are shown in the following table:

[0099] Table 2

[0100] Group Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Contact angle° 62.98 64.67 66.41 66.39 78.35 76.63

[0101] From the test results in Table 1, it can be seen that the antibacterial cleaning agent for glass cleaning machine prepared in Examples 1-4 of the present invention has excellent hydrophilic properties. From the comparison between Comparative Example 1 and Examples 1-4, it can be seen that the addition of fluorosilicone for modification can improve the hydrophilic properties of the antibacterial cleaning agent for glass cleaning machine; from the comparison between Comparative Example 2 and Examples 1-4, it can be seen that the addition of a degreasing agent can improve the hydrophilic properties of the antibacterial cleaning agent for glass cleaning machine.

[0102] 3. Antibacterial durability test

[0103] According to CB / T 16422.2-1999, after the antibacterial cleaning agent was placed under ultraviolet light for 500 hours, the antibacterial performance of the antibacterial cleaning agent was measured and the antibacterial performance retention rate was calculated. The results are shown in the following table:

[0104] Table 3

[0105] Group Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Antibacterial performance retention rate % 75.58 74.31 72.64 71.12 62.35 63.40

[0106] From the test results in Table 3, it can be seen that the antibacterial cleaning agents for glass cleaning machines prepared in Examples 1-4 of the present invention have excellent antibacterial durability. From the comparison between Comparative Example 1 and Examples 1-4, it can be seen that the antibacterial durability of the antibacterial cleaning agents for glass cleaning machines can be improved by adding fluorosilicone for modification; from the comparison between Comparative Example 2 and Examples 1-4, it can be seen that the antibacterial durability of the antibacterial cleaning agents for glass cleaning machines can be improved by adding a degreasing agent.

[0107] 4. Oil removal performance test

[0108] A certain weight of grease is placed in a conical flask, and an antibacterial cleaning agent is added to the conical flask. The conical flask is placed in a shaker at a speed of 180 rpm. After 2 hours, the remaining amount of grease is measured and the degreasing rate is calculated. The results are shown in the following table:

[0109] Table 4

[0110] Group Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Oil removal rate% 95.58 94.13 92.41 90.52 89.53 64.25

[0111] From the test results in Table 4, it can be seen that the antibacterial cleaning agents for glass cleaning machines prepared in Examples 1-4 of the present invention have excellent degreasing performance. From the comparison between Comparative Example 1 and Examples 1-4, it can be seen that the addition of fluorosilicone for modification can improve the degreasing performance of the antibacterial cleaning agent for glass cleaning machines; from the comparison between Comparative Example 2 and Examples 1-4, it can be seen that the addition of a degreasing agent can improve the degreasing performance of the antibacterial cleaning agent for glass cleaning machines.

[0112] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

[0113] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing an antibacterial cleaning agent for a glass cleaning machine, characterized in that: The following steps are involved: Step (1) using zinc acetate dihydrate, citric acid and ethylene glycol as raw materials to prepare zinc oxide nanoparticles, and then modifying the zinc oxide nanoparticles with fluorosilicone to obtain modified zinc oxide nanoparticles; Step (2) dispersing the modified zinc oxide nanoparticles and the degreasing agent in anhydrous ethanol to obtain an antibacterial cleaning agent.

2. The method for preparing the antibacterial cleaning agent for glass cleaning machine according to claim 1, characterized in that: The preparation method of the modified zinc oxide nanoparticles comprises the following steps: P1: Dissolve zinc acetate dihydrate and citric acid in deionized water, heat and stir in a water bath, then add ethylene glycol to the mixed solution, adjust the pH of the mixed solution with ammonia water, continue heating and stirring to obtain a precursor solution; dry the precursor solution in an oven to obtain a precursor gel, place the precursor gel in a tubular furnace, and sinter at high temperature to obtain zinc oxide nanoparticles; P2: Dissolve chloroplatinic acid in isopropanol, stir to dissolve, and allow to stand to obtain a Sperier catalyst. Then add tetrafluoropropyl allyl ether, toluene, and a Sperier catalyst into a three-necked flask, heat and stir, increase the temperature, dropwise add tetramethyltetrahydrocyclotetrasiloxane, and after the addition is complete, increase the temperature to react. After the temperature reaction is complete, stop heating, add activated carbon, stir, filter, and rotary evaporate to obtain fluorosilicone; P3: Add the obtained zinc oxide nanoparticles to anhydrous ethanol, stir magnetically, and pour into a three-necked flask after ultrasonic dispersion. Then add fluorosilicone to the three-necked flask, heat and stir the mixed solution containing fluorosilicone in a water bath under condensation reflux conditions. After the reaction is completed, the mixed solution is centrifuged and washed, and the precipitate after centrifugation is vacuum dried to obtain modified zinc oxide nanoparticles.

3. The method for preparing the antibacterial cleaning agent for glass cleaning machine according to claim 2, characterized in that: In the step P1, the volume ratio of zinc acetate dihydrate to citric acid is 1:(0.8-1.2); the concentration of zinc acetate dihydrate is 0.05 mol / L, the concentration of citric acid is 0.075 mol / L, the water bath heating temperature is 60-70°C, the stirring time is 1-2h, the volume ratio of ethylene glycol to citric acid is 1:(2.8-3.4), the volume fraction of ethylene glycol is 96vt%, pH=7, the heating and stirring time is continued for 0.3-0.8h, the drying temperature is 90-100°C, the drying time is 4-7h, the high-temperature sintering temperature is 500-600°C, and the high-temperature sintering time is 1-3h.

4. The method for preparing the antibacterial cleaning agent for glass cleaning machine according to claim 2, characterized in that: In the step P2, the dosage ratio of chloroplatinic acid to isopropanol is 1 g: (90-110) mL, the stirring temperature is 20-30° C., the standing time is 40-50 h, the three-necked flask contains a thermometer, a magnet, a reflux condenser with a CaCl2 drying tube at the upper end, and a constant pressure dropping funnel, the volume ratio of tetrafluoropropyl allyl ether to tetramethyltetrahydrocyclotetrasiloxane is 1: (0.2-0.3), the concentration of the Sperier catalyst is 6 ppm, the heating temperature is 40-50° C., the stirring time is 1-2 h, the heating temperature is 70-80° C., the temperature of the heating reaction is 80-85° C., the reaction time is 8-10 h, and the stirring time is 5-7 h.

5. The method for preparing the antibacterial cleaning agent for glass cleaning machine according to claim 2, characterized in that: In the step P3, the magnetic stirring time is 10-14 minutes, the ultrasonic dispersion time is 20-24 minutes, the mass ratio of zinc oxide nanoparticles to fluorosilicone is 1:(0.05-0.1), the water bath heating temperature is 50-80°C, the stirring time is 2-3 hours, the centrifugal washing is 3-5 times, the washing solvent is anhydrous ethanol, the vacuum drying temperature is 50-70°C, and the vacuum drying time is 12-20 hours.

6. The method for preparing the antibacterial cleaning agent for glass cleaning machine according to claim 1, characterized in that: The preparation method of the degreasing agent comprises the following steps: S1: molecular sieves, p-toluenesulfonic acid and mannitol were added to a three-necked flask, and then cyclohexanone was added, and the mixture was heated and stirred for reaction. After the reaction was completed, the mixture was cooled and triethylamine was added for neutralization; S2: extracting the product with ethyl acetate, filtering under reduced pressure, washing with deionized water, drying with magnesium sulfate, filtering, rotary evaporation, and concentrating to obtain a crude product; S3: Purify the crude product through a chromatographic column to obtain a degreasing agent.

7. The method for preparing the antibacterial cleaning agent for glass cleaning machine according to claim 6, characterized in that: The molecular sieve and cyclohexanone in S1 have a dosage ratio of 1 g: (0.8-1.2) mL, a heating temperature of 50-60° C., a reaction time of 2-4 h, and are cooled to room temperature; in S3, during the chromatographic column purification process, the eluent is a mixture of petroleum ether and ethyl acetate, and the ratio of petroleum ether to ethyl acetate is 2:1, and the eluent is rotary evaporated at 80-90° C.

8. An antibacterial cleaning agent for a glass cleaning machine prepared by the method according to any one of claims 1 to 7.

Citation Information

Cited By

  • Polyethylene clean film, packaging bag and preparation method of polyethylene clean film

    CN119661923A

  • Resistor disc for lightning arrester and preparation method of resistor disc

    CN121331579A