Method for solving ceramic tile glaze rod marks
By designing the raw material formula for base glaze and surface glaze, it is close to the initial melting point of the blank, and adding high-inflation blocks during the firing process, the problem of tiles roller rod printing is solved, and the hardness and wear resistance of the finished product are improved. An efficient production process is achieved.
Patent Information
- Application Number
- CN202411005251.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-25
AI Technical Summary
During the firing process, ceramic tiles are prone to roll rod printing defects, resulting in poor hardness, wear resistance and stain resistance of the finished product.
By designing the raw material formula for base glaze and surface glaze, the initial melting point is close to the initial melting point of the blank, and high-inflated fuses are added to the glaze, combined with sodium tripolyphosphate and methyl cellulose, and then ball milled and sieved. , after applying the base glaze and surface glaze slurry, inkjet design and spraying process, and finally fire in a kiln.
It effectively prevents the occurrence of roller rod printing defects, so that the finished tiles have high hardness, wear resistance and easy cleaning, and the production process is simple and easy to mass production.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic tiles, and in particular relates to a method for solving the problem of ceramic tile glaze stick marks. Background Art
[0002] The production process of ceramic tiles requires multiple steps, including the molding of the body, the preparation of glazes, the application of glazes, and high-temperature firing. In this process, the performance of the body and glaze and the matching between them have a crucial impact on the quality of the final product. Especially during the high-temperature firing process, the matching degree of the thermal expansion coefficient and melting point of the glaze and the body will directly affect the molding quality of the ceramic tile. In addition, as the output of ceramic glazed tiles continues to increase, the water absorption rate is getting lower and lower, and the "roller mark" is produced. The poor visual effect of the roller mark will seriously affect the appearance and quality of the finished ceramic tile. Under the premise that the hardness, wear resistance and stain resistance of the currently available ceramic glazed tiles are already poor, if the ceramic tile still produces roller mark defects during the firing process, the quality of the finished ceramic tile will be quite worrying. Therefore, providing a method to solve the above problems has excellent practical application value. Summary of the invention
[0003] The purpose of the present invention is to provide a method for solving the problem of roller marks on ceramic tile glaze, which solves the problems in the prior art that ceramic tiles still produce roller marks during the firing process and the hardness and wear resistance of the finished ceramic tiles are poor.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A method for solving the problem of tile glaze stick marks, comprising the following steps:
[0006] S1, making a green body to obtain a body A;
[0007] S2, weighing the raw materials of the base glaze and the top glaze respectively and mixing and stirring them evenly to obtain a pre-treated base glaze material and a pre-treated top glaze material;
[0008] S3, adding water, sodium tripolyphosphate and methylcellulose to the pretreated bottom glaze material and the pretreated top glaze material, respectively, ball milling, sieving, and removing iron to obtain bottom glaze slurry and top glaze slurry;
[0009] S4, applying the base glaze slurry to the surface of the body A to obtain the body B, subjecting the body B to color design by an inkjet machine and spraying matte ink on the surface of the body B to obtain the body C;
[0010] S5, applying the glaze slurry to the surface of the body C to obtain the body D;
[0011] S6. After the body D is dried on the glaze line, it is directly fired in the kiln to obtain the finished tile.
[0012] As a preferred technical solution of the present invention, the initial melting point of the blank A in step S1 is 1100-1110° C., and the expansion coefficient is 200-210.
[0013] As a preferred technical solution of the present invention, the raw materials of the base glaze in step S2 are calculated by weight and are specifically as follows: 15-25 parts by weight of nepheline, 20-35 parts by weight of albite, 5-10 parts by weight of kaolin, 2-5 parts by weight of ball clay, 3-10 parts by weight of calcined alumina, 5-8 parts by weight of quartz, 15-25 parts by weight of potassium feldspar, 10-20 parts by weight of high expansion frit, 2-2.2 parts by weight of zinc oxide and 2-5 parts by weight of dolomite.
[0014] As a preferred technical solution of the present invention, the raw materials of the glaze described in step S2 are calculated by weight and are specifically as follows: 20-25 parts by weight of albite, 20-25 parts by weight of potassium feldspar, 10-15 parts by weight of kaolin, 6-8 parts by weight of zinc oxide, 10-20 parts by weight of dolomite, 15-20 parts by weight of high expansion frit, 10-15 parts by weight of wollastonite, 5-10 parts by weight of strontium carbonate, and 3-5 parts by weight of barium carbonate.
[0015] Furthermore, the high expansion frit described in the base glaze and the top glaze of step S2 includes the following components by weight: 63.6 parts by weight of silicon dioxide, 9.01 parts by weight of aluminum oxide, 3.85 parts by weight of calcium oxide, 5.57 parts by weight of magnesium oxide, 3.18 parts by weight of potassium oxide, 12.08 parts by weight of sodium oxide, and 8.37 parts by weight of barium oxide.
[0016] As a preferred technical solution of the present invention, the mass ratios of the pretreated surface glaze, water, sodium tripolyphosphate and methyl cellulose and the pretreated bottom glaze, water, sodium tripolyphosphate and methyl cellulose in step S3 are all 1:0.3-0.5:0.0014-0.0015:0.0030-0.0035.
[0017] As a preferred technical solution of the present invention, the ball milling time in step S3 is 7-9 hours.
[0018] As a preferred technical solution of the present invention, the method of applying the base glaze slurry to the surface of the body A in step S4 is glazing.
[0019] Furthermore, in the glazing process: the specific gravity of the bottom glaze slurry is 1.82-1.88 g / mL, and the amount of glaze in the bottom glaze slurry is 80 g (300 mm*600 mm plate).
[0020] As a preferred technical solution of the present invention, the method of applying the glaze slurry to the surface of the body C in step S5 is glaze spraying.
[0021] Furthermore, in the glaze spraying process: the specific gravity of the surface glaze slurry is 1.82-1.85 g / mL, and the amount of glaze sprayed on the surface glaze slurry is 80-85 g (300 mm*600 mm plate).
[0022] As a preferred technical solution of the present invention, the kiln firing temperature in step S6 is 1150-1200° C. and the firing time is 40-45 minutes.
[0023] Beneficial effects of the present invention:
[0024] (1) The present invention selects a design scheme in which the initial melting points of the base glaze, the surface glaze and the body A are close, and uses this as the design concept to carry out a rigorous formula design for the raw materials of the base glaze and the surface glaze. Under the overall composition formula of the present invention, the initial melting points of the base glaze and the surface glaze are close to the initial melting point of the body A, and the shrinkage points of the body and the glaze are close, which effectively prevents the brick shape from being too concave or too convex in the oxidation zone of the kiln, and further avoids the brick shape that is too concave or too convex from entering the high temperature zone. After the brick is softened, the corners of the brick droop under the action of the gravity of the brick and the roller, thereby forming a wavy shape or a roller mark, which is of great help in improving the roller mark of the finished tile product, so that the body will not produce roller mark defects during the firing process.
[0025] (2) The composition formula of the glaze raw materials of the present invention has been rigorously designed and adjusted. The finished ceramic tile produced under the glaze formula has the advantages of high hardness, transparency, wear resistance and easy cleaning.
[0026] (3) The present invention adds high expansion frit to the constituent raw materials of the base glaze and the top glaze, and through the reasonable combination of the high expansion frit and the remaining raw materials in the base glaze and the top glaze, the high expansion frit is used to enhance the overall transparency and hardness of the base glaze and the top glaze, and the wear resistance of the finished tile is further improved.
[0027] (4) The equipment used in the production process of the present invention is simple, and the product preparation method is simple and easy to mass produce, which has excellent practical significance. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] A method for solving the problem of tile glaze stick marks, comprising the following steps:
[0031] S1, preparing a green body to obtain a body A having an initial melting point of 1100° C. and an expansion coefficient of 205;
[0032] S2, weighing the raw materials of the base glaze and the top glaze respectively and mixing and stirring them evenly to obtain a pre-treated base glaze material and a pre-treated top glaze material;
[0033] The raw materials of the base glaze are calculated by weight as follows: 15 parts by weight of nepheline, 35 parts by weight of albite, 7.5 parts by weight of kaolin, 2 parts by weight of ball clay, 10 parts by weight of calcined alumina, 5 parts by weight of quartz, 15 parts by weight of potassium feldspar, 20 parts by weight of high expansion frit, 2.1 parts by weight of zinc oxide and 5 parts by weight of dolomite;
[0034] The raw materials of the glaze are calculated by weight as follows: 25 parts by weight of albite, 20 parts by weight of potassium feldspar, 12.5 parts by weight of kaolin, 8 parts by weight of zinc oxide, 10 parts by weight of dolomite, 20 parts by weight of high expansion frit, 10 parts by weight of wollastonite, 5 parts by weight of strontium carbonate, and 3 parts by weight of barium carbonate;
[0035] The high expansion frit described in the above-mentioned base glaze and top glaze includes the following components by weight: 63.6 parts by weight of silicon dioxide, 9.01 parts by weight of aluminum oxide, 3.85 parts by weight of calcium oxide, 5.57 parts by weight of magnesium oxide, 3.18 parts by weight of potassium oxide, 12.08 parts by weight of sodium oxide, and 8.37 parts by weight of barium oxide.
[0036] S3, adding water, sodium tripolyphosphate and methyl cellulose to the pretreated bottom glaze and the pretreated top glaze, respectively, and ball-milling for 7 hours, sieving, and removing iron to obtain bottom glaze slurry and top glaze slurry;
[0037] The mass ratio of the pre-treated glaze, water, sodium tripolyphosphate and methyl cellulose is 1:0.4:0.0015:0.0033;
[0038] The mass ratio of the pre-treated base glaze, water, sodium tripolyphosphate and methyl cellulose is 1:0.3:0.0014:0.0030;
[0039] S4, applying the base glaze slurry to the surface of the body A to obtain the body B, subjecting the body B to color design by an inkjet machine and spraying matte ink on the surface of the body B to obtain the body C;
[0040] The method of applying the bottom glaze slurry to the surface of the body A is glazing. In the glazing process: the specific gravity of the bottom glaze slurry is 1.88g / mL, and the amount of the bottom glaze slurry is 80g (300mm*600mm plate);
[0041] S5, applying the glaze slurry to the surface of the body C to obtain the body D;
[0042] The method of applying the glaze slurry to the surface of the body C is glaze spraying. In the glaze spraying process: the specific gravity of the glaze slurry is 1.82g / mL, and the amount of the glaze slurry sprayed is 80g (300mm*600mm plate);
[0043] S6. After the body D is dried on the glaze line, it is directly put into the kiln and fired at 1150°C for 40 minutes to obtain the finished tile.
[0044] The initial melting points of the base glaze and the top glaze of this embodiment were detected using a gradient furnace (30-1300° C.) of the German Nabertherm brand. The initial melting point of the base glaze of this embodiment was 1100° C., and the expansion coefficient was 210; the initial melting point of the top glaze of this embodiment was 1115° C., and the expansion coefficient was 260;
[0045] The green body of this embodiment has no roller mark defect during the firing process.
[0046] Example 2
[0047] A method for solving the problem of tile glaze stick marks, comprising the following steps:
[0048] S1, preparing a green body to obtain a body A having an initial melting point of 1110° C. and an expansion coefficient of 200;
[0049] S2, weighing the raw materials of the base glaze and the top glaze respectively and mixing and stirring them evenly to obtain a pre-treated base glaze material and a pre-treated top glaze material;
[0050] The raw materials of the base glaze are calculated by weight as follows: 20 parts by weight of nepheline, 20 parts by weight of albite, 10 parts by weight of kaolin, 5 parts by weight of ball clay, 3 parts by weight of calcined alumina, 8 parts by weight of quartz, 20 parts by weight of potassium feldspar, 15 parts by weight of high expansion frit, 2 parts by weight of zinc oxide and 2 parts by weight of dolomite;
[0051] The raw materials of the glaze are calculated by weight as follows: 22.5 parts by weight of albite, 23 parts by weight of potassium feldspar, 10 parts by weight of kaolin, 7 parts by weight of zinc oxide, 15 parts by weight of dolomite, 15 parts by weight of high expansion frit, 12.5 parts by weight of wollastonite, 10 parts by weight of strontium carbonate, and 5 parts by weight of barium carbonate;
[0052] The high expansion frit described in the above-mentioned base glaze and top glaze includes the following components by weight: 63.6 parts by weight of silicon dioxide, 9.01 parts by weight of aluminum oxide, 3.85 parts by weight of calcium oxide, 5.57 parts by weight of magnesium oxide, 3.18 parts by weight of potassium oxide, 12.08 parts by weight of sodium oxide, and 8.37 parts by weight of barium oxide.
[0053] S3, adding water, sodium tripolyphosphate and methyl cellulose to the pretreated bottom glaze and the pretreated top glaze, respectively, and ball-milling for 8 hours, sieving, and removing iron to obtain bottom glaze slurry and top glaze slurry;
[0054] The mass ratio of the pre-treated glaze, water, sodium tripolyphosphate and methyl cellulose is 1:0.3:0.0015:0.0035;
[0055] The mass ratio of the pre-treated base glaze, water, sodium tripolyphosphate and methyl cellulose is 1:0.5:0.0014:0.0033;
[0056] S4, applying the base glaze slurry to the surface of the body A to obtain the body B, subjecting the body B to color design by an inkjet machine and spraying matte ink on the surface of the body B to obtain the body C;
[0057] The method of applying the bottom glaze slurry to the surface of the body A is glazing. In the glazing process: the specific gravity of the bottom glaze slurry is 1.82g / mL, and the amount of the bottom glaze slurry is 80g (300mm*600mm plate);
[0058] S5, applying the glaze slurry to the surface of the body C to obtain the body D;
[0059] The method of applying the glaze slurry to the surface of the body C is glaze spraying. In the glaze spraying process: the specific gravity of the glaze slurry is 1.85g / mL, and the amount of the glaze slurry sprayed is 82.5g (300mm*600mm plate);
[0060] S6. After the body D is dried on the glaze line, it is directly put into the kiln and fired at 1150°C for 42 minutes to obtain the finished tile.
[0061] The initial melting points of the base glaze and the top glaze of this embodiment were detected using a gradient furnace (30-1300°C) of the German Nabertherm brand. The initial melting point of the base glaze of this embodiment was 1105°C, and the expansion coefficient was 260; the initial melting point of the top glaze of this embodiment was 1115°C, and the expansion coefficient was 270.
[0062] The green body of this embodiment has no roller mark defect during the firing process.
[0063] Example 3
[0064] A method for solving the problem of tile glaze stick marks, comprising the following steps:
[0065] S1, making a green body to obtain a body A with an initial melting point of 1105°C and an expansion coefficient of 210;
[0066] S2, weighing the raw materials of the base glaze and the top glaze respectively and mixing and stirring them evenly to obtain a pre-treated base glaze material and a pre-treated top glaze material;
[0067] The raw materials of the base glaze are calculated by weight as follows: 25 parts by weight of nepheline, 27.5 parts by weight of albite, 5 parts by weight of kaolin, 3.5 parts by weight of ball clay, 6.5 parts by weight of calcined alumina, 6.5 parts by weight of quartz, 25 parts by weight of potassium feldspar, 10 parts by weight of high expansion frit, 2.2 parts by weight of zinc oxide and 3.5 parts by weight of dolomite;
[0068] The raw materials of the glaze are calculated by weight as follows: 20 parts by weight of albite, 25 parts by weight of potassium feldspar, 15 parts by weight of kaolin, 6 parts by weight of zinc oxide, 20 parts by weight of dolomite, 17.5 parts by weight of high expansion frit, 15 parts by weight of wollastonite, 7.5 parts by weight of strontium carbonate, and 4 parts by weight of barium carbonate;
[0069] The high expansion frit described in the above-mentioned base glaze and top glaze includes the following components by weight: 63.6 parts by weight of silicon dioxide, 9.01 parts by weight of aluminum oxide, 3.85 parts by weight of calcium oxide, 5.57 parts by weight of magnesium oxide, 3.18 parts by weight of potassium oxide, 12.08 parts by weight of sodium oxide, and 8.37 parts by weight of barium oxide.
[0070] S3, adding water, sodium tripolyphosphate and methyl cellulose to the pretreated bottom glaze and the pretreated top glaze, respectively, and ball-milling for 9 hours, sieving, and removing iron to obtain bottom glaze slurry and top glaze slurry;
[0071] The mass ratio of the pre-treated glaze, water, sodium tripolyphosphate and methyl cellulose is 1:0.5:0.0014:0.0030;
[0072] The mass ratio of the pre-treated base glaze, water, sodium tripolyphosphate and methyl cellulose is 1:0.4:0.0015:0.0035;
[0073] S4, applying the base glaze slurry to the surface of the body A to obtain the body B, subjecting the body B to color design by an inkjet machine and spraying matte ink on the surface of the body B to obtain the body C;
[0074] The method of applying the bottom glaze slurry to the surface of the body A is glazing. In the glazing process: the specific gravity of the bottom glaze slurry is 1.85g / mL, and the amount of the bottom glaze slurry is 80g (300mm*600mm plate);
[0075] S5, applying the glaze slurry to the surface of the body C to obtain the body D;
[0076] The method of applying the glaze slurry to the surface of the body C is glaze spraying. In the glaze spraying process: the specific gravity of the glaze slurry is 1.83g / mL, and the amount of the glaze slurry sprayed is 85g (300mm*600mm plate);
[0077] S6. After the body D is dried on the glaze line, it is directly put into the kiln and fired at 1175℃ for 45 minutes to obtain the finished tile.
[0078] The initial melting points of the base glaze and the top glaze of this embodiment were detected using a gradient furnace (30-1300°C) of the German Nabertherm brand. The initial melting point of the base glaze of this embodiment was 1110°C, and the expansion coefficient was 200; the initial melting point of the top glaze of this embodiment was 1120°C, and the expansion coefficient was 270.
[0079] The green body of this embodiment has no roller mark defect during the firing process.
[0080] Comparative Example 1
[0081] Compared with Example 2, the difference is that no high expansion frit is added to the raw materials of the base glaze described in Comparative Example 1, and the remaining operating steps and parameters are the same.
[0082] Comparative Example 2
[0083] Compared with Example 2, the difference is that no high expansion frit is added to the raw materials of the glaze described in Comparative Example 2, and the remaining operating steps and parameters are the same.
[0084] Comparative Example 3
[0085] Compared with Example 2, the difference is that in Comparative Example 3, step S5 is not performed, that is, the glaze slurry is not applied, and the remaining operating steps and parameters are the same.
[0086] Comparative Example 4
[0087] Compared with Example 2, the difference is that in Comparative Example 4, step S4 is not performed, that is, the base glaze slurry is not applied, and the remaining operating steps and parameters are the same.
[0088] Comparative Example 5
[0089] Compared with Example 2, the difference is that the blank A with an initial melting point of 1000° C. and an expansion coefficient of 200 is obtained in step S1 of Comparative Example 5, and the remaining operating steps and parameters are the same.
[0090] The comparative example green body produced roller mark defects during the firing process.
[0091] Comparative Example 6
[0092] Compared with Example 2, the difference is that the blank A with an initial melting point of 1200° C. and an expansion coefficient of 200 is obtained in step S1 of Comparative Example 6, and the remaining operating steps and parameters are the same.
[0093] The comparative example green body produced roller mark defects during the firing process.
[0094] Performance Testing
[0095] (1) Mohs hardness grade: The finished ceramic tiles prepared in Examples 1-3 and Comparative Examples 1-4 were placed steadily on a hard support with the glaze facing upward. Standard minerals with different Mohs values from small to large were selected to scratch the ceramic tile surfaces in sequence. The ceramic tile surfaces were scratched evenly and vertically with the mineral cutting edge. The lowest hardness value that could just produce obvious scratches was taken as the test result. The results are shown in Table 1.
[0096] (2) Abrasion resistance: According to GB / T3810.7-2016, the finished ceramic tiles prepared in Examples 1-3 and Comparative Examples 1-4 were tested for abrasion resistance. The results are shown in Table 1.
[0097] (3) Antifouling grade: According to GB / T 3810.14-2016, the antifouling grade of the finished ceramic tiles prepared in Examples 1-3 and Comparative Examples 1-4 was tested. The results are shown in Table 1.
[0098] Table 1
[0099] Mohs hardness grade (grade) Abrasion resistance Antifouling grade (level) Example 1 6 Level 4 6000 rpm 5 Example 2 6 Level 4 6000 rpm 5 Example 3 6 Level 4 6000 rpm 5 Comparative Example 1 4 Level 4 2100 rpm 4 Comparative Example 2 3 Level 3 1500 rpm 4 Comparative Example 3 3 Level 3 750 rpm 3 Comparative Example 4 3 Level 3 750 rpm 3
[0100] It can be seen from Table 1 that the finished ceramic tile produced under the formula of the present invention has the advantages of high hardness, good wear resistance and good antifouling degree. It can be seen from Examples 1-3 and Comparative Examples 5-6 that the present invention selects a design scheme in which the initial melting points of the base glaze, the top glaze and the body A are close to each other, which is of great help in improving the roller mark of the finished product, so that the body will not produce roller mark defects during the firing process.
[0101] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0102] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method to solve the problem of tile glaze stick marks. It is characterized in that The specific steps include: S1, making a green body to obtain a body A; S2, weighing the raw materials of the base glaze and the top glaze respectively and mixing and stirring them evenly to obtain a pre-treated base glaze material and a pre-treated top glaze material; S3, adding water, sodium tripolyphosphate and methylcellulose to the pretreated bottom glaze material and the pretreated top glaze material, respectively, ball milling, sieving, and removing iron to obtain bottom glaze slurry and top glaze slurry; S4, applying the base glaze slurry to the surface of the body A to obtain the body B, subjecting the body B to color design by an inkjet machine and spraying matte ink on the surface of the body B to obtain the body C; S5, applying the glaze slurry to the surface of the body C to obtain the body D; S6. After the body D is dried on the glaze line, it is directly fired in the kiln to obtain the finished tile.
2. The method for solving the problem of tile glaze stick marks according to claim 1, It is characterized in that The initial melting point of the blank A in step S1 is 1100-1110° C., and the expansion coefficient is 200-210.
3. The method for solving the problem of tile glaze stick marks according to claim 1, It is characterized in that The raw materials of the base glaze in step S2 are calculated by weight and are as follows: 15-25 parts by weight of nepheline, 20-35 parts by weight of albite, 5-10 parts by weight of kaolin, 2-5 parts by weight of ball clay, 3-10 parts by weight of calcined alumina, 5-8 parts by weight of quartz, 15-25 parts by weight of potassium feldspar, 10-20 parts by weight of high expansion frit, 2-2.2 parts by weight of zinc oxide and 2-5 parts by weight of dolomite.
4. The method for solving the problem of tile glaze stick marks according to claim 3, It is characterized in that The raw materials of the glaze described in step S2 are calculated by weight and are specifically as follows: 20-25 parts by weight of albite, 20-25 parts by weight of potassium feldspar, 10-15 parts by weight of kaolin, 6-8 parts by weight of zinc oxide, 10-20 parts by weight of dolomite, 15-20 parts by weight of high expansion frit, 10-15 parts by weight of wollastonite, 5-10 parts by weight of strontium carbonate, and 3-5 parts by weight of barium carbonate.
5. The method for solving the problem of tile glaze stick marks according to claim 4, It is characterized in that The high expansion frit described in the base glaze and the top glaze of step S2 includes the following components by weight: 63.6 parts by weight of silicon dioxide, 9.01 parts by weight of aluminum oxide, 3.85 parts by weight of calcium oxide, 5.57 parts by weight of magnesium oxide, 3.18 parts by weight of potassium oxide, 12.08 parts by weight of sodium oxide, and 8.37 parts by weight of barium oxide.
6. The method for solving the problem of tile glaze stick marks according to claim 1, It is characterized in that In step S3, the mass ratios of the pretreated surface glaze, water, sodium tripolyphosphate and methyl cellulose and the pretreated bottom glaze, water, sodium tripolyphosphate and methyl cellulose are all 1:0.3-0.5:0.0014-0.0015:0.0030-0.0035.
7. The method for solving the problem of tile glaze stick marks according to claim 1, It is characterized in that The ball milling time in step S3 is 7-9 hours.
8. The method for solving the problem of tile glaze stick marks according to claim 1, It is characterized in that In step S4, the method of applying the bottom glaze slurry to the surface of the body A is glazing; in the glazing process: the specific gravity of the bottom glaze slurry is 1.82-1.88g / mL, and the amount of the bottom glaze slurry is 80g (300mm*600mm plate).
9. The method for solving the problem of tile glaze stick marks according to claim 1, It is characterized in that In step S5, the glaze slurry is applied to the surface of the body C by spraying glaze; in the spraying glaze process: the specific gravity of the glaze slurry is 1.82-1.85g / mL, and the amount of the sprayed glaze slurry is 80-85g (300mm*600mm plate).
10. The method for solving the problem of tile glaze stick marks according to claim 1, It is characterized in that The kiln firing temperature in step S6 is 1150-1200° C. and the firing time is 40-45 minutes.
Citation Information
Patent Citations
Crystallization frit, jade light-transmitting brick and preparation method of jade light-transmitting brick
CN112408795A
Bright and sub integrated ceramic rock plate and preparation method thereof
CN117303944A