Preparation method of high-curvature nano array electrode for producing oxygen through electro-catalytic decomposition of water
By fabricating high-curvature nanoarray electrodes on conductive substrates through electrochemical deposition, the dependence of oxygen evolution reaction on noble metal catalysts is eliminated, achieving low-cost and high-efficiency water electrolysis oxygen production performance, which is suitable for large-scale applications.
Patent Information
- Application Number
- CN202411008212.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
In existing water electrolysis technologies, the oxygen evolution reaction requires precious metal catalysts, which are expensive and scarce. Non-precious metal catalysts have insufficient activity and are difficult to apply on a large scale.
A simple electrochemical deposition method was used to electrodeposit nickel metal salt, doped metal salt, sodium citrate, boric acid and ammonium chloride solution on a conductive substrate to form a high curvature nanoarray electrode. Combined with constant current, constant potential and pulse electrodeposition methods, a non-noble metal catalyst with high activity and stability was prepared.
The prepared high-curvature nanoarray electrode exhibits excellent catalytic activity and stability, with an overpotential lower than that of commercial noble metal catalysts. It is also low in cost and abundant in reserves, making it suitable for large-scale production.
Smart Images

Figure CN118932396A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrocatalytic water decomposition, and specifically relates to a method for preparing an electrode with a high-curvature nanoarray structure, which exhibits excellent catalytic activity and stability for electrocatalytic water decomposition to produce oxygen. Background Art
[0002] Exploring and developing clean, renewable energy is an effective way to solve energy and environmental problems. Solar energy, wind energy and tidal energy are typical renewable energy sources, but their development is limited by the fact that they are greatly affected by weather, occupy a large area, have low energy density and high cost. A more feasible solution is to convert these renewable energy sources into hydrogen that can be stored and transported, and release the stored energy through hydrogen-oxygen fuel cells when used. Hydrogen production by water electrolysis is a simple and convenient way to convert electrical energy into hydrogen, but it has not been put into practical use on a large scale. The main reason restricting the development of water electrolysis technology is the two half reactions of water electrolysis, the reduction hydrogen evolution reaction of water and the oxidation oxygen evolution reaction. Both half reactions require excellent electrocatalysts to reduce the overpotential, and the overpotential of oxygen evolution accounts for the majority. Therefore, the development of efficient and long-term stable oxygen evolution electrodes is extremely important for hydrogen production by water electrolysis.
[0003] Currently, Ru and Ir-based metal oxides are considered to be the most efficient oxygen-generating catalysts. However, both ruthenium and iridium are precious metals with extremely scarce reserves and high prices, making it difficult to develop them on a large scale for practical applications. Therefore, non-precious metal catalysts with abundant reserves have received widespread attention, and the activity of some of these non-precious metal catalysts can even be comparable to that of RuO2 and IrO2. Recently, there has been an increasing number of studies on non-precious metal catalysts for oxygen evolution.
[0004] Patent CN109837558A discloses a method for preparing an oxyhydroxide iron-nickel iron hydrotalcite oxygen evolution electrode by combining hydrothermal and electrodeposition methods. The method first loads a basic cobalt carbonate nanowire array with a length of 2 to 3 μm and a diameter of 50 to 500 nm on the surface of nickel foam by hydrothermal reaction at 100 to 180°C for 5 to 15 hours, and then loads an oxyhydroxide iron-nickel iron hydrotalcite sheet layer on the surface of the nanowire array by electrodeposition reaction. Although the method prepares an array electrode with a uniformly dispersed structure, the electrode prepared by the method does not show excellent oxygen evolution performance, and only has a low oxygen evolution performance at 10 mA cm -2 The stability test was carried out at a low current density and the test time was short (5h). Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a method for preparing a high-curvature nanoarray electrode for electrocatalytic decomposition of water to produce oxygen with high activity, high durability, low price and abundant reserves.
[0006] The method for preparing the high-curvature nanoarray electrode provided by the present invention comprises the following steps:
[0007] Step 1: Dissolve nickel metal salt, doping metal salt, sodium citrate, boric acid and ammonium chloride in deionized water, and add hydrochloric acid to adjust the pH value of the solution to 4-6 to obtain an electrodeposition solution.
[0008] Step 2: Use the conductive base material as the working electrode, Pt as the counter electrode, and the electrodeposition solution of step 1 as the electroplating solution, and adopt any one of constant current electrodeposition, constant potential electrodeposition, pulse electrodeposition, and cyclic voltammetry to carry out the electrodeposition reaction; the conductive base material after electrodeposition is rinsed with deionized water and vacuum dried to obtain a high-curvature nanoarray electrode.
[0009] In the above step 1, the concentration of nickel metal salt in the electrodeposition solution is 0.1-1 mol / L, the concentration of doping metal salt is 0.01-0.1 mol / L, the concentration of sodium citrate is 0.1-0.4 mol / L, the concentration of boric acid is 0.2-0.8 mol / L, and the concentration of ammonium chloride is 1.2-2.4 mol / L.
[0010] In the above step 1, the doping metal salt is selected from at least one soluble salt of Fe, Co, Zn, Mn, V, Cr, and Mo.
[0011] In the above step 1, the nickel metal salt is any one of nickel chloride, nickel sulfate, nickel nitrate, nickel bromide, and nickel phosphate.
[0012] In the above step 1, the soluble salt is any one of nitrate, sulfate and hydrochloride.
[0013] In the above step 2, the conductive base material is selected from any one of foamed nickel, foamed iron, foamed copper, foamed aluminum, nickel foil, copper foil, iron foil, carbon cloth, and carbon paper.
[0014] In the above step 2, the current density of the constant current electrodeposition method for electrodeposition is 10 to 60 mA / cm 2 , time is 100~1200s, temperature is 40~60℃.
[0015] In the above step 2, the potential of the constant potential electrodeposition method for electrodeposition is -1.5 to -2.5 V, the time is 100 to 1200 s, and the temperature is 40 to 60°C.
[0016] In the above step 2, the potential of the pulse electrodeposition method for electrodeposition is -1.5 to -2.5 V, the time is 100 to 1200 s, and the temperature is 40 to 60°C.
[0017] In the above step 2, the potential of the cyclic voltammetry for electrodeposition is -1.5 to 1.5 V, and the scan rate is 20 to 40 mV·s -1 , scan 40 to 100 cycles, temperature 40 to 60 °C.
[0018] The beneficial effects of the present invention are as follows:
[0019] 1. The present invention prepares a monolithic electrode material with a high-curvature nanoarray structure by a simple, controllable and effective electrochemical deposition method. The obtained high-curvature nanoarray electrode has a very high specific surface area and abundant active sites due to its unique high-curvature nanoarray structure, which is beneficial to reactant transport and charge transfer; and it has super-hydrophilic properties, which is beneficial to material transport and diffusion and the rapid release of oxygen bubbles, providing more active sites for water electrolysis reaction. The high-curvature nanoarray electrode of the present invention exhibits excellent activity and stability in the electrocatalytic water decomposition reaction, and has better electrochemical catalytic performance than the commercial catalyst Ir / C, which has very important theoretical and practical research significance for the development of hydrogen production by water electrolysis.
[0020] 2. Compared with other methods, the preparation method of the present invention is simpler to operate, has milder conditions, is less time-consuming, and has low energy consumption. The in-situ grown nanoarray electrode avoids the problem of active substances being easily detached and unstable due to the use of binders in traditional preparation methods, and greatly improves the electrochemical performance and stability of the electrode. In addition, the raw materials used are inexpensive and abundant in reserves, making them suitable for large-scale production. Compared with some traditional impregnation methods, hydrothermal methods, colloid methods, etc., the reaction conditions of the electrodeposition method are relatively mild. It only requires simple changes in the electrodeposition parameters (deposition time, voltage, current, temperature, pH, etc.), and the amount of deposition and the morphology of the electrode can be easily controlled. It is a method that is easy to control the synthesis and large-scale industrial production of electrodes.
[0021] 3. The present invention adopts a one-step electrodeposition method, using a deposition solution prepared with nickel metal salt, soluble metal salt, sodium citrate, boric acid and ammonium chloride in different proportions to perform electrodeposition, so that nickel metal and other metal elements synergistically catalyze each other to obtain a high-curvature nano-array nickel foam oxygen evolution electrode with excellent catalytic activity and stability. In addition, during the deposition process, a variety of electrodeposition methods are selected. The optimal deposition method can not only greatly reduce the energy loss during deposition, but also optimize the deposition process, greatly improving the performance of the electrode.
[0022] 4. Compared with the traditional electrode preparation method, the one-step electrodeposition method has the advantages of simple process, controllable conditions, low energy consumption, low cost, and easy industrial production. -2The overpotential under current density is 320mV for commercial noble metal Ir / C catalyst, while the overpotential of the electrode of the present invention is only 220mV, which shows that the electrode of the present invention has obvious advantages. In addition, the price of commercial noble metal catalyst Ir / C is 980 yuan / g, while the price of metal salts required by the present invention, such as nickel sulfate, is 0.46 yuan / g, the price of iron sulfate is 0.34 yuan / g, and the price of cobalt sulfate is 0.35 yuan / g. Moreover, the reserves of these transition metals are huge, which has a huge advantage in production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a high-magnification SEM image of the high-curvature nanoarray nickel foam electrode prepared in Example 1.
[0024] Figure 2 This is a high-magnification SEM image of the high-curvature nanoarray nickel foam electrode prepared in Example 2.
[0025] Figure 3 This is a high-magnification SEM image of the high-curvature nanoarray nickel foam electrode prepared in Example 3.
[0026] Figure 4 This is a high-magnification SEM image of the high-curvature nanoarray nickel foam electrode prepared in Example 4.
[0027] Figure 5 This is a high-magnification SEM image of the high-curvature nanoarray nickel foam electrode prepared in Example 5.
[0028] Figure 6 This is a high-magnification SEM image of the high-curvature nanoarray nickel foam electrode prepared in Example 6.
[0029] Figure 7 This is the EDX mapping spectrum of the high curvature nanoarray nickel foam electrode prepared in Example 1.
[0030] Figure 8 This is a contact angle diagram of the high-curvature nanoarray nickel foam electrode prepared in Example 1.
[0031] Fig. 9 It is the LSV curve of the OER reaction of the high curvature nanoarray electrode prepared in Example 1, Example 5, and Example 6 and commercial Ir / C.
[0032] Fig.10 This is a graph showing the stability test results of the high-curvature nanoarray electrode prepared in Example 1 under high current. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0034] Example 1
[0035] Step 1: At room temperature, weigh 0.05 mol of nickel chloride hexahydrate, 0.005 mol of sodium citrate, 0.004 mol of ferric chloride hexahydrate, 0.01 mol of boric acid, and 0.06 mol of ammonium chloride, put them in 50 mL of deionized water, stir and mix them evenly, and use 3 mol / L hydrochloric acid aqueous solution to adjust the pH of the resulting solution to 5.0 to obtain an electrodeposition solution.
[0036] Step 2: Cut the nickel foam into a 2cm×4cm rectangle, and remove the oxide layer on the surface of the nickel foam by ultrasonic treatment in a 3mol / L hydrochloric acid aqueous solution for 30 minutes. Then, ultrasonic treatment was performed in deionized water for 30 minutes to remove dust. After washing, ultrasonic treatment was performed in anhydrous ethanol for 30 minutes to remove oil stains. Then, ultrasonic cleaning was performed with distilled water, and finally, vacuum drying was performed at 60°C to obtain the pretreated nickel foam. The pretreated nickel foam was used as the working electrode, Pt as the counter electrode, and the electrodeposition solution in step 1 was used as the electroplating solution. Constant current electrodeposition was performed at 60°C with a flow rate of 20 mA cm -2 The electrodeposition reaction was carried out at a current density of , and the electrodeposition time was 600s; the nickel foam after electrodeposition was rinsed with deionized water and vacuum dried at 80°C for 12h to obtain a high curvature nanoarray electrode in which Ni-Fe was co-deposited on a porous nickel foam with a pore structure.
[0037] Example 2
[0038] Step 1: At room temperature, weigh 0.02 mol of nickel sulfate hexahydrate, 0.005 mol of sodium citrate, 0.001 mol of ferric chloride hexahydrate, 0.01 mol of boric acid, and 0.06 mol of ammonium chloride, place them in 50 mL of deionized water, stir and mix evenly, and use 3 mol / L hydrochloric acid aqueous solution to adjust the pH of the resulting solution to 5.0 to obtain an electrodeposition solution.
[0039] Step 2: Cut the nickel foam into a 2cm×4cm rectangle, ultrasonically treat the nickel foam in a 3mol / L hydrochloric acid aqueous solution for 30 minutes to remove the oxide layer on the surface, ultrasonically treat the nickel foam in deionized water for 30 minutes to remove dust, and then ultrasonically treat the nickel foam in anhydrous ethanol for 30 minutes to remove oil, and then ultrasonically clean the nickel foam with distilled water, and finally vacuum dry the nickel foam at 60°C to obtain the pretreated nickel foam. The pretreated nickel foam was used as the working electrode, Pt as the counter electrode, and the electroplating solution in step 1 was used as the electroplating solution. Constant current electrodeposition was performed at 60°C with a flow rate of 40 mA cm -2 The electrodeposition reaction was carried out at a current density of , and the electrodeposition time was 300s; the nickel foam after electrodeposition was rinsed with deionized water and vacuum dried at 80°C for 12h to obtain a high curvature nanoarray electrode in which Ni-Fe was co-deposited on a porous nickel foam with a pore structure.
[0040] Example 3
[0041] Step 1: At room temperature, weigh 0.02 mol of nickel nitrate hexahydrate, 0.005 mol of sodium citrate, 0.004 mol of ferric chloride hexahydrate, 0.01 mol of boric acid, and 0.06 mol of ammonium chloride, put them in 50 mL of deionized water, stir and mix them evenly, and use 3 mol / L hydrochloric acid aqueous solution to adjust the pH of the resulting solution to 5.0 to obtain an electrodeposition solution.
[0042] Step 2: Cut the nickel foam into a 2cm×4cm rectangle, remove the oxide layer on the surface of the nickel foam by ultrasonic treatment in a 3mol / L hydrochloric acid aqueous solution for 30 minutes, remove dust by ultrasonic treatment in deionized water for 30 minutes, remove oil stains by ultrasonic treatment in anhydrous ethanol for 30 minutes after washing, and then ultrasonic cleaning with distilled water, and finally vacuum drying at 60°C to obtain the pretreated nickel foam. Using the pretreated nickel foam as the working electrode, Pt as the counter electrode, and the electrodeposition solution of step 1 as the electroplating solution, the electrodeposition reaction was carried out at a potential of -2.0V at 60°C by constant potential electrodeposition method, and the electrodeposition time was 600s; the nickel foam after electrodeposition was rinsed with deionized water and vacuum dried at 80°C for 12 hours to obtain a high curvature nanoarray electrode of Ni-Fe co-deposited on a porous nickel foam with a pore structure.
[0043] Example 4
[0044] Step 1: At room temperature, weigh 0.05 mol of nickel chloride hexahydrate, 0.005 mol of sodium citrate, 0.004 mol of ferric chloride hexahydrate, 0.01 mol of boric acid, and 0.06 mol of ammonium chloride, put them in 50 mL of deionized water, stir and mix them evenly, and use 3 mol / L hydrochloric acid aqueous solution to adjust the pH of the resulting solution to 5.0 to obtain an electrodeposition solution.
[0045] Step 2: Cut the nickel foam into a 2cm×4cm rectangle, remove the oxide layer on the surface of the nickel foam by ultrasonic treatment in a 3mol / L hydrochloric acid aqueous solution for 30 minutes, remove dust by ultrasonic treatment in deionized water for 30 minutes, remove oil stains by ultrasonic treatment in anhydrous ethanol for 30 minutes after washing, and then ultrasonic cleaning with distilled water, and finally vacuum drying at 60°C to obtain the pretreated nickel foam. Using the pretreated nickel foam as the working electrode, Pt as the counter electrode, and the electrodeposition solution of step 1 as the electroplating solution, the electrodeposition reaction was carried out at a potential of -1.5V at 60°C by constant potential electrodeposition method, and the electrodeposition time was 900s; the nickel foam after electrodeposition was rinsed with deionized water and vacuum dried at 80°C for 12 hours to obtain a high curvature nanoarray electrode of Ni-Fe co-deposited on a porous nickel foam with a pore structure.
[0046] Example 5
[0047] Step 1: At room temperature, weigh 0.05 mol of nickel chloride hexahydrate, 0.005 mol of sodium citrate, 0.004 mol of cobalt chloride hexahydrate, 0.01 mol of boric acid, and 0.06 mol of ammonium chloride, put them in 50 mL of deionized water, stir and mix them evenly, and use 3 mol / L hydrochloric acid aqueous solution to adjust the pH of the resulting solution to 5.0 to obtain an electrodeposition solution.
[0048] Step 2: Cut the nickel foam into a 2cm×4cm rectangle, ultrasonically treat the nickel foam in a 3mol / L hydrochloric acid aqueous solution for 30 minutes to remove the oxide layer on the surface, ultrasonically treat the nickel foam in deionized water for 30 minutes to remove dust, and then ultrasonically treat the nickel foam in anhydrous ethanol for 30 minutes to remove oil, and then ultrasonically clean the nickel foam with distilled water, and finally vacuum dry the nickel foam at 60°C to obtain the pretreated nickel foam. The pretreated nickel foam was used as the working electrode, Pt as the counter electrode, and the electroplating solution in step 1 was used as the electroplating solution. Constant current electrodeposition was performed at 60°C with a flow rate of 40 mA cm -2 The electrodeposition reaction was carried out at a current density of , and the electrodeposition time was 800s; the nickel foam after electrodeposition was rinsed with deionized water and vacuum dried at 80°C for 12h to obtain a high curvature nanoarray electrode in which Ni-Co was co-deposited on a porous nickel foam with a pore structure.
[0049] Example 6
[0050] Step 1: At room temperature, weigh 0.05 mol of nickel chloride hexahydrate, 0.005 mol of sodium citrate, 0.002 mol of manganese chloride tetrahydrate, 0.01 mol of boric acid, and 0.06 mol of ammonium chloride, place them in 50 mL of deionized water, stir and mix them evenly, and use 3 mol / L hydrochloric acid aqueous solution to adjust the pH of the resulting solution to 5.0 to obtain an electrodeposition solution.
[0051] Step 2: Cut the nickel foam into a rectangle of 2cm×4cm, remove the oxide layer on the surface of the nickel foam by ultrasonic treatment in a 3mol / L hydrochloric acid aqueous solution for 30min, remove dust by ultrasonic treatment in deionized water for 30min, remove oil stains by ultrasonic treatment in anhydrous ethanol for 30min, and then ultrasonic cleaning with distilled water, and finally vacuum drying at 60℃ to obtain the pretreated nickel foam. Using the pretreated nickel foam as the working electrode, Pt as the counter electrode, and the electrodeposition solution of step 1 as the electroplating solution, the electrodeposition reaction was carried out by cyclic voltammetry at 60℃ at a potential between 0.1 and -1.5V, and the scan rate was 20mV·s -1 The number of cycles was 80; the nickel foam after electrodeposition was rinsed with deionized water and vacuum dried at 80°C for 12 h to obtain a high-curvature nanoarray electrode in which Ni-Mn was co-deposited on a porous nickel foam with a pore structure.
[0052] The electrodes obtained in Examples 1 to 6 were characterized by scanning electron microscopy. Figures 1 to 6 As can be seen from the figure, a neatly arranged, uniformly sized, high-curvature nanoarray grows in situ on the surface of the substrate material. The nanocones are uniform in size, 0.5 to 1.5 μm long, 100 to 300 nm in diameter, and grow perpendicular to the surface of the substrate material.
[0053] The electrode obtained in Example 1 was characterized by SEM Mapping. Figure 7 ,It can be seen from the figure that Ni, Fe, and O elements are ,evenly distributed on the surface of the nanostructure, indicating the successful ,doping of metal elements.
[0054] The contact angle test of the electrode obtained in the above embodiment 1 is shown in FIG. Figure 8 As can be seen from the figure, the liquid droplet instantly penetrates into the electrode when it contacts the electrode surface, indicating that the electrode material prepared by the present invention has extremely strong hydrophilicity.
[0055] Electrochemical tests were performed on the electrodes obtained in Examples 1, 5, and 6 using a CHI 660E electrochemical workstation. The specific method was as follows: In a 1 mol / L KOH aqueous solution, a three-electrode system was used, with the electrodes obtained in Examples 1, 5, and 6 as working electrodes, a carbon rod as a counter electrode, and saturated Ag / AgCl as a reference electrode. Linear voltammetry tests were performed at 25°C, and the performance was compared with that of the commercial catalyst Ir / C drop-coated on nickel foam. The results are shown in Table 1. Fig. 9 As can be seen from the figure, at 100mA cm -2 Under the current density, the overpotential of the electrode prepared in Example 1 is 220 mV, the overpotential of the electrode prepared in Example 5 is 243 mV, the overpotential of the electrode prepared in Example 6 is 251 mV, and the overpotential of the commercial catalyst Ir / C is 320 mV, indicating that the electrode prepared in the present invention has excellent oxygen evolution catalytic activity.
[0056] The electrode obtained in Example 1 was subjected to 500 mA cm -2 The oxygen evolution stability test was carried out at the current density, and the results are shown in Fig.10 As can be seen from the figure, the electrode of the present invention can maintain long-term stability for 48 hours at a high current density, and the voltage rise is less than 10%.
Claims
1. A method for preparing a high-curvature nanoarray electrode for electrocatalytic decomposition of water to produce oxygen, characterized in that: The method comprises the following steps: Step 1: dissolving nickel metal salt, doping metal salt, sodium citrate, boric acid and ammonium chloride in deionized water, and adding hydrochloric acid to adjust the pH value of the solution to 4-6 to obtain an electrodeposition solution; Step 2: Use the conductive base material as the working electrode, Pt as the counter electrode, and the electrodeposition solution of step 1 as the electroplating solution, and adopt any one of constant current electrodeposition, constant potential electrodeposition, pulse electrodeposition, and cyclic voltammetry to carry out the electrodeposition reaction; the conductive base material after electrodeposition is rinsed with deionized water and vacuum dried to obtain a high-curvature nanoarray electrode.
2. The method for preparing a high-curvature nanoarray electrode for electrocatalytic water decomposition and oxygen production according to claim 1, characterized in that: The concentration of nickel metal salt in the electrodeposition solution is 0.1-1 mol / L, the concentration of doped metal salt is 0.01-0.1 mol / L, the concentration of sodium citrate is 0.1-0.4 mol / L, the concentration of boric acid is 0.2-0.8 mol / L, and the concentration of ammonium chloride is 1.2-2.4 mol / L.
3. The method for preparing a high-curvature nanoarray electrode for electrocatalytic water decomposition and oxygen production according to claim 1 or 2, characterized in that: The doping metal salt is selected from at least one soluble salt of Fe, Co, Zn, Mn, V, Cr, and Mo.
4. The method for preparing a high-curvature nanoarray electrode for electrocatalytic water decomposition and oxygen production according to claim 1 or 2, characterized in that: The nickel metal salt is any one of nickel chloride, nickel sulfate, nickel nitrate, nickel bromide and nickel phosphate.
5. The method for preparing a high-curvature nanoarray electrode for electrocatalytic water decomposition and oxygen production according to claim 3, characterized in that: The soluble salt is any one of nitrate, sulfate and hydrochloride.
6. The method for preparing a high-curvature nanoarray electrode for electrocatalytic water decomposition and oxygen production according to claim 1, characterized in that: The conductive base material is selected from any one of foamed nickel, foamed iron, foamed copper, foamed aluminum, nickel foil, copper foil, iron foil, carbon cloth, and carbon paper.
7. The method for preparing a high-curvature nanoarray electrode for electrocatalytic water decomposition and oxygen production according to claim 1, characterized in that: The current density of the constant current electrodeposition method for electrodeposition is 10 to 60 mA / cm 2 , time is 100~1200s, temperature is 40~60℃.
8. The method for preparing a high-curvature nanoarray electrode for electrocatalytic water decomposition and oxygen production according to claim 1, characterized in that: The constant potential electrodeposition method is performed at a potential of -1.5 to -2.5 V, a time of 100 to 1200 seconds, and a temperature of 40 to 60°C.
9. The method for preparing a high-curvature nanoarray electrode for electrocatalytic water decomposition and oxygen production according to claim 1, characterized in that: The pulse electrodeposition method is performed at a potential of -1.5 to -2.5 V, a time of 100 to 1200 seconds, and a temperature of 40 to 60°C.
10. The method for preparing a high-curvature nanoarray electrode for electrocatalytic water decomposition and oxygen production according to claim 1, characterized in that: The potential for electrodeposition by cyclic voltammetry is -1.5 to 1.5 V, and the scan rate is 20 to 40 mV·s -1 , scan 40 to 100 cycles, temperature 40 to 60 °C.
Citation Information
Cited By
Preparation method and application of low-crystallinity NiFe LDH three-dimensional nanosheet array catalyst