Preparation method of cobalt-nitrogen-doped carbon positive electrode material for zinc-iodine battery as well as product and application of cobalt-nitrogen-doped carbon positive electrode material

Through the preparation of cobalt nitrogen-doped carbon positive electrode material, the problems of low iodine conductivity and shuttle effect in zinc-iodine batteries were solved, and high cycle stability and electrochemical performance were improved. Co-NC materials showed that under high current Excellent capacity and long cycle performance.

CN118943366AActive Publication Date: 2024-11-12NINGBO JIERONG NEW MATERIALS CO LTD +1

Patent Information

Application Number
CN202410857198.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-12
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

The low conductivity of iodine and the shuttle effect caused by the dissolution of active substances in zinc-iodine batteries reduces the cycle stability and energy density of the battery. Traditional porous carbon materials do not have enough physical constraints on iodine, which affects energy storage efficiency.

Method used

The preparation method of cobalt nitrogen doped carbon positive electrode material is used to mix the carbon source, nitrogen source and manganese carbonate, and react with cobalt salt and iodine element after heating to form a cobalt nitrogen coordination structure, providing a stable anchor positioning point and accelerating Iodine redox reaction improves catalytic activity.

Benefits of technology

The cycling stability and electrochemical performance of zinc-iodine batteries have been significantly improved. The capacity of Co-NC materials is 185mAh g-1 at 5C current, and can cyclize 20,000 times. The Coulomb efficiency is close to 100%, and the iodine is improved through physical and chemical constraints. Reversible transformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943366A_ABST
    Figure CN118943366A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a cobalt-nitrogen-doped carbon positive electrode material of a zinc-iodine battery as well as a product and application of the cobalt-nitrogen-doped carbon positive electrode material. The formation of a cobalt-nitrogen coordination structure can provide a stable anchoring site for iodine species, accelerate rapid conversion of an iodine redox reaction and enhance reaction kinetics. Through the formation of the structure, the catalytic activity of iodine conversion reaction can be remarkably improved, and the cycling stability of the zinc-iodine battery is improved. The Co-NC has the capacity of 185 mAh g <-1 > under the current of 5C, can maintain the capacity of 102 mAh g <-1 > under the current of 50C, and can stably circulate for 20000 circles, and the coulombic efficiency is close to 100%. According to the invention, cobalt-nitrogen coordination provides catalytic active sites and conductivity, the cobalt-nitrogen coordination has the effect of accelerating and catalyzing conversion of polyiodide and the effect of adsorbing iodine, reversible conversion of iodine is improved through a physical and chemical constraint effect, and the long cycle performance of the zinc-iodine battery under high current is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of zinc-iodine battery materials, and specifically relates to a preparation method of a cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries, and a product and application thereof. Background Art

[0002] The doping of sulfur element (non-metallic element) has high electrocatalytic activity. The doping of sulfur element improves the electrochemical performance of zinc-iodine batteries, but there are still certain problems. The capacity provided by nitrogen-sulfur dual-doped carbon materials used in zinc-iodine batteries is relatively low.

[0003] Since the active material of Zn-I2 battery (ZIB) will be l3 - and I5 - The I3 is dissolved in the water-based electrolyte in the form of Zn, resulting in a serious shuttle effect and reducing the cycling stability of the Zn negative electrode, thereby reducing the actual energy density of the battery and accelerating capacity degradation. - and I5 - The formation of I2 is mainly due to the slow kinetics of the iodine conversion reaction in zinc-iodine batteries, and the poor conductivity of iodine further exacerbates the charge transfer barrier of the electrochemical reaction. Due to its poor conductivity, the positive electrode usually relies on a conductive carrier (such as porous carbon, carbon cloth, graphene, etc.) to transport electrons.

[0004] Loading iodine on a conductive carrier can effectively enhance the electron transfer capacity and redox conversion. Traditional porous carbon materials only provide physical confinement for iodine and polyiodides. Although porous carbon materials can confine iodine in the positive electrode through physical action, the formation of soluble iodide species will reduce the energy storage efficiency and cycle stability. Summary of the invention

[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and to briefly introduce some preferred embodiments.

[0006] As one aspect of the present invention, the present invention provides a method for preparing a cobalt-nitrogen doped carbon positive electrode material for a zinc-iodine battery, which comprises:

[0007] (1) mixing a carbon source, a nitrogen source and manganese carbonate uniformly, heating to 800-850° C., washing and drying to obtain an NC material;

[0008] (2) mixing the NC material obtained in step (1) with a cobalt salt, drying the obtained mixture, heating it to 800-850° C., filtering, washing, and drying to obtain a Co-NC material;

[0009] (3) The Co-NC material obtained in step (2) is mixed with iodine, ground, heated to 110-130° C. in an inert atmosphere for reaction, and then heated in air to remove iodine to obtain a positive electrode material.

[0010] As a preferred embodiment of the method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to the present invention: in step (1), the carbon source includes methyl cellulose, and the nitrogen source includes urea.

[0011] As a preferred embodiment of the method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to the present invention: in step (1), the mass ratio of the carbon source, the nitrogen source and the manganese carbonate is 1:0.5 to 1:5 to 10.

[0012] As a preferred embodiment of the method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries of the present invention: in step (1), the heating is carried out at 5°C min under an inert atmosphere. -1 Heat to 250℃ and keep warm for 1-2h, then heat at 5℃min. -1 Raise the temperature to 800℃ and keep it for 2 to 3 hours.

[0013] As a preferred embodiment of the method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to the present invention: in step (2), the cobalt salt includes cobalt nitrate hexahydrate, and the mass ratio of the NC material to the cobalt salt is 1:0.97.

[0014] As a preferred embodiment of the method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries of the present invention: in step (2), the heating is carried out at 10°C min under an inert atmosphere. -1 Heat to 130℃ and keep warm for 3-4h, then heat at 5℃min -1 Raise the temperature to 800℃ and keep it for 2 to 3 hours.

[0015] As a preferred embodiment of the method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries described in the present invention: in step (3), the mass ratio of the Co-NC material to the iodine element is 1:1.

[0016] As a preferred embodiment of the method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to the present invention: in step (3), the inert atmosphere includes argon; the heating to 110-130°C for reaction is heating to 120°C for reaction for 8-10 hours; the heating in air is heating to 100°C in air and keeping warm for 12-24 hours.

[0017] Beneficial effects of the present invention: The formation of the cobalt-nitrogen coordination structure of the present invention can provide a stable anchoring site for iodine species, accelerate the rapid conversion of iodine redox reaction, and enhance the reaction kinetics. Electrochemical tests show that the formation of this structure can significantly improve the catalytic activity of iodine conversion reaction and enhance the cycle stability of zinc-iodine battery. The capacity of Co-NC at 5C current is 185mAh g -1 , can maintain 102mAh g at a current of 50C -1 , and can stably cycle 20,000 times, and the coulombic efficiency is close to 100%. The present invention verifies that cobalt-nitrogen coordination provides catalytic active sites and conductivity, has the function of accelerating the conversion of catalytic polyiodides and the adsorption of iodine, and improves the reversible conversion of iodine through the physical and chemical constraint effect, thus achieving the long cycle performance of zinc-iodine battery under high current. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following briefly introduces the drawings required for describing the embodiment, wherein:

[0019] Figure 1 Flow chart for the preparation of Co-NC.

[0020] Figure 2 SEM images of C-I2, NC-l2 and Co-NC-l2; EDS element distribution image of Co-NC-l2.

[0021] Figure 3 The LSV curves of the oxidation process of C, NC and Co-NC, the Tafel slope curve calculated from the LSV curve of the oxidation process, the LSV curve of the reduction process, and the Tafel slope curve calculated from the LSV curve of the reduction process.

[0022] Figure 4 CV curves of C, NC and Co-NC at different scan rates; b value calculated from CV; Co-NC at 5 mV s -1 Capacitance contribution rate; Nyquist plots of C, NC and Co-NC.

[0023] Figure 5 is the adsorption capacity of C, NC and Co-NC in 2M ZnSO4+0.02M l2(2m M l3-) aqueous solution, and the intensity of UV-visible absorbance I3v after adsorption for 48 h.

[0024] Figure 6 This is the in-situ Raman image at 0.3C.

[0025] Figure 7 SEM images of dendrites on the surface of zinc negative electrode after C-l2 and Co-NC-l2 were cycled 1000 times.

[0026] Figure 8 Schematic diagram of the principle of rechargeable Zn-I2 battery based on Co-NC positive electrode.

[0027] Fig. 9 For C, NC and Co-NC at 0.5 mV s -1 CV curve, the starting potential of the positive and negative electrode reactions of CV, and the Tafel slope calculated based on CV; at 0.5 mV s -1 Overlap test of the first 4 CV curves.

[0028] Fig.10 Rate performance of C, NC and Co-NC at different currents; charge and discharge curves of Co-NC at different currents.

[0029] Fig.11 The self-discharge time-voltage curves of C, NC and Co-NC after standing for 48 hours.

[0030] Fig.12 The cycling performance of C, NC and Co-NC at 5C, the charge-discharge curve of the 800th cycle at 5C, the long-cycle performance of Co-NC at 50C and the charge-discharge curves of different cycles at 5C. DETAILED DESCRIPTION

[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.

[0032] Preparation of Co-NC, NC, and C materials:

[0033] Preparation of C materials: Methyl cellulose (article number: C03X006; viscosity: 15 cPs; molecular weight: 454.5; cas number: 9004-67-5) and manganese carbonate were mixed at a mass ratio of 1:5. The mixed mixture was heated at 5 °C min in an argon atmosphere. -1 Heat to 250℃ and keep warm for 1h, then heat at 5℃min -1 The temperature was raised to 800°C and kept for 2 hours. The obtained product was pickled with hydrochloric acid to remove manganese carbonate, then filtered and washed for multiple times, and finally vacuum dried to obtain the product.

[0034] NC material preparation: Methyl cellulose, urea and manganese carbonate were mixed at a mass ratio of 1:0.5:5, and the mixed mixture was heated at 5 °C min in an argon atmosphere. -1 Heat to 250℃ and keep warm for 1h, then heat at 5℃min -1 The temperature was raised to 800°C and kept for 2 hours. The obtained product was washed with hydrochloric acid to remove manganese carbonate, and then filtered and washed for multiple times, and finally vacuum dried to obtain the product.

[0035] Preparation of Co-NC material: NC and cobalt nitrate hexahydrate were mixed in deionized water at a mass ratio of 1:0.97 and stirred for 4 hours. The obtained mixture was evaporated to dryness using a rotary evaporator. The dried mixture was heated at 10 °C min under an argon atmosphere. -1 Heat to 130℃ and keep warm for 3h, then -1 The temperature was raised to 800°C and kept for 2 hours. The obtained product was washed with hydrochloric acid, filtered and washed for several times, and finally dried in vacuum to obtain the product.

[0036] Figure 1 Flow chart for the preparation of Co-NC.

[0037] Preparation of Co-NC-l2, NC-l2 and C-l2 materials:

[0038] like Figure 1 As shown, the prepared C, NC and Co-NC materials are respectively mixed with iodine in a mass ratio of 1:1 and fully ground. The ground mixture is loaded into a 50 mL reactor liner under an argon atmosphere. The reactor is kept warm at 120°C for 8 hours. The obtained mixture is kept warm at 100°C for 12 hours in air to remove the iodine on its surface.

[0039] Electrode preparation:

[0040] The electrode sheet was prepared by wet method. The Co-NC-l2, NC-l2 or C-l2 active material, conductive agent (conductive carbon black) and binder (polyvinylidene fluoride) prepared above were mixed in a mass ratio of 8:1:1 and added to the mixer in batches. Then, an appropriate amount of N-methylpyrrolidone solution (150 microliters of N-methylpyrrolidone solution per 10 mg of the mixture) was added, and the mixture was degassed and mixed to form a uniform slurry. 15 microliters of slurry was taken with a pipette and dropped onto the steel sheet. The active material loading of each electrode sheet was 1.5 mg cm -2 , and placed it in a vacuum oven at 40°C and dried for 12 h as the positive electrode material.

[0041] Battery Assembly:

[0042] The zinc sheet was carefully polished with fine sandpaper before use, then ultrasonically placed in anhydrous ethanol for half an hour, and dried as a negative electrode, with a 2M ZnSO4 solution as the electrolyte. The positive electrode shell, the positive electrode material, the electrolyte, the diaphragm, the electrolyte, the zinc sheet, the gasket, the shrapnel, and the negative electrode shell were assembled in the order of the positive electrode shell. 30 microliters of electrolyte were placed above and below the diaphragm for each battery. After the assembly was completed, the battery was sealed with a sealing machine at a pressure of 50M Pa, and the assembly process was kept consistent each time.

[0043] Experimental results:

[0044] Morphology and structure characterization:

[0045] Cobalt-doped active sites were introduced into the porous carbon structure, which significantly promoted the adsorption and reduction kinetics of iodine. Scanning electron microscopy (SEM) images of C-l2, NC-l2 and Co-NC-l2 were studied. The morphology of the sample did not change significantly after iodine was added, and there was no obvious iodine crystal distribution on the surface, indicating that iodine was diffusely deposited inside the pores instead of accumulating on the outer surface. EDS mapping images are shown in Figure 2. Figure 2 As shown in (d), the elements C, N, Co, and I are uniformly dispersed throughout the sample, indicating that iodine has been successfully loaded into the carbon material and is uniformly distributed in the carbon material.

[0046] Figure 2 SEM images of (a) C-l2, (b) NC-l2 and (c) Co-NC-l2; (d) EDS element distribution image of Co-NC-l2.

[0047] Electrocatalytic activity characterization:

[0048] In order to further explore the profound effect of the electrocatalytic sites of cobalt-nitrogen doped carbon materials on the kinetics of redox reactions, the Tafel slopes of the reduction and oxidation reactions were compared and analyzed. According to the linear sweep voltammetry (LSV) test of Zn-l2 battery ( Figure 3 ) shows that during the iodine oxidation process ( Figure 3 a), the potential change of Co-NC-l2 is 1.08V, while that of C-l2 and NC-l2 is 1.19V and 1.13V respectively, indicating that Co-NC-l2 can undergo iodine oxidation reaction at a lower voltage. Figure 3 c), the overpotential of Co-NC-l2 is smaller. Figure 3 In b, in the iodine oxidation reaction, Co-NC-l2 (16.7mVdec -1 ) Lower than Nc-I2 (158.1mV dec -1 ) and C-l2 (424.1mV dec -1 ), which is attributed to the excellent catalytic activity of the Co-NC active center. Similarly, in the iodine reduction reaction, Co-NC-l2 (98mV dec -1 ) has a lower Tafel slope than NC-12 (189mV dec -1 ) and C-l2 (204mV dec -1 ), Co-NC exhibited better catalytic performance in iodine oxidation reaction. These results indicate that Co-NC has a better catalytic effect on l2 / l -The conversion has a higher electrocatalytic activity.

[0049] Figure 3 (a) LSV curves of the oxidation process for C, NC and Co-NC, (b) Tafel slope curve calculated from the LSV curve of the oxidation process, (c) LSV curves of the reduction-oxidation process, and (d) Tafel slope curve calculated from the LSV curve of the reduction process.

[0050] In order to evaluate the electrochemical performance of C-l2, NC-I2 and Co-NC-I2 cathodes, we assembled zinc-iodine batteries and conducted Figure 4 Cyclic voltammetry test with 0.5 to 5 mV s -1 The CV curves at different scan rates further analyzed the kinetics of the C-I2, NC-l2, and Co-NC-l2 cathodes. As the scan rate increased, the redox current also increased accordingly ( Figure 4 ac), the oxidation peak and reduction peak of the zinc-iodine battery assembled with the C-I2 positive electrode deviate with the increase of the scan rate, indicating the polarization enhancement. At the same time, the zinc-iodine battery assembled with the Co-NC-l2 positive electrode has the highest current response and the largest peak potential difference, indicating the superior kinetic conversion of iodine species in Co-NC. The type of electrochemical behavior can be determined by measuring the equation of scan rate (v) and current (i) to determine the parameters (i = a·v b ), where the b value indicates an electrochemical process dominated by ion diffusion (when the b value is close to 0.5) or a capacitive process (when the b value is close to 1). Figure 4 As shown in Figure 1, the b values ​​of the oxidation peak and reduction peak of the zinc-iodine battery assembled with C-l2 positive electrode are 0.65 and 0.87, respectively. Figure 4 d), the b values ​​of the oxidation peak and reduction peak of the zinc-iodine battery assembled with NC-I2 positive electrode are 0.82 and 0.84 respectively ( Figure 4 e), the b values ​​of the oxidation peak and reduction peak of the zinc-iodine battery assembled with Co-NC-l2 positive electrode are 0.82 and 0.84, respectively ( Figure 4 f), which means that C-I2, NC-l2 and Co-NC-l2 are affected by diffusion-controlled processes and surface capacitance control. Among them, the b value of Co-NC-l2 is the largest, which means that the capacitive reaction plays a more dominant role in the charge storage mechanism. The pseudocapacitive contribution is given by Log i = b·Log v +Log a Calculation: where k1v is the pseudo capacity contribution, k2v 1 / 2 is a diffusion-controlled process. As the scan rate increases, the capacitive charge contribution becomes dominant. Figure 4 It can be seen that at 0.5, 0.8, 1.0, 2.0, and 5.0 mV s -1When , the capacitance contributions of Co-NC-l2 are 82%, 85%, 88%, 90% and 95%, respectively, indicating that Co-NC-l2 has high electrochemical kinetics. -1 At high scan rates, the capacitance contribution rate reaches about 95% ( Figure 4 g), which means the excellent rate performance of Co-NC-l2. The strong capacitance contribution originates from the fast redox reaction of iodine caused by the porous carbon structure and electrocatalysis. Electrochemical impedance spectroscopy (EIS) tests were carried out to detect the charge transfer kinetics of zinc-iodine batteries. In the Nyquist plot ( Figure 4 i), in the original state, the charge transfer resistance (R Ct ) of Co-NC-l2 (55Ω) is lower than that of NC-I2 (65Ω) and C-l2 (234Ω), which indicates that Co-NC-l2 has higher catalytic activity.

[0051] Figure 4 CV curves of (a) C, (b) NC and (c) Co-NC at different scan rates; b values ​​calculated from CV for (d) C, (e) NC and (f) Co-NC; Co-NC (g) at 5 mV s -1 Capacitance contribution rate, (h) capacitance contribution rate statistics; (i) Nyquist plot of C, NC and Co-NC.

[0052] Adsorption experiments and iodine conversion kinetics studies:

[0053] In order to observe the adsorption capacity of C, NC and Co-NC for polyiodide, the adsorption capacity of C, NC and Co-NC was studied by immersing them in 2MZnSO4+0.02M I2 (2mM l3-) aqueous solution for 48 hours. Figure 5 a. Compared with other solutions, the Co-NC solution is almost transparent. The UV-visible absorbance spectrum shows that ( Figure 5 b), Co-NC has the weakest l3-signal, the smallest proportion of polyiodide in the solution, and the strongest adsorption of polyiodide. Compared with C-l2 and NC-I2 cathodes, Co-NC-I2 cathode shows the lowest peak intensity and the weakest yellow color after 48h, indicating that Co-NC host has a strong physical / chemical adsorption effect on l2.

[0054] Figure 5 For C, NC and Co-NC (a) in 2M ZnSO4+0.02M l2(2mM l3 - ) adsorption capacity of aqueous solution, (b) intensity of UV-vis absorbance l3- after 48 h of adsorption.

[0055] In order to explore the redox kinetics of Co-NC in Zn-l2 batteries, in situ Raman measurements were performed at 0.3 C. The in situ Raman spectrum of the Zn-l2 battery using Co-NC-l2 cathode showed two main peaks at 110 and 165 cm -1 ( Figure 6 ), which can be attributed to l3 - and I5 - The symmetric stretching mode of the two Raman peaks increases in intensity during charging and reaches a maximum intensity at 1.7 V, demonstrating a highly reversible transformation of polyiodide. During discharge, the intensity of these Raman peaks decreases slightly until they disappear completely, indicating that polyiodide transformation occurs (l5 - →I3 - →I - ). The introduction of Co-NC successfully accelerated the reversible transformation of iodine species.

[0056] Due to the confinement of iodine and iodide by Co-NC, the polyiodide anions are firmly anchored on the positive electrode side during the cycle, thus preventing the shuttle effect and the corrosion of the polyiodide on the zinc negative electrode, thereby increasing the cycle stability and battery life of the battery. Figure 7 As shown in a, in the SEM image of the negative electrode of the zinc-iodine battery assembled with the C-l2 positive electrode after 1000 cycles, it can be seen that the surface of the zinc negative electrode has obvious corrosion, showing the serious shuttle effect of the C-l2 positive electrode. Figure 7 As shown in b, the SEM image of the zinc negative electrode shows a clean, flat surface and fewer by-products after 1000 cycles of the zinc-iodine battery assembled with the Co-NC-l2 positive electrode. The results show that the iodine host based on Co-NC-l2 can effectively inhibit the shuttle effect, prevent the corrosion of the zinc negative electrode by polyiodides and the occurrence of side reactions, thereby realizing a very stable, long-lasting and shuttle-free Zn-I2 battery.

[0057] Figure 6 In-situ Raman at 0.3C. Figure 7 SEM images of dendrites on the zinc negative electrode surface after (a) C-l2 and (b) Co-NC-I2 cycles for 1000 times.

[0058] Therefore, the combination of electrochemistry and in situ Raman spectroscopy demonstrates that Co-NC can effectively confine polyiodides within the abundant micro-mesopores, thereby preventing their significant leakage and shuttling during the discharge / charge process. More impressively, the embedded Co can serve as an electrocatalytic site to promote the fast redox reaction of iodine chemistry ( Figure 8 ). The synergistic effect of these two advantages contributes to the excellent electrochemical performance of Zn-L2 batteries.

[0059] Figure 8Schematic diagram of the principle of rechargeable Zn-l2 battery based on Co-NC positive electrode.

[0060] Electrochemical performance characterization:

[0061] The cyclic voltammetry (CV) curves of C-l2, NC-l2 and Co-NC-l2 are shown in Fig. 9 The fast redox kinetics of the zinc-iodine battery was verified by using C as the conductive carrier and the scan rate was 0.5 mV s -1 , a fuzzy redox peak with large voltage polarization was observed for the zinc-iodine battery assembled by C-l2, demonstrating a slow dynamic process, while the redox peak polarization of the zinc-iodine battery assembled by Co-NC-l2 was small, with the redox peak center at approximately 1.26 / 1.31 V and a potential difference as small as 40 mV, showing better reversibility. Fig. 9 b shows the starting potentials of the three electrodes according to the first CV curve. The positive electrode starting potential of the Co-NC-l2 electrode is 1.53V, which is greater than that of C-l2 (1.36V) and NC / I2 (1.50V). The zinc-iodine battery assembled by Co-NC-l2 has a smaller overpotential and faster reaction kinetics. In addition, the Tafel slopes of the three electrodes like Fig. 9 c, obtained from the CV curve. The Tafel slopes of the zinc-iodine batteries assembled by C-I2, NC-l2 and Co-NC-l2 in the reduction reaction are 234, 114 and 105 mV dec, respectively. -1 , the Co-NC-l2 cathode has the lowest Tafel slope among the three electrodes during the cathode reaction. The above results show that Co-NC has the fastest reaction kinetics, the best reversibility, the smallest polarization voltage and the largest peak area, which indicates that it has the ability to increase the redox kinetics of polyiodides.

[0062] Fig. 9 C, NC and Co-NC (a) at 0.5 mV s -1 CV curves, (b) the starting potentials of the positive and negative electrode reactions of CV, and (c) the Tafel slope calculated based on CV; at 0.5 mV s -1 Overlap test of the first 4 cycles of CV curves of (d) C, (e) NC and (f) Co-NC.

[0063] like Fig. 9 As shown in Figure df, the CV overlap experiment of zinc-iodine batteries assembled with C-l2, NC-l2 and Co-NC-l2 found that there was a pair of obvious redox peaks near 1.25V, and compared with the zinc-iodine battery assembled with C-I2, the zinc-iodine battery assembled with Co-NC-l2 had better overlap, proving that Co-NC has smaller polarization, better reversibility and faster reaction kinetics.

[0064] Influenced by the catalysis of cobalt-nitrogen doped carbon materials, we used zinc-iodine batteries assembled with C-l2, NC-I2 and Co-NC-I2 positive electrodes to conduct rate tests on the batteries. Fig.10 As shown in a, the Co-NC-I2 cathode reaches 201.1, 184.9, 177.1, 172.8, 157.3, 145.1, 133.2, and 121.8 mAh g at 2C, 5C, 8C, 10C, 20C, 30C, 40C, and 50C, respectively. -1 The NC-l2 and C-l2 cathodes reached 160.4 and 64.8 mAh g at 10C. -1 The capacity of NC-I2 cathode at high rate 50C is higher than that of Co-NC-I2 cathode. We believe that this is because the iodine loading is too low, while the iodine loading of Co-NC-l2 is much higher than that of NC-l2 cathode. In fact, the real capacity is partly provided by carbon. Since we fill in the iodine loading mass when testing the amount of active substances, carbon also provides a certain capacity in the case of trace iodine, which is higher than that of Co-NC-I2 cathode. At high rate current, Co-NC-I2 achieves a stable high coulombic efficiency, which is higher than C-l2 and NC-l2, highlighting the importance of catalysis.

[0065] The constant current charge and discharge (GCD) curves of Co-NC-I2 batteries at different rates (2C-50C) are shown in Figure 2. Fig.10 As shown in b. With the increase of rate, the specific capacity of Co-NC-l2 cathode shows little attenuation and has a uniform and clear charge and discharge platform, which is consistent with the CV curve. The above shows that Co-NC-l2 has high reversibility and more efficient iodine redox conversion.

[0066] Fig.10 (a) Rate performance of C, NC and Co-NC at different currents; (b) Charge and discharge curves of Co-NC at different currents.

[0067] The self-discharge of the battery was explored by static tests. The open circuit voltage of Co-NC-l2 provided ultrahigh stability for about 48 h at a higher voltage, thus indicating that the dissolution and shuttling of polyiodides can be well suppressed. Fig.11 As shown, the voltage difference of the Co-NC-l2 battery is stable at 0.57V, while the voltage differences of the C-l2 and NC-l2 batteries are 0.76V and 0.62V, indicating that the self-discharge of the Co-NC-l2 battery is well suppressed. In contrast, the C-l2 and NC-l2 batteries show significant self-discharge.

[0068] Fig.11 The self-discharge (time-voltage curve) of C, NC and Co-NC after standing for 48 hours.

[0069] Zn-iodine batteries assembled with C-l2, NC-l2 and Co-NC-l2 cathodes were tested at 5C to investigate the cycling stability ( Fig.12 a). Obviously, at a current of 5C, compared with C-l2 (77.1 mAhg -1 ) and NC-l2 (150.8mAh g -1 Compared with the zinc-iodine battery assembled with the positive electrode of Co-NC-l2, the zinc-iodine battery assembled with the positive electrode of Co-NC-l2 has a high efficiency of 183.6 mAh g -1 The Coulombic efficiency of 96% verifies the excellent reversibility of the Co-NC-l2 electrode. At the same time, the Co-NC-l2 electrode also has excellent stable cycle performance and high specific capacity. The charge and discharge curves of C-l2, NC-l2 and Co-NC-l2 batteries are shown in Figure 2. Fig.12 As shown in Figure b. After 1000 cycles, the charge and discharge platform of the zinc-iodine battery assembled with C and NC positive electrodes is significantly reduced. The voltage polarization of the zinc-iodine battery assembled with C positive electrode (159mV) and the voltage polarization of the zinc-iodine battery assembled with NC positive electrode (140mV) are much larger than that of the zinc-iodine battery assembled with Co-NC positive electrode (75mV), indicating that Co-NC has smaller polarization and faster redox reaction kinetics. Fig.12 As shown in c, Co-NC-l2 achieved 20,000 stable cycles at an ultra-high current of 50C and was able to provide 102 mAh g -1 The reversible capacity of 2.5 W is 0.1 W, indicating its extraordinary cycle stability.

[0070] The constant current charge-discharge (GCD) curves of zinc-iodine batteries assembled with C-l2, NC-l2 and Co-NC-l2 positive electrodes at different cycles (100, 200, 500, 800, 1000) are shown in Figure 2. Fig.12 As shown in Figure 1, the capacity decay of the zinc-iodine battery assembled with Co-NC-l2 positive electrode is small at different cycles, and the capacity decay is not obvious with the increase of cycle number, while the zinc-iodine battery assembled with NC-l2 positive electrode decays seriously after 500 cycles, and the zinc-iodine battery assembled with C-l2 positive electrode decays obviously from beginning to end. Therefore, Co-NC-l2 has high reversibility and stable cyclability.

[0071] Fig.12 (a) Cycling performance of C, NC and Co-NC at 5C, (b) charge and discharge curve of the 800th cycle at 5C; (c) long cycle performance of Co-NC at 50C; charge and discharge curves of different cycles at 5C (d) Co-NC, (e) NC and (f) C.

[0072] The present invention aims to solve the problems of low conductivity, easy sublimation and severe shuttling effect of multiple iodides of iodine. By using metal doping to enhance the catalytic effect, a cobalt-nitrogen doped carbon material is prepared, thereby accelerating the conversion of iodine redox and improving the electrochemical performance:

[0073] (1) A cobalt-nitrogen doped carbon material (Co-NC) was prepared by introducing metal elements with higher catalytic activity through the template method for application in aqueous zinc-iodine batteries. The test results show that the N-anchored Co active site exhibits high catalytic activity for the I2 / l- electrochemical reaction process, with the lowest Tafel slope (16.7 mV dec) in the oxidation / reduction process. -1 / 98mVdec -1 ), and CV showed that Co-NC had only a 40mV voltage difference. The overlap degree of Co-NC in the overlapping CV experiment was the highest, which better confirmed its optimal reversible conversion.

[0074] (2) In situ Raman spectroscopy confirmed the reaction kinetics of iodine species. Ex situ SEM testing of the cycled battery revealed that the surface of the zinc negative electrode of the zinc-iodine battery assembled with Co-NC was smooth and flat, indicating that the material can inhibit the growth of zinc dendrites and the shuttling effect of multiple iodides, and enhance the adsorption and conversion of iodine species. The capacity of Co-NC at a current of 5C is 185 mAh g -1 , it can stably cycle 20,000 times at a current of 50C, and the voltage drop is minimal in the 48h self-discharge experiment.

[0075] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a cobalt-nitrogen doped carbon positive electrode material for a zinc-iodine battery, characterized in that: include, (1) mixing a carbon source, a nitrogen source and manganese carbonate uniformly, heating to 800-850° C., washing and drying to obtain an NC material; (2) mixing the NC material obtained in step (1) with a cobalt salt, drying the obtained mixture, heating it to 800-850° C., filtering, washing, and drying to obtain a Co-NC material; (3) The Co-NC material obtained in step (2) is mixed with iodine, ground, heated to 110-130° C. in an inert atmosphere for reaction, and then heated in air to remove iodine to obtain a positive electrode material.

2. The method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to claim 1, characterized in that: In step (1), the carbon source includes methyl cellulose, and the nitrogen source includes urea.

3. The method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to claim 1 or 2, characterized in that: In step (1), the mass ratio of the carbon source, the nitrogen source and the manganese carbonate is 1:0.5 to 1:5 to 10.

4. The method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to claim 1 or 2, characterized in that: In step (1), the temperature is raised at 5°C min under an inert atmosphere. -1 Heat to 250℃ and keep warm for 1-2h, then heat at 5℃min. -1 Raise the temperature to 800℃ and keep it for 2 to 3 hours.

5. The method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to claim 1 or 2, characterized in that: In step (2), the cobalt salt includes cobalt nitrate hexahydrate, and the mass ratio of the NC material to the cobalt salt is 1:0.

97.

6. The method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to claim 1 or 2, characterized in that: In step (2), the temperature is raised at 10°C min under an inert atmosphere. -1 Heat to 130℃ and keep warm for 3-4h, then heat at 5℃min -1 Raise the temperature to 800℃ and keep it for 2 to 3 hours.

7. The method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to claim 1 or 2, characterized in that: In step (3), the mass ratio of the Co-NC material to the iodine element is 1:

1.

8. The method for preparing the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries according to claim 1 or 2, characterized in that: In step (3), the inert atmosphere includes argon; the heating to 110-130°C for reaction is heating to 120°C for reaction for 8-10 hours; the heating in air is heating to 100°C in air and keeping warm for 12-24 hours.

9. The cobalt-nitrogen doped carbon positive electrode material for zinc-iodine battery prepared by the preparation method according to claim 1.

10. Application of the cobalt-nitrogen doped carbon positive electrode material for zinc-iodine batteries prepared by the preparation method according to claim 1 in zinc-iodine batteries.

Citation Information

Patent Citations

  • High-stability zinc-iodine battery positive electrode composite material as well as preparation method and application thereof

    CN113036144A

  • Amorphous carbon material with multi-layer gradient microstructure as well as preparation method and application of amorphous carbon material

    CN114512646A

  • Nitrogen-doped porous carbon felt material and application thereof in zinc-based flow battery

    CN114583182A

  • Preparation method of M-coated N-C catalyst applied to zinc-iodine battery as well as product and application of M-coated N-C catalyst

    CN118198356A

  • Group 3 nitride epitaxy wafer for HEMT power semiconductors and manufacturing method thereof

    KR102823966B1

Cited By

  • S, n co-doped carbon material for positive electrode of four-electron zinc-iodine battery and preparation method thereof