Preparation method and application of selective adsorbent for magnesium-lithium separation
By grinding, pretreating and activation of the layered chain silicate, selective adsorption sites are constructed, and the problems of small adsorption amount and poor selection adsorption properties of natural layered chain silicate are solved, and magnesium lithium in salt lake brine are realized Reuse of selective adsorbents for efficient separation and magnesium lithium separation.
Patent Information
- Application Number
- CN202410994115.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the adsorption amount of natural layer chain silicate is small and the selective adsorption property is poor, making it difficult to effectively use magnesium lithium separation in salt lake brine, resulting in difficulty in separation of magnesium lithium.
By grinding, pretreating and activating the layered chain silicate, selective adsorption sites are constructed, nanopores are unblocked and expanded, and a selective adsorbent separation of magnesium lithium with selective adsorption and high adsorption amount is prepared.
The efficient separation of magnesium lithium in the salt lake brine was achieved. The adsorbent of the prepared adsorbent to magnesium ions reached 17-35 mg/g, the separation coefficient of magnesium lithium reached 100-600, and the adsorbent can be recycled.
Smart Images

Figure CN118949920A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adsorption materials, and specifically relates to a preparation method and application of a magnesium-lithium separation selective adsorbent. Background Art
[0002] As the lightest alkali metal, metallic lithium plays an important role in many fields due to its unique properties, such as batteries, thermonuclear fusion, and medical drugs. my country's salt lake brine-type lithium resources account for more than 80% of the total reserves, and salt lake brine-type lithium resources have gradually become the main source of lithium resources. However, the separation of magnesium and lithium in the process of lithium extraction from salt lakes has always been a core problem. The most fundamental reason for the difficulty in separating the two is that magnesium and lithium have similar physical and chemical properties, especially Mg. 2+ and Li + The hydration radii of and
[0003] In recent years, the research on lithium extraction from salt lake brine has progressed rapidly, and many technologies have been rapidly developed, such as extraction, precipitation, electrochemical method, ion sieve adsorption and membrane separation. Among them, the more commonly used methods are adsorption and membrane separation. The membrane separation method can achieve precise separation of monovalent and divalent ions on a microscopic scale by designing and regulating the membrane structure, but the cost of membrane separation is high, and there are problems of pore clogging and short service life. The adsorption method mainly enriches lithium through a highly selective lithium ion sieve adsorbent, and utilizes the selectivity of the adsorbent for lithium ions to extract Li from the solution. + The key to this method is to develop selective adsorbents with excellent performance. Ion sieve adsorbents can combine with target ions to form a stable crystal structure due to their specific void structure, and their narrow void position can limit the entry of other ions, thus showing selective adsorption and screening effects on target ions. However, traditional lithium ion sieves usually have to be synthesized under specific conditions using two or more pure chemical substances. The synthesis conditions are often harsh, often high-temperature hydrothermal synthesis with a long synthesis cycle, and there will be problems such as dissolution of specific elements.
[0004] Compared with synthetic adsorbent materials, layered silicate minerals such as palygorskite and sepiolite are abundant in reserves, low in price, environmentally friendly, and have nanopores and abundant surface functional groups, as well as isomorphous substitution and permanent negative charge on the surface, and are widely used in adsorption. However, natural palygorskite and sepiolite have defects such as easy aggregation and narrow pores that are difficult to enter, resulting in small adsorption capacity and poor selective adsorption, so they are difficult to be directly applied to lithium extraction from salt lake brine. Summary of the invention
[0005] In order to overcome the problems of small adsorption capacity and poor selective adsorption of natural layered chain silicates in the prior art, the present invention provides a preparation method and application of a selective adsorbent for magnesium-lithium separation, wherein the structure of layered chain silicate minerals is regulated by activation treatment, selective adsorption sites are constructed, and nanopores are dredged and expanded at the same time, thereby preparing an adsorbent with selective adsorption for magnesium ions and a high adsorption capacity, thereby realizing magnesium-lithium separation in salt lake brine.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a selective adsorbent for magnesium-lithium separation comprises the following steps:
[0008] (S1) grinding: grinding and sieving the layered silicate to obtain a layered silicate powder;
[0009] (S2) Pretreatment: adding layered silicate powder and dispersant to water for ultrasonic treatment, allowing to stand, taking the upper suspension, centrifuging and drying to obtain pretreated powder;
[0010] (S3) Activation: adding the pretreated powder to an inorganic acid solution with a hydrogen ion concentration of 0.1 to 4 M, activating under heating conditions, and separating, washing, drying, and sieving after the activation to obtain a magnesium-lithium separation selective adsorbent;
[0011] Wherein, the magnesium content of the layered chain silicate in step (S1) is 7-15wt%; and the total content of magnesium, aluminum and iron is 10-30%.
[0012] Layered chain silicate is a 2:1 type layered chain octahedral mineral with a nanoporous structure. After activation in an inorganic acid solution, the nanopores of the layered chain silicate are unblocked and expanded, which is conducive to the diffusion of adsorbed ions and enhances its adsorption capacity. At the same time, the Mg in the octahedral structure 2+ 、Al 3+ , Fe 2+ The plasma will partially dissolve, thus constructing octahedral vacancy defects, among which magnesium vacancy defects are more numerous and are similar in size, charge and energy to Mg in the solution. 2+ Highly consistent, thus showing a strong Mg 2+ Selective adsorption and high Mg 2+Adsorption amount. The inventors have found through research that after the layered silicate with a magnesium content of 7-15wt% and a total content of magnesium, aluminum and iron of 10-30% is activated in an inorganic acid solution with a hydrogen ion concentration of 0.1-4M, the residual octahedron with vacancy defects is still stable and has a supporting effect, so that the activated layered silicate still has an octahedral layer structure, avoiding structural collapse. The magnesium content in the layered silicate, the total content of magnesium, aluminum and iron, and the activation conditions must be within a certain range. If it is too low, it will cause limited vacancy defects and thus low adsorption; if it is too high, it will cause excessive dissolution, and too many vacancy defects will cause the octahedral structure to collapse. In summary, the selective adsorbent for magnesium-lithium separation prepared by layered silicates with specific element contents under specific activation conditions has a stable structure and more adsorption sites, and thus has the ability to selectively adsorb Mg. 2+ And high adsorption capacity.
[0013] Furthermore, the layered chain silicate in step (S1) is selected from at least one of magnesium-rich palygorskite and sepiolite; preferably magnesium-rich palygorskite.
[0014] Furthermore, in step (S1), the screening is through a 100-400 mesh sieve.
[0015] Furthermore, in step (S2), the dispersant is selected from at least one of sodium hexametaphosphate, sodium tripolyphosphate, and sodium pyrophosphate; the amount of the dispersant is 0.5-1.5wt% of the layered silicate powder; the ultrasound is for 3-6 hours; the standing is for 1-2 hours; and the drying is for 12-36 hours at 60-110°C.
[0016] Impurities such as quartz can be removed through grinding and pretreatment, and the dissociation of crystal bundles can be promoted, which can promote the subsequent activation effect.
[0017] Furthermore, in step (S3), the inorganic acid solution is selected from one of hydrochloric acid solution, sulfuric acid solution and phosphoric acid solution.
[0018] Furthermore, in step (S3), the hydrogen ion concentration in the inorganic acid solution is 1 to 4M.
[0019] During the activation process, if the hydrogen ion concentration in the inorganic salt solution is too low, the magnesium, aluminum, and iron will dissolve less, resulting in fewer vacancy defects in the layered silicate, and thus its adsorption amount will be low; if the hydrogen ion concentration in the inorganic salt solution is too high, the magnesium, aluminum, and iron will dissolve too much, resulting in too many vacancy defects in the layered silicate, and too many vacancy defects will cause the octahedral structure to collapse.
[0020] Furthermore, in step (S3), the ratio of the pretreated powder to the inorganic acid solution is 1 g: 15-30 ml.
[0021] Furthermore, in step (S3), the activation under heating conditions is carried out at 60-80° C. for 5-8 hours.
[0022] The separation, washing, drying and screening are well known to those skilled in the art. For example, separation is by centrifugation or filtration; washing is by washing until neutral; drying is by drying at 60-110° C. for 12-36 hours; and screening is by screening through a 200-400 mesh sieve.
[0023] For ease of use, the magnesium-lithium separation selective adsorbent prepared by the above preparation method can be subjected to molding treatment, including granulation and film formation. Granulation and film formation techniques are well known to those skilled in the art.
[0024] After the magnesium ions are adsorbed, the crystal structure of the magnesium-lithium separation selective adsorbent prepared by the preparation method of the present invention can be partially restored to that before activation. Therefore, after the magnesium ions are adsorbed and subjected to a de-magnesium treatment, the magnesium-lithium separation selective adsorbent can be repeatedly recycled.
[0025] In a second aspect, the present invention provides the use of the magnesium-lithium separation selective adsorbent prepared by the above preparation method in the separation of magnesium and lithium in the process of lithium extraction from salt lake brine.
[0026] Furthermore, the application is: at a pH of 9 to 10, the above-mentioned magnesium-lithium separation selective adsorbent is added to salt lake brine for adsorption for 24 to 48 hours.
[0027] Furthermore, the application also includes: vibrating and adsorbing the above-mentioned magnesium-lithium separation selective adsorbent, then performing a magnesium removal treatment, and then repeatedly recycling it; the specific process of the magnesium removal treatment is: washing the adsorbed magnesium-lithium separation selective adsorbent with water to neutrality, drying it in an oven, and then adding it to a dilute acid, and after oscillating for 8 to 12 hours, the product is washed with water and dried at 60 to 90° C. to obtain a solid powder, that is, the magnesium-lithium separation selective adsorbent after magnesium removal, thereby completing the magnesium removal process.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] First, the Mg content of the octahedron can be activated by heating a layered chain silicate having a magnesium content of 7 to 15 wt% and a total content of magnesium, aluminum and iron of 10 to 30% in an inorganic acid solution having a hydrogen ion concentration of 0.1 to 4 M. 2+ 、Al 3+ , Fe 2+ Partial dissolution produces more octahedral vacancies, thus constructing Mg 2+ selective adsorption sites; at the same time, the stability of the layered chain structure is maintained, and finally a magnesium-lithium separation selective adsorbent with stability and high adsorption capacity is prepared. 2+The adsorption capacity reaches 17-35 mg / g, and the magnesium-lithium separation coefficient reaches 100-600, realizing the enrichment and extraction of lithium resources and the efficient recovery of magnesium resources; among which the preferred embodiment has an adsorption capacity of magnesium ions of more than 30 mg / g, and a magnesium-lithium separation coefficient of 300-600.
[0030] 2. After the magnesium ions are adsorbed, the crystal structure of the magnesium-lithium separation selective adsorbent prepared by the preparation method of the present invention can be partially restored to that before activation. Therefore, after the magnesium ions are adsorbed, the adsorbent is subjected to de-magnesium treatment and can be repeatedly recycled. The adsorption capacity of the fifth cycle can still reach more than 80% of the first cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is the SEM picture of the magnesium-lithium separation selective adsorbents HPlg-1, HPlg-2 and HPlg-4 prepared in the examples.
[0032] Figure 2 It is the SEM pictures of the magnesium-lithium separation selective adsorbents HSep-1, HSep-2 and HSep-4 prepared in the examples.
[0033] Figure 3 The HP1g series of magnesium-lithium separation selective adsorbents prepared in the examples are Mg 2+ Histogram of adsorption amount.
[0034] Figure 4 The Hsep series of magnesium-lithium separation selective adsorbents prepared in the examples are Mg at different pH values. 2+ Histogram of adsorption amount.
[0035] Figure 5 This is a bar graph of the adsorption amount of each ion by the magnesium-lithium separation selective adsorbent HPlg-1 prepared in Example 3 at a pH of 10.
[0036] Figure 6 This is a bar graph of the adsorption amount of each ion by the magnesium-lithium separation selective adsorbent HSep-0.5 prepared in Example 7 at a pH of 10.
[0037] Figure 7 The magnesium-lithium separation selective adsorbent HPlg-1 prepared in Example 3 is used for adsorbing Mg 2+ XRD patterns before and after.
[0038] Figure 8 The magnesium-lithium separation selective adsorbent HSep-0.5 prepared in Example 7 is effective in adsorbing Mg 2+ XRD patterns before and after.
[0039] Fig. 9The magnesium-lithium separation selective adsorbent HP1g-1 prepared in Example 3 at pH 10 is 2+ Cyclic adsorption histogram.
[0040] Fig.10 The Mg content of the magnesium-lithium separation selective adsorbent HSep-0.5 prepared in Example 7 at pH 10 is 2+ Cyclic adsorption histogram. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] In the examples of the present invention, unless otherwise specified, all reagents used are commercially available in the art.
[0043] Magnesium-rich palygorskite (Plg) is produced in Xuyi, Jiangsu Province. The main element content is:
[0044] Element Si Mg Al Fe Ca Ti O Content (wt%) 30.78 8.49 5.37 3.98 1.27 0.43 48.26
[0045] Magnesium-rich sepiolite (Sep) is produced in Shijiazhuang, with the following main elements:
[0046] Element Si Mg Ca Fe Na K O Content (wt%) 21.08 10.41 0.70 0.30 0.02 0.02 65.97
[0047] The origin of magnesium-poor palygorskite is Linze, Gansu Province. The main element content is:
[0048] Element Si Mg Al Fe Ca Ti O Content (wt%) 24.50 2.51 7.43 5.27 8.43 0.61 49.55
[0049] Example 1
[0050] A method for preparing a selective adsorbent for magnesium-lithium separation comprises the following steps:
[0051] (S1) grinding: grinding magnesium-rich palygorskite (Plg) and passing it through a 200-mesh sieve to obtain magnesium-rich palygorskite powder;
[0052] (S2) Pretreatment: 20 g of magnesium-rich palygorskite powder and 0.2 g of dispersant sodium hexametaphosphate were added to water for ultrasonic treatment for 3 h, and then allowed to stand for 1 h. The upper suspension was centrifuged and dried at 80° C. for 24 h to obtain the pretreated powder;
[0053] (S3) Activation: 5 g of the pretreated powder was added to 100 mL of 0.1 M hydrochloric acid solution and reacted at 60° C. for 8 h. After the reaction, the mixture was centrifuged, washed alternately with ethanol and deionized water until neutral, dried at 80° C. for 24 h, and passed through a 200-mesh sieve to obtain a selective adsorbent for magnesium-lithium separation, recorded as HP1g-0.1.
[0054] Example 2
[0055] The rest is the same as Example 1, except that the concentration of the hydrochloric acid solution in step (S3) is 0.5M, the activation temperature is 70°C, and the time is 6h; the obtained magnesium-lithium separation selective adsorbent is recorded as HPlg-0.5.
[0056] Example 3
[0057] The rest is the same as Example 1, except that the concentration of the hydrochloric acid solution in step (S3) is 1 M, the activation temperature is 80° C., and the activation time is 5 h; the obtained magnesium-lithium separation selective adsorbent is recorded as HPlg-1.
[0058] Example 4
[0059] The rest is the same as Example 1, except that the concentration of the hydrochloric acid solution in step (S3) is 2M, the activation temperature is 80°C, and the time is 5h; the obtained magnesium-lithium separation selective adsorbent is recorded as HPlg-2.
[0060] Example 5
[0061] The rest is the same as Example 1, except that the concentration of the hydrochloric acid solution in step (S3) is 4M, the activation temperature is 80°C, and the time is 5h; the obtained magnesium-lithium separation selective adsorbent is recorded as HPlg-4.
[0062] SEM images of Plg, HPlg-1, HPlg-2, and HPlg-4 are shown in Figure 1 HPlg-1 adsorbs Mg 2+ The XRD patterns before and after are as follows Figure 7 As shown, HPlg-1 adsorbs Mg 2+ It is hereinafter referred to as XPlg, and the raw material magnesium-rich palygorskite before activation is referred to as Plg.
[0063] Example 6
[0064] The rest is the same as Example 1, except that in step (S1), sepiolite (Sep) is used instead of magnesium-rich palygorskite, and the obtained magnesium-lithium separation selective adsorbent is recorded as HSep-0.1.
[0065] Examples 7-10
[0066] The rest is the same as Example 6, except that the concentrations of the hydrochloric acid solution in step (S3) are 0.5M, 1M, 2M, and 4M, respectively. Implementations 7-10 are carried out sequentially, and the obtained magnesium-lithium separation selective adsorbents are recorded as HSep-0.5, HSep-1, HSep-2, and HSep-4, respectively.
[0067] The SEM images of Sep, HSep-1, HSep-2, and HSep-4 are shown in Figure 2 The XRD patterns of HSep-0.5 before and after the adsorption of magnesium ions are shown in Figure 8 As shown, HSep-0.5 after adsorbing magnesium ions is denoted as Xsep, and the raw material sepiolite before activation is denoted as Sep.
[0068] Embodiment 11
[0069] The rest is the same as Example 1, except that in step (S3), 0.05 M sulfuric acid solution is used instead of 0.1 M hydrochloric acid solution.
[0070] Example 12
[0071] The rest is the same as Example 1, except that in step (S3), 0.033 M phosphoric acid solution is used instead of 0.1 M hydrochloric acid solution.
[0072] Comparative Example 1
[0073] The rest is the same as Example 1, except that in step (S3), the concentration of the hydrochloric acid solution is 6 M, the activation time is 10 h, and the obtained magnesium-lithium separation selective adsorbent is recorded as HP1g-6-10h.
[0074] Comparative Example 2
[0075] The rest is the same as Example 1, except that in step (S3), the concentration of the hydrochloric acid solution is 0.05 M, the activation time is 2 h, and the obtained magnesium-lithium separation selective adsorbent is recorded as HP1g-0.05-2h.
[0076] Comparative Example 3
[0077] The rest is the same as Example 1, except that magnesium-poor palygorskite is used instead of magnesium-rich palygorskite in step (S1), and the obtained magnesium-lithium separation selective adsorbent is recorded as HLP1g-0.1.
[0078] Test Case
[0079] The magnesium-lithium separation selective adsorbents prepared in the above examples and comparative examples were tested as follows:
[0080] (1) Element content test
[0081] The element content of the magnesium-lithium separation selective adsorbent prepared in each embodiment and comparative example was tested, and the results are shown in Table 1 and Table 2.
[0082] (2)Mg 2+ Adsorption test: 0.05 g of magnesium ion selective adsorbent was added to 25 mL of MgCl2 solution with different pH values (7, 8, 9, 10), and the solution was placed in an oscillator and oscillated at 250 rpm at 25 °C. After adsorption, the solid adsorbent was removed from the solution with a filter (0.22 μm), and then the Mg content in the filtrate was determined using ICP-OES. 2+ The content.
[0083] The adsorption capacity was calculated by the following formula (2-1).
[0084]
[0085] In the formula, Q e (mg / g) is the adsorption capacity, V (L) is the solution volume, M (g) is the amount of magnesium ion selective adsorbent used, C o (mg / L) and C e (mg / L) are the initial concentration and equilibrium concentration of the solution, respectively.
[0086] HPlg series magnesium and lithium separation selective adsorbents at different pH values 2+ The adsorption amount bar graph is as follows Figure 3 As shown in the figure; Hsep series magnesium-lithium separation selective adsorbent Mg at different pH 2+ The adsorption amount bar graph is as follows Figure 4 shown.
[0087] (3) Selective adsorption test: In the presence of Mg 2+ , Li + , K + , Ca 2+ and Na + The selectivity experiment was carried out in a mixed solution of 100 mg / L each. 0.05 g of magnesium ion selective adsorbent was added to 25 mL of the mixed solution, and the concentration of ions in the solution was detected by ICP-OES after oscillation for 24 hours. The separation coefficient was calculated according to the following formula:
[0088]
[0089] Where K d (L / g) is the distribution factor, is the separation coefficient, M represents Mg, Li, K, Ca and Na respectively; where Q e (mg / g) is the adsorption capacity, C e(mg / L) are the equilibrium concentrations of the solutions, respectively.
[0090] When the pH value is 10, the selective adsorbent for separation of magnesium and lithium prepared in the examples and comparative examples has a high affinity for Mg 2+ , Li + The calculated results of the adsorption amount are shown in Table 3. The bar graph of the adsorption amount of each ion by the ion selective adsorbent HP1g-1 prepared in Example 3 is shown in Table 3. Figure 5 As shown; the bar graph of the adsorption amount of each ion by the magnesium-lithium separation selective adsorbent HSep-0.5 prepared in Example 7 is as follows Figure 6 shown.
[0091] (4) Cyclic performance test: The magnesium-lithium separation selective adsorbent HP1g-1 prepared in Example 3 and the magnesium-lithium separation selective adsorbent HSep-0.5 prepared in Example 7 were subjected to the first adsorption of Mg 2+ Then, de-magnesium treatment was performed. The specific process was as follows: HPlg-1 and HSep-0.5 were washed with pure water until neutral, dried in an oven, and then added to 0.1M dilute hydrochloric acid. After oscillation for 12 hours, the product was washed with pure water and dried at 90°C to obtain a solid powder. 2+ The de-magnesiumized HPlg-1 and HSep-0.5 were added to a MgCl2 solution with a pH of 10 to determine their absorption / desorption of Mg 2+ The adsorption amount was increased and the cycle was repeated 5 times.
[0092] Results and Analysis
[0093] SEM image analysis
[0094] Figure 1 1 is a SEM image of the magnesium-lithium separation selective adsorbents HP1g-1, HP1g-2 and HP1g-4 prepared in the examples; Figure 2 HSep-1, HSep-2 and HSep-4 are SEM images of the magnesium-lithium separation selective adsorbents prepared in the examples. Figure 1 It can be seen that in the original state, the palygorskite rod crystals are stacked into dense nested aggregates, which are severely agglomerated and difficult to dissociate. Therefore, the specific surface area of the palygorskite ore is small and the adsorption performance is also affected. As the concentration of inorganic acid increases from 0.1M to 4M, the surface of the palygorskite aggregates is gradually dissolved, the impurities are gradually dissolved, and it can be clearly observed that the rod-shaped individuals are gradually presented, and the rod crystals are arranged neatly. Figure 2 It can be seen that the original sepiolite presents a slender nanofiber structure, with the fiber length reaching several microns or even tens of microns, the diameter of a single fiber bundle is about 0.1μm, the overall fiber structure is symmetrical and uniform, and the crystallinity is good; the sepiolite fiber structure after inorganic acid activation is partially dissolved, the edges are corroded and broken, the overall length of the fiber becomes shorter, and the surface becomes rough.
[0095] Element change analysis
[0096] The magnesium content of the selective adsorbents for separation of magnesium and lithium prepared in each embodiment and comparative example was tested, and the results are shown in Table 1 and Table 2.
[0097] Table 1 Main element content of magnesium-lithium separation selective adsorbent HPlg (Wt.%)
[0098]
[0099]
[0100] The metal elements in magnesium-rich palygorskite (Plg) are mainly magnesium, aluminum, and iron. As can be seen from Table 1, the magnesium content of the HPlg series magnesium-lithium separation selective adsorbent prepared in the embodiment is reduced from 8.49wt% of the raw material to 1-7.5wt%, and the total content of magnesium, aluminum, and iron is reduced from 17.84wt% of the raw material to 3.5-16wt%, that is, magnesium, aluminum, and iron are partially dissolved. The magnesium content of the magnesium-lithium separation selective adsorbent prepared in Comparative Example 1 is only 0.45wt%, and the total content of magnesium, aluminum, and iron is only 2.36wt%, which are lower than those in the embodiment, that is, compared with the embodiment, the magnesium, aluminum, and iron of Comparative Example 1 are more dissolved. The magnesium content of the magnesium-lithium separation selective adsorbent prepared in Comparative Example 2 is relatively high, which is only reduced from 8.49wt% of the raw material to 8.10wt%, and the total content of magnesium, aluminum, and iron is only reduced from 17.84wt% of the raw material to 17.14wt%, that is, compared with the embodiment, the magnesium, aluminum, and iron in Comparative Example 2 are less eroded, so the prepared magnesium-lithium separation selective adsorbent has fewer vacancy defects. Comparative Example 3 uses magnesium-poor palygorskite to prepare a magnesium-lithium separation selective adsorbent, and the magnesium content is only reduced from 2.51wt% of the raw material to 1.82wt%, indicating that the amount of magnesium erosion is less, so the magnesium vacancies generated are less, which may be due to the Mg in the magnesium-poor palygorskite. 2+ / (Al 3+ +Fe 3+ ) ratio is relatively low, and it is not easily activated by acid relative to magnesium-rich palygorskite.
[0101] Table 2 Main element content of magnesium-lithium separation selective adsorbent HSep (Wt.%)
[0102]
[0103] The metal element in Sepiolite (Sep) is mainly magnesium. As can be seen from Table 2, the magnesium content of the HSep series magnesium-lithium separation selective adsorbent prepared in the example is reduced from 10.41wt% of the raw material to 1-7.5wt%.
[0104] Based on Table 1 and Table 2, the magnesium content of the HP1g and HSep series magnesium-lithium separation selective adsorbents prepared in the examples can be maintained at 1-7.5wt%.
[0105] Adsorption performance analysis
[0106] Figure 3 The Mg content of HPlg, a selective adsorbent for separation of magnesium and lithium, at different pH values 2+ Adsorption amount bar graph; Figure 4 The Mg content of Hsep, a selective adsorbent for separation of magnesium and lithium, at different pH values 2+ Adsorption amount bar graph. Figure 3 and Figure 4 It can be seen that the magnesium-lithium separation selective adsorbent prepared by the preparation method of the present invention has a high selectivity to Mg at a pH of 9 to 10. 2+ It has a high adsorption capacity, which is above 15 mg / g. The Mg 2+ The adsorption capacity is about 35 mg / g. At the same time, it can be seen that pH has a great influence on the adsorption capacity. When the pH is 7-8, the adsorption capacity of the adsorbent is low; and as the pH increases, the adsorption capacity increases sharply, indicating that the alkaline environment is conducive to Mg 2+ This is determined by the characteristics of palygorskite and sepiolite. The surface of palygorskite and sepiolite is negatively charged. Under alkaline conditions, the surface charge density is higher, which is more sensitive to Mg 2+ However, when the pH exceeds 10, Mg(OH)2 precipitation will form.
[0107] Figure 5 is a bar graph of the adsorption capacity of various ions of the magnesium-lithium separation selective adsorbent HP1g-1 prepared in Example 3 at a pH of 10; Figure 6 HSep-0.5 is a bar graph showing the adsorption capacity of various ions when pH is 10. Figure 5 As can be seen, HPlg-1 has an effect on Mg 2+ The adsorption capacity is 33.15 mg / g, which is much higher than other ions. The selectivity order of each ion is Mg 2+ >>Ca 2+ >Na + >Li + >K + .from Figure 5 As can be seen, HSep-0.5 has a significant effect on Mg 2+ The adsorption capacity is 25.75 mg / g, which is much higher than other ions. The selectivity order of each ion is Mg 2+ >>Ca 2+ >Na + >K + >Li + .
[0108] When the pH is 10, the adsorption amount and separation coefficient of magnesium and lithium by the magnesium-lithium separation selective adsorbent prepared in each embodiment and comparative example are shown in Table 3.
[0109] Table 3 Magnesium-lithium adsorption and magnesium-lithium separation coefficient
[0110]
[0111]
[0112] It can be seen from Table 3 that the HPlg and Hsep series of magnesium-lithium separation selective adsorbents prepared by the preparation method of the present invention have an adsorption capacity of 17 to 35 mg / g for magnesium ions at pH 10, and a magnesium-lithium separation coefficient of 100 to 600, wherein the preferred embodiment has an adsorption capacity of more than 30 mg / g for magnesium ions, and a magnesium-lithium separation coefficient of 300 to 600. Combining the data of Tables 1 and 2, it can be seen that the magnesium content of the HPlg and HSep series of magnesium-lithium separation selective adsorbents prepared by the embodiments of the present invention is maintained at 1 to 7.5 wt %. This may be because they have more vacancy defects and thus construct more selective adsorption sites while still having stability and the octahedral structure does not collapse, and the prepared magnesium-lithium separation selective adsorbent has high Mg 2+ high adsorption capacity and high magnesium-lithium separation coefficient.
[0113] Compared with Example 1, the adsorbent HSep-6-10h prepared in Comparative Example 1 has a higher 2+ The adsorption capacity and magnesium-lithium separation coefficient are significantly lower; combined with the data in Table 1, the magnesium, aluminum and iron in Comparative Example 1 are more dissolved, which may cause the collapse of the octahedral structure, thereby reducing the adsorption capacity and selective adsorption performance.
[0114] Compared with Example 1, the magnesium-lithium separation coefficient of the adsorbent HP1g-0.1-2h prepared in Comparative Example 2 is higher, but the magnesium-lithium separation coefficient is 2+ The adsorption capacity is low, only 7.12 mg / g; combined with the data in Table 1, the magnesium, aluminum and iron in Comparative Example 2 are less dissolved, indicating that the magnesium-lithium separation selective adsorbent prepared when the hydrochloric acid concentration is 0.1M and the activation time is 2h has fewer vacancy defects, and the nanopore dredging and expansion are limited, resulting in a low adsorption capacity.
[0115] Comparative Example 3: Effect of magnesium-lithium separation selective adsorbent prepared by magnesium-poor palygorskite on Mg 2+ The adsorption capacity and magnesium-lithium separation coefficient of the magnesium-poor palygorskite are both low, which may be due to the Mg 2+ / (Al 3+ +Fe 3+) ratio is relatively low, and it is not easy to be activated by acid compared with magnesium-rich palygorskite; at the same time, the magnesium content in magnesium-poor palygorskite is limited, and fewer magnesium vacancies are generated after activation.
[0116] Adsorption of Mg 2+ XRD pattern analysis before and after and cycle performance analysis
[0117] Figure 7 The magnesium-lithium separation selective adsorbent HPlg-1 prepared in Example 3 is used for adsorbing Mg 2+ XRD diagram before and after, HPlg-1 adsorbs Mg 2+ It is denoted as XPlg. Figure 7 As can be seen in (a), after activation with inorganic acid, the crystal structure of magnesium-rich palygorskite did not change significantly, but the intensity of its characteristic peaks weakened, while the intensity of quartz characteristic peaks increased. Figure 7 From the enlarged image of the (110) diffraction peak in (b), it can be seen that the peak position of the (110) characteristic peak shifts slightly to a higher angle after activation; this phenomenon occurs because during the inorganic acid activation, Mg 2+ With H + Ion exchange occurs due to H + The ionic radius is smaller than that of Mg 2+ The ionic radius of MgO decreases, resulting in a decrease in the unit cell parameters. 2+ When H + After being exchanged from the adsorbent, the peak position of the (110) characteristic peak shifted to a lower angle. Repeated experiments showed the same peak position shift phenomenon, that is, the adsorption of Mg 2+ The XRD pattern of HPlg-1 after MgO adsorption showed a trend of diffraction peak position recovery, indicating that HPlg-1 adsorbed Mg 2+ The structure was later partially restored.
[0118] Figure 8 The magnesium-lithium separation selective adsorbent HSep-0.5 prepared in Example 7 is effective in adsorbing Mg 2+ XRD patterns before and after HSep-0.5 is recorded as XSep after magnesium ion adsorption. Figure 8 As can be seen in (a), only the characteristic peak intensity of sepiolite changes before and after mineral acid activation and adsorption, and no other diffraction peaks are generated, indicating that the overall structure of sepiolite is still maintained after mineral acid activation and adsorption. Figure 8 From the magnified image of the (110) diffraction peak in (b), it can be seen that the (110) peak position of HSep-0.5 after activation with inorganic acid shifts slightly to a higher angle, indicating that the adsorbed Mg 2+ The XRD spectrum of HSep-0.5 after adsorption showed a trend of diffraction peak position recovery, and repeated experiments showed the same peak position shift phenomenon, indicating that HSep-0.5 adsorbed Mg2+ The structure was later partially restored.
[0119] The trend of the restoration of the diffraction peak position on the above XRD spectrum shows that the magnesium-lithium separation selective adsorbent prepared by the present invention is effective in adsorbing Mg 2+ After that, the structure is partially restored, so after adsorbing magnesium ions and undergoing de-magnesium treatment, the adsorbent can be recycled and reused. Fig. 9 is Mg of HPlg-1 2+ Cyclic adsorption amount bar graph, Fig.10 Mg for HSep-0.5 2+ Cyclic adsorption amount bar graph, from Fig. 9 and Fig.10 It can be seen that the adsorption capacity of HPlg-1 and HSep-0.5 in the fifth cycle can still reach more than 80% of the first cycle, indicating that both can be recycled and reused.
[0120] In summary, the magnesium-lithium separation selective adsorbent prepared by the preparation method of the present invention has a stable structure, high Mg 2+ Adsorption capacity and excellent Mg 2+ Selective adsorption; at the same time, since the crystal structure can be partially restored to the state before activation, the adsorbent can be repeatedly recycled after being de-magnesiumized after adsorbing magnesium ions.
Claims
1. A method for preparing a selective adsorbent for magnesium-lithium separation, It is characterized in that The following steps are involved: (S1) grinding: grinding and sieving the layered silicate to obtain a layered silicate powder; (S2) Pretreatment: adding layered silicate powder and dispersant to water for ultrasonic treatment, allowing to stand, taking the upper suspension, centrifuging and drying to obtain pretreated powder; (S3) Activation: adding the pretreated powder to an inorganic acid solution with a hydrogen ion concentration of 0.1 to 4 M, activating under heating conditions, and separating, washing, drying, and sieving after the activation to obtain a magnesium-lithium separation selective adsorbent; Wherein, the magnesium content of the layered chain silicate in step (S1) is 7-15wt%; and the total content of magnesium, aluminum and iron is 10-30%.
2. The magnesium-lithium separation selective adsorbent according to claim 1, It is characterized in that In step (S1), the layered chain silicate is selected from at least one of magnesium-rich palygorskite and sepiolite; preferably magnesium-rich palygorskite; and the screening is through a 100-400 mesh sieve.
3. The magnesium-lithium separation selective adsorbent according to claim 1, It is characterized in that In step (S2), the dispersant is selected from at least one of sodium hexametaphosphate, sodium tripolyphosphate, and sodium pyrophosphate; the amount of the dispersant is 0.5-1.5wt% of the layered silicate powder; the ultrasound is for 3-6 hours; the standing is for 1-2 hours; and the drying is for 12-36 hours at 60-110°C.
4. The magnesium-lithium separation selective adsorbent according to claim 1, It is characterized in that In step (S3), the inorganic acid solution is selected from one of hydrochloric acid solution, sulfuric acid solution and phosphoric acid solution.
5. The magnesium-lithium separation selective adsorbent according to claim 1, It is characterized in that In step (S3), the hydrogen ion concentration in the inorganic acid solution is 1 to 4M.
6. The magnesium-lithium separation selective adsorbent according to claim 1, It is characterized in that In step (S3), the ratio of the pretreated powder to the inorganic acid solution is 1 g: 15-30 ml.
7. The magnesium-lithium separation selective adsorbent according to claim 1, It is characterized in that In step (S3), the activation under heating conditions is carried out at 60-80°C for 5-8h.
8. Application of the magnesium-lithium separation selective adsorbent prepared by the preparation method according to any one of claims 1 to 7 in the separation of magnesium and lithium in the process of lithium extraction from salt lake brine.
9. The use according to claim 8, It is characterized in that The application is: adding the magnesium-lithium separation selective adsorbent into salt lake brine at a pH of 9 to 10 for adsorption for 24 to 48 hours.
10. The use according to claim 8, It is characterized in that The application also includes: vibrating and adsorbing the magnesium-lithium separation selective adsorbent, then removing the magnesium, and then repeatedly recycling it.
Citation Information
Patent Citations
Amino silane grafted and modified sepiolite adsorbent and preparation method and application thereof
CN108654578A
Method for comprehensive utilization of lithium and magnesium resources in brine of salt lake
CN109110788A
Attapulgite pretreatment method
CN110193341A
Attapulgite-based water pollution treatment adsorbent and preparation method thereof
CN116920790A