Method for preparing composite photocatalytic layer by using polydopamine

By bonding the photocatalyst with a polydopamine-zeolite composite structure, the problem of weak photocatalyst adhesion was solved, achieving highly efficient and stable photocatalytic performance and improving air purification effect.

CN118950071APending Publication Date: 2024-11-15SHAANXI FANRUIWEI PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411155856.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing photocatalysts do not adhere firmly to the support, resulting in reduced photocatalytic activity and failing to simultaneously meet the requirements of high photocatalytic activity and stability.

Method used

Polydopamine is used as a binder to form a composite structure between photocatalytic particles and zeolite. Polydopamine is used to stably bond the particles to the substrate, and the photothermal conversion properties of polydopamine are combined to improve the stability and efficiency of the photocatalyst.

Benefits of technology

It improved the stability and photocatalytic efficiency of the photocatalyst, increased the contact area between the photocatalytic particles and organic pollutants, enhanced the purification effect, and increased the degradation efficiency by 84%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950071A_ABST
    Figure CN118950071A_ABST
Patent Text Reader

Abstract

The invention relates to the field of preparation of polymers and catalytic materials, and particularly provides a method for preparing a composite photocatalytic layer by using polydopamine, which comprises the following steps: step 1, dissolving tris (hydroxymethyl) aminomethane powder in deionized water, and adding a regulator to obtain a buffer solution; dissolving dopamine hydrochloride in a buffer solution to obtain a polydopamine solution; 2, the substrate is completely immersed in the polydopamine solution, the substrate is taken out after being immersed for the first time and dried at the first preset temperature, and a polydopamine coating is formed on the surface of the substrate; 3, photocatalytic particles are taken and added into deionized water, and a solution A is obtained; adding zeolite into the solution A, and adjusting the pH value of the solution to a second preset pH value to obtain a solution B; and 4, spraying the solution B obtained in the step 3 on the substrate obtained in the step 2, and drying at a second preset temperature. The stability of the obtained photocatalytic layer is 0.91; and the purification efficiency is high, and the formaldehyde concentration is reduced by 84% after purification for 60 min.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of preparation of polymers and catalytic materials, and in particular, to a method for preparing a composite photocatalytic layer using polydopamine. Background Art

[0002] Under the irradiation of ultraviolet light or visible light, photocatalytic particles can catalyze the degradation of organic pollutants into harmless small molecules, such as carbon dioxide and water, to achieve the purpose of purifying the air; for example, titanium dioxide particles, which are usually nanometer-sized, are widely used in air purification, water treatment, self-cleaning surfaces and other fields. Since photocatalytic particles themselves have no adhesion ability and cannot be directly attached to the carrier, the stable loading of photocatalytic particles is very critical and determines the stability of photocatalytic performance and catalytic efficiency.

[0003] When in use, the photocatalytic particles need to be fixed on a carrier to form a photocatalytic layer, and a photocatalytic reaction is carried out under light to purify the air. The fixing methods of the photocatalytic particles include physical loading method and chemical loading method to prevent them from falling off during use and reducing the photocatalytic efficiency. Among them, the chemical loading method will lead to insufficient adhesion between the photocatalytic particles and the carrier, for example, they are easy to fall off in vibration, humidity and other environments, affecting their photocatalytic efficiency and service life. The applicant used a spraying method to load the photocatalytic particles onto a glass substrate, a hexagonal honeycomb aluminum filter substrate and a sandpaper substrate, and found that the photocatalyst would fall off by gently touching it with the hand; specifically, the solid loading amount was 0.22g, the drop amount was 0.09g, and the stability was only 0.59, that is, nearly 40% of the photocatalytic particles fell off, the loading effect was poor, and the vibration frequency of the vibration table was 50Hz. Using polymer materials such as polyurethane as adhesives can enhance the interaction between the carrier and the photocatalytic particles, making the photocatalytic particles less likely to fall off and improving the adhesion effect; however, the photocatalytic particles cannot come into contact with the air at the contact point between the adhesive and the photocatalytic particles, and part of the photocatalytic particles are covered by the adhesive, resulting in low activity of the photocatalytic particles and reduced photocatalytic performance.

[0004] In summary, the photocatalysts obtained by existing methods cannot simultaneously meet the requirements of high photocatalytic activity and strong adhesion. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a composite photocatalytic layer using polydopamine in view of the above-mentioned deficiencies in the prior art, so as to solve the problem that the photocatalyst obtained by the existing method cannot simultaneously meet the requirements of high photocatalytic activity and strong adhesion.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows: The present application provides a method for preparing a composite photocatalytic layer using polydopamine, the method comprising the following steps: Step 1: dissolving tris(hydroxymethyl)aminomethane) powder in deionized water, adding a regulator, and adjusting the pH value of the solution to a first preset pH value to obtain a buffer solution; dissolving dopamine hydrochloride in the buffer solution to obtain a polydopamine solution; Step 2: completely immerse the substrate in the polydopamine solution, stir it, take it out after immersing for a first time, wash it with deionized water, and dry it at a first preset temperature for a second time to form a polydopamine coating on the surface of the substrate; Step 3: adding the photocatalytic particles to deionized water and performing ultrasonic dispersion to obtain solution A; adding the cleaned zeolite to solution A, adjusting the pH value of the solution to a second preset pH value, performing magnetic stirring and ultrasonic dispersion to obtain solution B; Step 4: placing the substrate provided with the polydopamine coating obtained in step 2 on a rotating table, spraying the solution B obtained in step 3 on the substrate on the rotating table, and drying at the second preset temperature for a third time.

[0007] Furthermore, in step 1, the solute concentration of tris(hydroxymethyl)aminomethane is 1% to 1.2114% (w / v), and the solute concentration of dopamine hydrochloride is 0.2% to 0.5% (w / v).

[0008] Furthermore, after dopamine hydrochloride is added to the buffer solution, it is placed on a magnetic stirrer for stirring. The speed of the magnetic stirring is 300-800 rpm / min, and the stirring time is 2 h.

[0009] Furthermore, the first time is 12 hours; the first preset temperature is 50°C~150°C; and the second time is 12 hours.

[0010] Furthermore, in step 2, the stirring is carried out in a magnetic stirrer, the stirring speed is 300-800 rpm / min, and the stirring time is 10-24 h; and the substrate is a porous aluminum filter.

[0011] Furthermore, the photocatalytic particles are one of titanium dioxide, zinc oxide, g-C3N4 or a combination thereof, and the diameter of the photocatalytic particles is 5-10 nm.

[0012] Furthermore, in step 3, the solute concentration of the photocatalytic particles is 2%~3% (w / v), the solute concentration of the zeolite is 1%~3% (w / v), and the diameter of the zeolite is less than or equal to 10 um.

[0013] Furthermore, the second preset temperature is 100° C. to 200° C., and the third time is 12 hours.

[0014] Furthermore, the rotation speed of the rotating table is 20~60rpm / min.

[0015] Furthermore, the regulator is sodium hydroxide; the first preset pH value is 8.5; and the second preset pH value is 7.

[0016] Compared with the prior art, the present invention has the following beneficial effects: In the present application, the photocatalytic particles and zeolite form a composite structure, and the composite structure is stably bonded to the substrate by sticky polydopamine; in this way, the photocatalytic particles are not easy to fall off, and the surface is not covered by adhesive, so they can fully contact with organic pollutants, and the stability is improved while the photocatalytic efficiency is not reduced. The stability is 0.91, which is much greater than 0.59 of direct spraying. At the same time, polydopamine has strong absorption in the ultraviolet band, which improves the intensity of the interaction between ultraviolet light and photocatalytic particles; polydopamine also has photothermal conversion characteristics, converting light energy into heat energy, increasing the surface temperature of the photocatalyst, and promoting the separation of electrons and holes in the photocatalytic particles, thereby reducing electron-hole recombination and improving the efficiency of the photocatalyst. Zeolite is a porous structure that adsorbs the air to be purified, increases the time for organic pollutants to interact with photocatalytic particles, and improves the degradation efficiency of the photocatalyst. After 60 minutes of purification, the formaldehyde concentration dropped by 84%. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A microscopic image of a sample obtained by a method for preparing a composite photocatalytic layer using polydopamine provided in Example 1 of the present invention; Figure 2 A comparison of the transmission spectra of a sample obtained by using polydopamine and a method for preparing a composite photocatalytic layer using polydopamine provided in Example 1 of the present invention; Figure 3 A comparison result of the photocatalytic performance of samples obtained by a method for preparing a composite photocatalytic layer using polydopamine provided in Example 1 and Example 3 of the present invention. DETAILED DESCRIPTION

[0018] In order to make the implementation process of the present invention clearer, it will be described in detail below with reference to the accompanying drawings.

[0019] Embodiment 1: The present application provides a method for preparing a composite photocatalytic layer using polydopamine, the method comprising the following steps: Step 1: Dissolve tris(hydroxymethylaminomethane) powder in deionized water, wherein the solute concentration of tris(hydroxymethylaminomethane) is 1% to 1.2114% (w / v); preferably, weigh 1.2114 g of tris(hydroxymethylaminomethane) powder and dissolve it in 100 ml of deionized water, add a regulator, and adjust the pH value of the solution to a first preset pH value to obtain a buffer solution; the regulator is sodium hydroxide, and the first preset pH value is 8.5; the oxidation rate and polymerization rate under this pH condition are relatively moderate, which is conducive to the formation of uniform polydopamine film or particles. If the pH value is too high, the oxidation and polymerization rates may be too fast, resulting in uneven products; if the pH is too low, the reaction rate is too slow, and polydopamine may not be formed. Dopamine hydrochloride is dissolved in a buffer solution to obtain a polydopamine solution, wherein the solute concentration of dopamine hydrochloride is 0.2% to 0.5% (w / v). Within the concentration range of 0.2% to 0.5% (w / v), dopamine hydrochloride can be fully dissolved in the buffer solution to ensure a uniform reaction system. Avoid uneven polymerization due to excessive local concentration, so that the generated polydopamine film or particles are uniform. Preferably, 0.2 g of dopamine hydrochloride is dissolved in a prepared tris(hydroxymethyl)aminomethane buffer solution. After dopamine hydrochloride is added to the buffer solution, it is placed on a magnetic stirrer and stirred at a speed of 300 to 800 rpm / min. Preferably, the stirring speed is 500 rpm / min and the stirring time is 2 hours; in this way, sufficient mixing can be performed. The role of tris(hydroxymethyl)aminomethane is mainly to promote the oxidation of dopamine by providing an alkaline environment.

[0020] Step 2: Place the substrate in deionized water, ethanol and acetone for ultrasonic cleaning, each ultrasonic time is greater than 5 minutes, and then blow dry with nitrogen to obtain a clean substrate. The cleaned substrate is completely immersed in the polydopamine solution and stirred. In the magnetic stirrer, the stirring speed is 300~800rpm / min and the stirring time is 10~24h; after soaking for the first time, take it out, wash it with deionized water, and dry it at the first preset temperature for the second time to form a polydopamine coating on the surface of the substrate. The first time is 12h, the first preset temperature is 50℃~150℃, and the second time is 12h. The substrate is a porous aluminum filter, and the shape of the hole can be a hexagonal honeycomb with a side length of 2mm. Specifically, the porous aluminum filter is placed in deionized water, ethanol and acetone for ultrasonic cleaning for 10 minutes respectively, and then blow dried with nitrogen. It is completely immersed in the polydopamine solution and continues to be magnetically stirred at 400rpm / min. After 12 hours, the substrate was taken out, washed with deionized water, and dried at 100 °C for 2 hours. As a substrate, the porous aluminum filter has the following advantages: on the one hand, the porous structure of the porous aluminum filter provides a large number of attachment points for the polydopamine coating, increasing the loading amount. The dopamine molecules can form a firm coating on the substrate surface through oxidative polymerization. The porous structure makes the coating adhesion more stable, reducing the risk of the coating falling off in subsequent operations, and improving the overall efficiency of the photocatalytic reaction; on the other hand, aluminum has excellent thermal conductivity, and the porous aluminum filter can better disperse the heat generated during the photocatalytic reaction. In the photocatalytic reaction, during the process of converting light energy into heat energy, the heat can be rapidly diffused through the aluminum substrate to avoid local overheating. Local high temperature causes catalyst failure or a decrease in reaction rate; on the other hand, the pore structure of the porous aluminum filter can serve as a channel for the transfer of reactants and products, so that the reactants can more easily reach the surface of the photocatalytic particles, and the products after the reaction can also quickly leave the reaction area. This effective mass transfer effect helps to improve the overall efficiency of the photocatalytic reaction.

[0021] Step 3: Add photocatalytic particles to deionized water and perform ultrasonic dispersion to obtain solution A; add the cleaned zeolite to solution A, adjust the pH value of the solution to the second preset pH value, perform magnetic stirring and ultrasonic treatment, the magnetic stirring speed is 400-600rpm / min, and the ultrasonic treatment is performed at 30 kHz and 200 watts for 10 minutes. Solution B is obtained. The photocatalytic particles are one or a combination of titanium dioxide, zinc oxide, and g-C3N4, and the diameter of the photocatalytic particles is 5-10nm. The solute concentration of the photocatalytic particles is 2%-3% (w / v), and the solute concentration of the zeolite is 1%-3% (w / v); the concentration of the photocatalytic particles is 2%-3% (w / v), which can provide sufficient active surface area to absorb light energy and catalyze the reaction. If the concentration is too low, the amount of photocatalyst is insufficient and the reaction rate may be limited; while too high a concentration may cause agglomeration between particles, which in turn reduces the efficiency of light utilization and hinders the progress of the photocatalytic reaction. The diameter of the zeolite is less than or equal to 10 um. The second preset pH value is 7. The zeolite needs to be added to deionized water for ultrasonic cleaning, and then dried at high temperature to obtain impurity-free zeolite particles. Specifically, 3g of titanium dioxide is added to 100ml of deionized water for ultrasonic dispersion for 10min to obtain solution A, and the zeolite is added to deionized water for ultrasonic cleaning for 30min, and then dried at 100°C for 12h to obtain impurity-free zeolite particles; 1.5g of impurity-free zeolite particles are added to solution A, and the solution pH value is adjusted to 7, and then magnetically stirred at 400rpm / min for 2h, and then ultrasonicated for 10min to obtain composite solution B. The mass ratio of zeolite to titanium dioxide is 1:2, so that the amount of titanium dioxide is large, and more titanium dioxide can be loaded on the zeolite. Titanium dioxide has strong light absorption ability and efficient photocatalytic activity. A higher proportion of titanium dioxide can ensure that there is enough photocatalyst exposed to the light source, thereby maximizing light absorption and increasing the reaction rate. Zeolite can capture reactants and concentrate them on the surface of titanium dioxide, enhance the contact opportunities between reactants and photocatalysts, and promote the reaction; zeolite mainly plays its adsorption and dispersion role at a lower ratio, effectively dispersing titanium dioxide particles and preventing them from agglomerating. The porous structure of zeolite not only helps to adsorb reactants, but also improves the stability of the composite material, prevents the agglomeration of titanium dioxide particles, and ensures that its active surface can fully contact the reactants.

[0022] Step 4: Place the substrate provided with the polydopamine coating obtained in step 2 on a rotating table, and the rotation speed of the rotating table is 20-60rpm / min, preferably, the rotation speed is 30rpm / min. After spraying the solution B obtained in step 3 on the substrate on the rotating table, the drying time is the third time at the second preset temperature; the second preset temperature is 100℃~200℃, 100℃ in this embodiment, and the third time is 12h; at a temperature of 100℃, the solvent in the solution can be rapidly and completely volatilized to ensure uniform drying of the coating. This avoids coating defects that may be caused by any solvent residue, thereby ensuring that the photocatalytic coating has good physical and chemical properties. Enhance the binding force between zeolite and photocatalytic material, and the higher temperature enables the zeolite and photocatalytic material in the coating to be better shaped and cured on the surface of the substrate, thereby improving the adhesion between them and the stability of the overall structure. And the temperature of 100℃ is relatively mild, which is suitable for the tolerance range of most common substrate materials (such as metals, glass, heat-resistant polymers, etc.). This can avoid thermal deformation or degradation of the substrate material due to high temperature, thereby maintaining the integrity and mechanical strength of the substrate. The microscopic image of the photocatalytic layer is as follows: Figure 1 As shown, the dark part is a mixture of polydopamine, zeolite, and photocatalyst particles, and the light part is the base, indicating that the photocatalytic layer of the present application has been successfully prepared.

[0023] In the photocatalytic layer obtained by the method of the present application, the polydopamine on the surface of the substrate has strong adhesion, which can adhere the photocatalytic particles to the substrate, making it difficult to fall off; in the stability test, the sample is placed on a vibration table with a frequency of 50 Hz, and the stability is obtained according to the solid loading and the drop amount. Specifically, the stability is expressed by the ratio of the difference between the solid loading and the drop amount to the solid loading. The solid loading of the photocatalytic layer obtained in this embodiment is 0.22g, the drop amount is 0.02g, and the stability is 0.91, which is much greater than 0.59 of direct spraying. Its stability and long-term effectiveness under complex environmental conditions are guaranteed. And polydopamine is self-assembled polymerization, which is environmentally friendly. The photocatalytic nanoparticles can be fixed on the polydopamine coating by simple dipping or spraying, and the preparation process is simple. Polydopamine has photothermal conversion properties and absorbs light in the ultraviolet, visible and infrared regions. It can effectively convert light energy into heat energy, increase the surface temperature of the photocatalyst, and promote the separation of electrons and holes in the photocatalytic particles, thereby reducing electron-hole recombination and improving the efficiency of the photocatalyst. Figure 2 The transmission spectra of polydopamine (red curve) and polydopamine composite photocatalyst (black curve, the photocatalytic layer of the present application); after the composite, the transmittance decreases, which means that the absorption is enhanced, and the interaction between the photocatalytic layer of the present application and the light field is stronger, thus further improving the photocatalytic efficiency. When the photocatalytic particles are used for air purification, the light source required is also an ultraviolet light source, which matches its energy band gap.

[0024] The photocatalytic particles are not in direct contact with polydopamine. Zeolite is a porous material, and nanoscale photocatalytic particles (such as titanium dioxide) are attached to the surface of zeolite and in the pores of zeolite. In this way, on the one hand, the contact area between the photocatalytic particles and the adhesive is small, and the surface will not be covered by a large area of ​​the adhesive, so the contact area with the organic pollutants in the air is larger. On the other hand, zeolite has a porous structure, and the organic pollutants in the air will be adsorbed in the porous structure of the zeolite when passing through, thereby increasing the interaction time between the organic pollutants and the photocatalytic particles and improving the degradation efficiency of the photocatalyst. Figure 3 The comparison results of formaldehyde degradation by the photocatalytic layer prepared in this embodiment and in embodiment 3 are as follows. After 60 minutes, the formaldehyde concentration in this embodiment decreased by 84%, while the formaldehyde concentration in embodiment 3 decreased by 73%. The photocatalytic layer obtained in this embodiment has a better purification effect.

[0025] Embodiment 2: Step 1: Weigh 1.2114 g of tris(hydroxymethyl)aminomethane powder and dissolve it in 100 ml of deionized water, add sodium hydroxide to adjust the pH value to 8.5 to obtain a buffer solution. Dissolve 0.2 g of dopamine hydrochloride in the prepared tris(hydroxymethyl)aminomethane buffer solution. Then place the dopamine solution on a magnetic stirrer and stir at 500 rpm / min for 2 hours.

[0026] Step 2: Place a 3mm hexagonal honeycomb porous aluminum filter in deionized water, ethanol and acetone for ultrasonic cleaning for 10 minutes, then blow dry with nitrogen. Make it completely immersed in the polydopamine solution and continue to stir magnetically at 400rpm / min. Take out the substrate after 12h, wash it with deionized water, and dry it at 100℃ for 2 hours.

[0027] Step 3: Add 3 g of titanium dioxide to 100 ml of deionized water and ultrasonically disperse for 10 minutes to obtain solution A. Add zeolite to deionized water and ultrasonically clean it for 30 minutes. Then dry it at 100°C for 12 hours to obtain impurity-free zeolite particles. Add 3 g of impurity-free zeolite particles to solution A, adjust the solution pH to 7, and then magnetically stir at 400 rpm / min for 2 hours, and then ultrasonicate for 10 minutes to obtain composite solution B.

[0028] Step 4: Place the substrate with the polydopamine coating obtained in step 2 on a rotating table at a rotation speed of 30 rpm / min. Spray the solution B obtained in step 3 on the substrate on the rotating table, place in a drying oven, and dry at 100° C. for 12 hours.

[0029] Step 1: Weigh 1.2114 g of tris(hydroxymethyl)aminomethane powder and dissolve it in 100 ml of deionized water, add sodium hydroxide to adjust the pH value to 8.5 to obtain a buffer solution. Dissolve 0.5 g of dopamine hydrochloride in the prepared tris(hydroxymethyl)aminomethane buffer solution. Then place the dopamine solution on a magnetic stirrer and stir at 500 rpm / min for 2 hours.

[0030] Step 2: Place a 1 mm thick glass substrate in deionized water, ethanol, and acetone for ultrasonic cleaning for 10 minutes, then blow dry with nitrogen. Completely immerse it in the polydopamine solution and continue to stir it magnetically at 400 rpm / min. Take out the substrate after 12 hours, rinse it with deionized water, and dry it at 100°C for 2 hours.

[0031] Step 3: Add 3 g of titanium dioxide to 100 ml of deionized water and ultrasonically disperse for 5 minutes to obtain solution A. Add zeolite to deionized water and ultrasonically clean it for 30 minutes. Then dry it at 150°C for 12 hours to obtain impurity-free zeolite particles. Add 3 g of impurity-free zeolite particles to solution A, adjust the solution pH to 7, and then magnetically stir at 400 rpm / min for 2 hours, and then ultrasonicate for 10 minutes to obtain composite solution B.

[0032] Step 4: Place the glass substrate with polydopamine coating obtained in step 2 on a rotating table at a rotation speed of 30 rpm / min. Spray solution B obtained in step 3 on the substrate on the rotating table, place in a drying oven, and dry at 100° C. for 12 hours.

[0033] Step 1: Weigh 1.0 g of tris(hydroxymethyl)aminomethane powder and dissolve it in 100 ml of deionized water, add sodium hydroxide to adjust the pH value to 8.5 to obtain a buffer solution. Dissolve 0.5 g of dopamine hydrochloride in the prepared tris(hydroxymethyl)aminomethane buffer solution. Then place the dopamine solution on a magnetic stirrer and stir at 500 rpm / min for 2 hours.

[0034] Step 2: Place the sandpaper in deionized water, ethanol and acetone for ultrasonic cleaning for 10 minutes respectively, and then blow it dry with nitrogen. Make it completely immersed in the polydopamine solution and continue to stir it magnetically at 400 rpm / min. Take out the substrate after 12 hours, wash it with deionized water, and dry it at 100℃ for 2 hours.

[0035] Step 3: Add 3 g of titanium dioxide to 100 ml of deionized water and ultrasonically disperse for 10 minutes to obtain solution A. Add zeolite to deionized water and ultrasonically clean it for 30 minutes. Then dry it at 100°C for 12 hours to obtain impurity-free zeolite particles. Add 3 g of impurity-free zeolite particles to solution A, adjust the solution pH to 7, and then magnetically stir at 400 rpm / min for 2 hours, and then ultrasonicate for 10 minutes to obtain composite solution B.

[0036] Step 4: Place the sandpaper with polydopamine coating obtained in step 2 on a rotating table at a rotation speed of 30 rpm / min. Spray solution B obtained in step 3 on the substrate on the rotating table, place in a drying oven, and dry at 100° C. for 12 hours.

[0037] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a composite photocatalytic layer using polydopamine, characterized in that: The method comprises the following steps: Step 1: dissolving tris(hydroxymethyl)aminomethane) powder in deionized water, adding a regulator, and adjusting the pH value of the solution to a first preset pH value to obtain a buffer solution; dissolving dopamine hydrochloride in the buffer solution to obtain a polydopamine solution; Step 2: completely immersing the substrate in the polydopamine solution, stirring, taking out after immersion for a first time, washing with deionized water, and drying at a first preset temperature for a second time to form the polydopamine coating on the surface of the substrate; Step 3: adding the photocatalytic particles into deionized water and performing ultrasonic dispersion to obtain solution A; Adding the cleaned zeolite to the solution A, adjusting the pH value of the solution to a second preset pH value, performing magnetic stirring and ultrasound to obtain a solution B; Step 4: placing the substrate provided with the polydopamine coating obtained in step 2 on a rotating table, spraying the solution B obtained in step 3 on the substrate on the rotating table, and drying at a second preset temperature for a third time.

2. The method for preparing a composite photocatalytic layer using polydopamine according to claim 1, characterized in that: In the step 1, the solute concentration of tris(hydroxymethyl)aminomethane is 1% to 1.2114% (w / v), and the solute concentration of dopamine hydrochloride is 0.2% to 0.5% (w / v).

3. The method for preparing a composite photocatalytic layer using polydopamine according to claim 2, characterized in that: In the step 1, after the dopamine hydrochloride is added to the buffer solution, it is placed on a magnetic stirrer for stirring. The speed of the magnetic stirring is 300-800 rpm / min, and the stirring time is 2 h.

4. The method for preparing a composite photocatalytic layer using polydopamine according to claim 3, characterized in that: The first time is 12 hours; the first preset temperature is 50° C. to 150° C.; the second time is 12 hours.

5. The method for preparing a composite photocatalytic layer using polydopamine according to claim 4, characterized in that: In the step 2, the stirring is carried out in a magnetic stirrer, the stirring speed is 300-800 rpm / min, and the stirring time is 10-24 hours; and the substrate is a porous aluminum filter.

6. The method for preparing a composite photocatalytic layer using polydopamine according to claim 5, characterized in that: The photocatalytic particles are one of titanium dioxide, zinc oxide, g-C3N4 or a combination thereof, and the diameter of the photocatalytic particles is 5-10 nm.

7. The method for preparing a composite photocatalytic layer using polydopamine according to claim 6, characterized in that: In the step 3, the solute concentration of the photocatalytic particles is 2% to 3% (w / v), the solute concentration of the zeolite is 1% to 3% (w / v), and the diameter of the zeolite is less than or equal to 10 um.

8. The method for preparing a composite photocatalytic layer using polydopamine according to claim 7, characterized in that: The second preset temperature is 100° C. to 200° C., and the third time is 12 hours.

9. The method for preparing a composite photocatalytic layer using polydopamine according to claim 8, characterized in that: The rotation speed of the rotating table is 20-60 rpm / min.