Efficient sorting method for iron ore concentrate
Through reselection screening, magnetic separation, reverse flotation and alkali leaching joint selection processes, the problem of difficult to improve Fe grade and impurity content in iron concentrate in Aba mining area in Sichuan was solved, and the improvement of Fe grade and effective removal of impurities was achieved. Meets the raw material requirements of high-value-added products.
Patent Information
- Application Number
- CN202410805564.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-15
AI Technical Summary
The Fe grade in iron concentrate in Aba Mine Area in Sichuan is 69.49%, and the main impurity elements Al2O3 and SiO2 account for 0.85% and 1.95% respectively. The existing magnetic separation + flotation methods are difficult to meet the requirements of iron concentrate grade and impurity content.
Reselecting screening, magnetic separation, reverse flotation and alkali leaching joint selection processes are adopted, and deep removal is carried out through the shaker, ball mill, five-stage magnetic separation column, reverse flotation desulfurization and alkali leaching steps. Impurities, improve the grade and purity of iron concentrate.
The Fe grade of the raw ore was increased to 72.19%, the Al2O3 and SiO2 contents were reduced to 0.12% and 0.04%, respectively, and the Fe3O4 purity reached 99.77%, meeting the raw material requirements of high-value-added products and improving the recovery and yield of concentrates.
Smart Images

Figure CN118950236A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron ore beneficiation, and in particular to a method for efficiently separating iron ore concentrate. Background Art
[0002] In recent years, with the rapid development of the steel industry, the development and utilization of various high value-added products such as reduced iron powder for powder metallurgy, magnetic materials, and iron red are becoming research hotspots. Such products have extremely high requirements for upstream raw materials, generally requiring iron ore concentrate TFe grade higher than 71.50%, SiO2 content less than 0.25%, and other impurities content less than 0.20%.
[0003] However, the iron ore concentrate in the Aba mining area of Sichuan Province has an Fe grade of 69.49%, and the main impurity elements Al2O3 and SiO2 account for 0.85% and 1.95% respectively, followed by trace amounts of CaO, MgO, SO3 and MgO. The iron mineral is mainly magnetite, and the impurity minerals are mainly quartz, chlorite, dolomite, pyrrhotite and mica. Magnetite is mostly produced in semi-automorphic or irregular granular form, with a particle size ranging from 0.02 to 0.30 mm, a dissociation degree of 97.17%, and the intergrowth is mostly rich intergrowth, mainly interlocked with chlorite, dolomite, mica and quartz. Gangue minerals are mostly produced in semi-automorphic granular, plate-like or irregular granular form, with a particle size between 0.02 and 0.50 mm. A small part is produced as a monomer, and most of them are interlocked with magnetite and gangue minerals. Fine grinding is required to achieve complete dissociation of gangue mineral monomers. In addition, the gangue mineral pyrrhotite is the main occurrence mineral of S element, and it is mostly produced in the form of single particles, and the particle size varies from 0.02 to 0.15 mm. Since the density and specific magnetic susceptibility of pyrrhotite are similar to those of magnetite, it is difficult to separate it by conventional magnetic separation. Further flotation method can be used to partially remove it, but it still cannot meet the above-mentioned standards for iron ore concentrate.
[0004] That is, the prior art generally adopts a separation system consisting of a magnetic separation device and a flotation device for separation. However, the grade and impurity content of the iron concentrate obtained by adopting such a system do not meet the requirements. Summary of the invention
[0005] The purpose of the present invention is to provide a method for efficiently separating iron ore concentrate to solve the above problems.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows: an efficient separation method for iron concentrate, which comprises a gravity separation step, a magnetic separation step, a reverse flotation step and an alkali leaching step in sequence.
[0007] The present invention aims at the difference in magnetic susceptibility and density between the useful mineral magnetite and the gangue mineral (such as quartz) in the concentrate, adopts the gravity separation and magnetic separation process with high processing efficiency, low cost and simple process, and further performs flotation on the basis of gravity separation and magnetic separation to strengthen the deep removal of fine-grained gangue minerals. In order to efficiently remove the extremely fine-grained gangue minerals in the concentrate and the gangue that is difficult to remove due to lattice substitution and doping, a chemical leaching combined method is further used for separation.
[0008] The existing technology generally adopts the method of "magnetic separation + flotation". The present application performs gravity separation and screening before magnetic separation, which effectively reduces the content of impurities such as Al and Si and improves the grade of iron concentrate.
[0009] As a preferred technical solution, the re-selection and screening step is carried out using a shaking table and a ball mill is used for grinding.
[0010] As a preferred technical solution, the magnetic separation step is five-stage magnetic separation column separation-grinding-three-stage magnetic separation column re-selection.
[0011] As a further preferred technical solution, the process parameters during magnetic column separation are: rising water flow rate is 5.7L / min~18L / min, preferably 15.6L / min; current is 0.25A~1.25A, preferably 1.00A; feeding rate is 50g / min~200g / min, preferably 100g / min; slurry concentration is 15wt.%~30wt.%, preferably 20wt.%, and the fineness of the grinding is -0.038mm, accounting for 99.73%.
[0012] As a further preferred technical solution, after the three-stage magnetic separation column is re-selected, a two-stage shaking table separation is performed.
[0013] As a further preferred technical solution, the process parameters of the shaking table operation are: the flushing water flow rate is 2.5L / min~15L / min, preferably 12.5L / min, the ore feeding rate is 60g / min~240g / min, preferably 120g / min, and the inclination angle is set at 1°~3°, preferably 2°.
[0014] As a more preferred technical solution, the reverse flotation step includes reverse flotation desulfurization, reverse flotation desiliconization roughing and reverse flotation desiliconization cleaning in sequence.
[0015] Reverse flotation desulfurization is also one of the final innovative points of this application. The inventors analyzed and found that the iron concentrate contains a small amount of pyrrhotite and pyrite. These two types of gangue minerals not only reduce the Fe content in the concentrate, but also bring in harmful elements S. Through a large number of experiments, desulfurization was first carried out during flotation, which significantly improved the sorting effect. After desulfurization, the Fe grade of the heavy-magnetic concentrate was increased from 72.10% to 72.11%, the Al2O3 content was reduced from 0.152% to 0.151%, and the SiO2 content was reduced from 0.072% to 0.070%.
[0016] As a further preferred technical solution, during the reverse flotation desulfurization, the pH is adjusted to 6.0, the desulfurizer is 50g / t of amyl xanthate, and terpineol is added; the reverse flotation desiliconization roughing and reverse flotation desiliconization selection both use dodecylamine as the reverse flotation collector, the aeration volume is 5.0L / min~10.0L / min, preferably 8.0L / min, the stirring speed is 600r / min~1000r / min, preferably 800r / min, and the amount of dodecylamine is 50g / t~90g / t, preferably 60g / t.
[0017] As a further preferred technical solution, fine grinding is performed before the alkali leaching step, and the particle size after grinding is about -10 μm, accounting for 98.65%.
[0018] As a further preferred technical solution, the process parameters of the alkali leaching are: the alkali is NaOH, and its dosage is 40g / L~80g / L, preferably 80g / L; the leaching temperature is 150℃~180℃; the pressure is 0Mpa~3Mpa; the stirring speed is 400r / min~800r / min; and the reaction time is 3h~4h.
[0019] Aluminum silicon oxides can react with NaOH to generate water-soluble aluminates and silicates. At the same time, during the reaction, the dissolution of aluminum silicon oxides can be promoted by adding excess NaOH, increasing the reaction temperature, increasing the pressure and mechanical stirring to achieve separation from magnetite.
[0020] Compared with the prior art, the advantages of the present invention are: the present invention adopts the "gravity separation-magnetic separation-reverse flotation-alkaline leaching" joint selection process to increase the Fe grade of the original ore from 69.49% to 72.19%, reduce the proportion of the main impurity element Al2O3 from 0.85% to 0.12%, and reduce the proportion of SiO2 from 1.95% to 0.04%. The purity of Fe3O4 in the obtained concentrate is 99.77%, thereby meeting the requirements of upstream raw materials, the leaching concentrate yield is 17.35%, the concentrate Fe recovery rate is 18.02%, and the industrial practicability is strong. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1It is a flow chart of Example 1 of the present invention and a quality result diagram of each step. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the accompanying drawings. Unless otherwise specified, the percentages in the following embodiments are all by mass.
[0023] Embodiment 1:
[0024] The raw ore in this embodiment is: the raw ore Fe grade is 69.49% in the iron concentrate taken from the Aba mining area in Sichuan, and the main impurity elements Al2O3 and SiO2 account for 0.85% and 1.95% respectively, followed by trace amounts of CaO, MgO, SO3 and MgO. The iron mineral is mainly magnetite, and the impurity minerals are mainly quartz, chlorite, dolomite, pyrrhotite and mica;
[0025] See also Figure 1 The above-mentioned method for efficiently separating iron ore concentrate comprises the following steps:
[0026] (1) Gravity screening:
[0027] Use shaking table to reselect and screen the raw ore:
[0028] Process parameters: flushing water flow rate is 12.5L / min, at this time the concentrate yield is 85.35%, the Fe grade is 70.86%, and the Al2O3 and SiO2 grades are 0.41% and 0.68% respectively;
[0029] The feed rate is 120g / min; the inclination angle is set at 2°;
[0030] Ball mill grinding, the best grinding fineness is -0.038mm, accounting for 99.73%;
[0031] The mass proportion of +0.15mm particle size in the original ore is 8.80%, and its Fe, Al2O3 and SiO2 contents are 59.23%, 2.82% and 9.09% respectively, and the element distribution rates are 7.50%, 32.03% and 43.24% respectively. The coarse particle size can be discarded in advance through the above simple gravity separation and screening operation, which greatly reduces the Al2O3 and SiO2 contents in the concentrate. After discarding the tailings, the Fe, Al2O3 and SiO2 contents in the concentrate are 70.50%, 0.58% and 1.15% respectively.
[0032] (2) Magnetic separation, specifically including:
[0033] 1) Five-stage magnetic separation of magnetic separation column:
[0034] The parameters are: rising water flow rate is 15.6L / min, current is 1.00A, feed rate is 100g / min, slurry concentration is 20%, grinding fineness is -0.038mm, accounting for 99.73%;
[0035] After five stages of magnetic separation, the Fe content of the concentrate can be enriched to 71.75%, the Al2O3 content of the concentrate is 0.23%, and the SiO2 content is 0.12%.
[0036] 2) Grinding:
[0037] When the grinding fineness is -0.038mm, accounting for 99.34%, the sorting effect is better. At this time, the Fe grade of the concentrate is 71.88%, the Al2O3 and SiO2 grades are 0.21% and 0.11% respectively, and the Fe recovery rate of the concentrate is 35.15%;
[0038] 3) Three-stage magnetic column reselection:
[0039] The three-stage magnetic column reselection operation can achieve better indicators, the concentrate Fe grade can be increased to 72.04%, the Al2O3 and SiO2 contents are 0.16% and 0.10% respectively, and the total recovery rate of concentrate Fe is 28.84%. At this time, the purity of Fe3O4 is 99.56%;
[0040] 4) One-stage shaking table:
[0041] Process parameters: When the flushing water flow rate is 12.5L / min, the sorting index is the best, at which the concentrate yield is 85.35%, the Fe grade is 70.86%, and the Al2O3 and SiO2 grades are 0.41% and 0.68% respectively;
[0042] The best feeding rate is 120g / min; the inclination angle is set at 2°;
[0043] After one stage of shaking table sorting, the Fe grade of the concentrate can be increased to 72.07%, the Al2O3 content is reduced to 0.15%, the SiO2 content is reduced to 0.08%, the total recovery rate of Fe in the concentrate is 26.94%, and the purity of Fe3O4 is 99.60%
[0044] 5) Two-stage shaking table:
[0045] After the second stage of shaking, the concentrate Fe grade was 72.10%, Al2O3 content was 0.15%, SiO2 content was 0.07%, the total recovery rate of concentrate Fe was 23.41%, and the purity of Fe3O4 was 99.64%
[0046] 3. Reverse flotation, including:
[0047] 1) Reverse flotation desulfurization:
[0048] Adopt Outotec's intelligent control flotation machine;
[0049] Process parameters: sulfuric acid adjusted to pH 6.0, desulfurizer: 50g / t of amyl xanthate, add 2 drops of pinene alcohol,
[0050] After desulfurization, the Fe grade of the concentrate increased from 72.101% to 72.106%, the Al2O3 content decreased from 0.152% to 0.151%, and the SiO2 content decreased from 0.072% to 0.070%.
[0051] 2) Reverse flotation desiliconization roughing
[0052] Adopt Outotec's intelligent control flotation machine;
[0053] Dodecylamine (DDA) was used as the reverse flotation collector, the aeration volume was 8.0 L / min, the stirring speed was 800 r / min, and the DDA dosage was 60 g / t;
[0054] 3) Reverse flotation desiliconization and concentration
[0055] Adopt Outotec's intelligent control flotation machine;
[0056] Dodecylamine (DDA) was used as the reverse flotation collector, the aeration volume was 8.0 L / min, the stirring speed was 800 r / min, and the DDA dosage was 60 g / t;
[0057] After the above two stages of desiliconization, the Fe grade of the concentrate continued to increase from 72.11% to 72.16%, and the Al2O3 and SiO2 contents of the concentrate were reduced to 0.14% and 0.05% respectively;
[0058] (4) Alkali leaching
[0059] In a high-pressure reactor, in order to accelerate the reaction rate of NaOH with Al2O3 and SiO2, the concentrate was finely ground with an Isa mill before leaching. The particle size after grinding was about -10μm, accounting for 98.65%; the product after grinding was used as the leaching sample;
[0060] During leaching, when the amount of NaOH increased from 40 g / L to 80 g / L, the TFe grade of the leached concentrate increased from 72.17% to 72.18%, the SiO2 content decreased from 0.05% to 0.04%, and the Fe3O4 purity also increased to 99.75%;
[0061] When the leaching temperature increased from 150℃ to 180℃, the TFe grade and SiO2 content of the leached concentrate did not change significantly, while the Al2O3 content decreased from 0.13% to 0.12%;
[0062] When the pressure increases from 0Mpa to 3Mpa, there is no obvious change in the concentrate index;
[0063] When the stirring speed increased from 400 to 800 r / min, there was no significant change in the Al2O3 and SiO2 contents of the concentrate;
[0064] After the reaction time increased from 3h to 4h, the Fe grade of the concentrate could be further increased to 72.19%. At this time, the purity of Fe3O4 was 99.77%, the leaching concentrate yield was 17.35%, and the concentrate Fe recovery rate was 18.02%.
[0065] After the above treatment, the Fe grade of the concentrate was increased to 72.19%, the Al2O3 and SiO2 contents were 0.12% and 0.04% respectively, the Fe3O4 purity was 99.77%, the leaching concentrate yield was 17.35%, and the concentrate Fe recovery rate was 18.02%.
[0066] Comparative Example 1
[0067] In step (1) of Example 1, the process parameters for the shaking table gravity separation were screened as follows:
[0068] (1) Flushing water flow rate: As the flushing water flow rate increases from 2.5L / min to 12.5L / min, the yield and recovery rate of the shaking table concentrate show a trend of gradual decrease, with the yield decreasing from 88.04% to 85.35%, and the recovery rate decreasing from 89.53% to 87.01%. The Fe grade of the concentrate increased from 70.68% to 70.86%, the Al2O3 content decreased from 0.46% to 0.41%, and the SiO2 content decreased from 0.86% to 0.68%. When the flushing water flow rate is 12.5L / min, the sorting index is the best, at which the concentrate yield is 85.35%, the Fe grade is 70.86%, and the Al2O3 and SiO2 grades are 0.41% and 0.68%, respectively. Continuing to increase the flushing water flow rate will cause high-grade fine-grained magnetite to enter the middlings or tailings, resulting in a deterioration of its sorting index, so the optimal water volume is 12.5L / min;
[0069] (2) Feed rate: As the feed rate increases from 60 g / min to 240 g / min, the concentrate yield and recovery rate show a trend of gradual decrease, with the yield decreasing from 86.06% to 82.89% and the recovery rate decreasing from 87.66% to 84.58%. The Fe grade of the concentrate increases from 70.81% to 70.93%, the Al2O3 content decreases from 0.43% to 0.38%, and the SiO2 content decreases from 0.71% to 0.66%. Considering the recovery rate and grade comprehensively, the separation index is better when the feed rate is 120 g / min;
[0070] (3) The inclination angle of the shaking table has an important influence on the sorting effect. Increasing the lateral slope enhances the sliding effect of the ore particles and increases the discharge speed of the tailings, but the zoning of the selected area becomes narrower; as the inclination angle increases from 1° to 3°, the concentrate yield decreases from 86.97% to 76.95%, and the recovery rate decreases from 88.52% to 78.71%. The Fe grade of the concentrate increases from 70.75% to 71.10%, the Al2O3 content decreases from 0.45% to 0.36%, and the SiO2 content decreases from 0.73% to 0.56%; considering the recovery rate and grade comprehensively, it is more appropriate to set the inclination angle of 2°;
[0071] (4) Grinding: With rod mill as grinding equipment, the proportion of -0.074mm gradually increases with the increase of grinding time. The Fe grade of concentrate shows a trend of gradual increase with the increase of grinding fineness, while the grades of Al2O3 and SiO2 show a trend of gradual decrease as a whole. When the grinding fineness is -0.074mm, accounting for 81.12%, the sorting index is the best, and the grades of Fe, Al2O3 and SiO2 in the concentrate are 71.21%, 0.37% and 0.54% respectively. After continuing to increase the grinding fineness, the concentrate grade has no obvious increase, but the recovery rate has decreased significantly. The appropriate grinding fineness is -0.074mm, accounting for 81.12%. At the same time, it can be seen that although the particle size of the rod mill is relatively uniform and can reduce over-crushing, its overall particle size is coarse. After the grinding time reaches 20 minutes, the fineness change is small. The reason is that there is line contact between the grinding medium steel rods, and the steel rods will have surface wear and depression after long-term use. In order to improve the grinding fineness, a ball mill is used for grinding;
[0072] (5) Coarse and fine classification-grinding-shaking table test
[0073] In order to reduce the over-crushing of fine-grained materials during ball milling and avoid the generation of "mudification", the materials can be coarsely graded, where the +0.038mm particle size is combined with the -0.038mm particle size after ball milling and enters the shaking table for sorting. The results are shown in Table 1:
[0074] Table 1 Effect of grinding fineness on coarse and fine classification-grinding-shaking table separation index
[0075]
[0076] As can be seen from Table 1 above, with the increase of grinding fineness, the yield of shaking table concentrate gradually decreases. When the grinding fineness increases from -0.038mm (accounting for 25.39%) to 99.92%, the concentrate yield and recovery rate show a trend of gradual decrease, among which the yield decreases from 85.35% to 44.76%, and the recovery rate decreases from 87.01% to 46.24%. The Fe grade of the concentrate increases from 70.86% to 71.81%, the Al2O3 content decreases from 0.41% to 0.18%, and the SiO2 content decreases from 0.68% to 0.21%. When the grinding fineness is -0.038mm (accounting for 99.86%), the sorting index is better. At this time, the Fe grade of the concentrate is 71.79%, and the Al2O3 and SiO2 grades are 0.19% and 0.20%, respectively. Compared with the test of direct grinding without classification, the test process of grinding after classification has a certain effect on the recovery rate of Fe in concentrate. Since the coarse and fine classification increases the operation process and the increase in the recovery rate of Fe in concentrate is not large, direct grinding is preferred.
[0077] Comparative Example 2
[0078] For the magnetic separation in step (2) of the above embodiment 1,
[0079] (1) As for the magnetic separation device, the inventors tested a magnetic separation tube as the magnetic separation device, and the results were:
[0080] As the magnetic induction intensity gradually increases, the concentrate yield gradually increases. When the magnetic induction intensity increases from 5mT to 50mT, the concentrate yield and recovery rate show a trend of gradual increase, with the yield increasing from 13.81% to 68.69%, and the recovery rate increasing from 14.25% to 70.24%. The Fe grade of the concentrate decreased from 71.76% to 71.08%, the Al2O3 content increased from 0.19% to 0.44%, and the SiO2 content increased from 0.18% to 0.46%. The above data show that the magnetic separation effect of the magnetic separator is relatively poor, and it is difficult to obtain good separation indicators;
[0081] On this basis, the inventors investigated the influence of grinding fineness. The results showed that as the grinding fineness increased from -0.074mm (57.61%) to 97.65%, the overall change in concentrate yield was small, and the concentrate Fe grade showed a gradual increase from 71.61% to 71.82%; while the Al2O3 and SiO2 contents showed a gradual decrease, with the Al2O3 content decreasing from 0.25% to 0.21%, and the SiO2 content decreasing from 0.25% to 0.19%. When the grinding fineness was -0.074mm (95.88%), the sorting index was better, and the concentrate Fe, Al2O3 and SiO2 grades were 71.81%, 0.21% and 0.18%, respectively. The above experimental results show that it is difficult to obtain satisfactory sorting indicators even after grinding operations using magnetic separation tubes as sorting equipment.
[0082] (2) Elutriation magnetic separator test:
[0083] The elutriation magnetic separator uses a special magnetic system design and superposition of multiple magnetic fields to make the horizontal magnetic field in the elutriation machine barrel evenly distributed, and form a continuous and composite magnetic field with downward magnetic force in the vertical direction. After the minerals enter the separation barrel, the magnetic particles form a "magnetic chain" and float downward under the combined action of the continuous downward magnetic force, gravity, and the impact of the rising water, and form concentrate discharged at the bottom of the equipment. Since the magnetic field is uniform in the horizontal direction, the magnetic chain cannot move left and right under the action of the magnetic field, and the magnetic minerals will not "agglomerate" to the barrel wall. Impurities such as gangue in the mineral are distributed around the magnetic chain, and overflow at the top under the action of the rising water to form tailings;
[0084] Results: By adding one grinding operation to the one coarse and two fine operations of the elutriation magnetic separator, the concentrate yield and recovery rate increased slightly, while the grades of Fe, Al2O3 and SiO2 in the concentrate did not change much.
[0085] (3) Investigation of process parameters of magnetic separation column:
[0086] As the rising water flow rate increased from 5.7 to 18.0L / min, the concentrate yield decreased from 86.15% to 64.38%, and the recovery rate decreased from 87.92% to 66.10%; while the concentrate Fe grade increased from 70.94% to 71.37%, the Al2O3 content decreased from 0.51% to 0.38%, and the SiO2 content decreased from 0.68% to 0.49%. When the rising water flow rate was 15.6L / min, the sorting index was the best, at which the concentrate yield was 69.62%, the Fe grade was 71.33%, and the Al2O3 and SiO2 grades were 0.39% and 0.46%, respectively. At the same time, it can be seen that it is more difficult to reduce Al2O3 in the concentrate than to reduce SiO2;
[0087] As the current value increases from 0.25 to 1.25A, the concentrate yield increases from 56.34% to 76.88%, and the recovery rate increases from 57.96% to 78.58%; while the concentrate Fe grade decreases from 71.51% to 71.05%, the Al2O3 content increases from 0.31% to 0.46%, and the SiO2 content increases from 0.34% to 0.46%. When the current is 1.00A, the sorting effect is better, at which the concentrate yield is 69.62%, the Fe grade is 71.33%, and the Al2O3 and SiO2 grades are 0.39% and 0.46%, respectively. Continuing to increase the current to 1.25A, the grade drops significantly;
[0088] As the feed rate increases from 50g / min to 200g / min, the concentrate yield increases from 61.26% to 73.42%, and the recovery rate increases from 63.09% to 75.24%; while the concentrate Fe grade decreases from 71.59% to 71.23%, the Al2O3 content increases from 0.31% to 0.42%, and the SiO2 content increases from 0.31% to 0.48%. When the feed rate is 100g / min, the concentrate Fe grade and recovery rate are relatively good, at which the concentrate yield is 67.14%, the Fe grade is 71.51%, and the Al2O3 and SiO2 grades are 0.35% and 0.34%, respectively;
[0089] As the pulp concentration increases from 15% to 30%, the concentrate yield increases from 61.38% to 70.13%, and the recovery rate increases from 63.26% to 72.09%; while the concentrate Fe grade decreases from 71.64% to 71.45%, the Al2O3 content increases from 0.31% to 0.37%, and the SiO2 content increases from 0.25% to 0.36%. When the pulp concentration is 20%, the separation index is better, at which time the concentrate Fe grade is 71.62%, and the Al2O3 and SiO2 grades are 0.32% and 0.28% respectively;
[0090] As the grinding fineness increases from -0.038mm (25.39%) to 99.73%, the concentrate yield decreases from 65.67% to 42.38%, and the recovery rate decreases from 67.66% to 43.78%; while the concentrate Fe grade increases from 71.62% to 71.81%, the Al2O3 content decreases from 0.32% to 0.25%, and the SiO2 content decreases from 0.28% to 0.24%. When the grinding fineness is -0.038mm (99.73%), the sorting index is better, and the concentrate Fe grade is 71.81%, and the Al2O3 and SiO2 grades are 0.25% and 0.24% respectively. Continuing to increase the grinding fineness, the concentrate yield decreases significantly while the grade change is not obvious, so the appropriate grinding fineness is -0.038mm (99.73%).
[0091] (4) Investigation of “coarse and fine grading - grinding - magnetic separation”
[0092] In order to reduce the over-crushing of fine-grained materials during ball milling and avoid the generation of "mudification", the materials can be coarsely graded, and the +0.038mm particle size is combined with the -0.038mm particle size after ball milling and enters the magnetic separation;
[0093] Results As the grinding fineness increased from -0.038 mm (accounting for 25.39%) to 99.56%, the concentrate yield decreased from 65.67% to 38.76%, and the recovery rate decreased from 67.66% to 40.06%; while the concentrate Fe grade increased from 71.62% to 71.84%, the Al2O3 content decreased from 0.32% to 0.24%, and the SiO2 content decreased from 0.28% to 0.25%. When the grinding fineness was -0.038 mm (accounting for 99.31%), the separation effect was better, and the concentrate Fe grade was 71.83%, and the Al2O3 and SiO2 grades were 0.24% and 0.23% respectively. Compared with the test of direct grinding without classification, the test process of re-grinding after classification has a certain effect on improving the concentrate Fe recovery rate, but the improvement effect is not obvious, so the direct grinding method is preferred.
[0094] (5) Investigation of magnetic separation process:
[0095] 1) One roughing and one concentrating: On the basis of magnetic roughing, one concentrating operation is added. As a result, the Fe grade of the magnetic concentrate increases from 71.83% to 71.85%, the Al2O3 content decreases from 0.25% to 0.24%, and the SiO2 grade decreases from 0.24% to 0.23%;
[0096] 2) One coarse and two fines: On the basis of one coarse and one fine on the shaking table, another fine cleaning operation is added. The Fe grade of the concentrate increases from 71.85% to 71.87%, the Al2O3 content has no obvious change, and the SiO2 grade decreases from 0.23% to 0.22%;
[0097] 3) Stage grinding-stage selection: In order to reduce the over-crushing problem caused by the first stage grinding, it is considered to add a stage grinding operation before the magnetic separation and concentration. The test process is that the first stage grinding fineness is -0.038mm, accounting for 81.23%, and the second stage grinding is -0.038mm, accounting for 99.32%; on the basis of the one coarse and two fine magnetic separation columns, an additional grinding operation is added, and the concentrate grade is further improved. The Fe grade of the concentrate increases from 71.87% to 71.89%, and the Al2O3 and SiO2 contents in the concentrate are reduced to 0.22% and 0.19%, respectively.
[0098] (6) Magnetic separation column long process test
[0099] We investigated one-stage magnetic separation, two-stage magnetic separation, three-stage magnetic separation, four-stage magnetic separation, five-stage magnetic separation, and six-stage magnetic separation, and the results are as follows:
[0100]
[0101]
[0102]
[0103]
[0104]
[0105]
[0106] It can be seen that compared with the concentrate produced by five magnetic separations, the Fe grade of the concentrate produced by six magnetic separations has been improved less, and the Al2O3 content and SiO2 content have not changed much. The reason may be that the dissociation degree of the original ore is not enough, and the separation effect is limited by continuing to increase the number of magnetic separation operations. Therefore, it is preferred to add grinding operations on the basis of five magnetic separations.
[0107] On this basis, five-stage magnetic separation-grinding-one-stage magnetic separation test, five-stage magnetic separation-grinding-two-stage magnetic separation test, five-stage magnetic separation-grinding-three-stage magnetic separation test, five-stage magnetic separation-grinding-four-stage magnetic separation test, and five-stage magnetic separation-grinding-five-stage magnetic separation test were also carried out. The results are as follows:
[0108]
[0109]
[0110]
[0111]
[0112]
[0113] From the above results, it can be seen that the three-stage magnetic separation operation after regrinding can achieve good indicators, the Fe grade of the concentrate can be increased to 72.04%, the Al2O3 and SiO2 contents are 0.16% and 0.10% respectively, and the total recovery rate of Fe in the concentrate is 28.84%. At this time, the purity of Fe3O4 is 99.56%. After the three-stage magnetic separation operation of the concentrate, the Fe grade of the concentrate can continue to increase, but the increase is small, while the Al2O3 and SiO2 contents have almost no obvious changes, indicating that it is difficult to reduce the Al2O3 and SiO2 contents by continuing to increase the number of magnetic separation operations.
[0114] Gravity-magnetic separation test:
[0115] In order to enrich the Fe grade of the concentrate by physical separation as much as possible and reduce the contents of Al2O3 and SiO2, based on the above-mentioned experiments of gravity separation and magnetic separation, it is planned to further enrich the concentrate by continuing to optimize the process parameters and adopting the combined separation method of gravity separation and magnetic separation. Therefore, shaking table-magnetic separation column separation test, elutriation magnetic separator-magnetic separation column separation test, elutriation magnetic separator-magnetic separation column-shaking table separation test, magnetic separation column-shaking table separation test, etc. were carried out respectively. The results showed that the magnetic separation column-shaking table had the best effect. After multiple stages of magnetic separation and then two stages of shaking table separation, the Fe grade of the concentrate can be increased to 72.10%, the Al2O3 content has no obvious change, SiO2 is reduced to 0.07%, the total recovery rate of Fe in the concentrate is 23.41%, and the purity of Fe3O4 is 99.64%. Shaking table separation can improve the Fe grade of the concentrate to a certain extent. After the magnetic separation concentrate is separated by three stages of shaking table after multiple stages of magnetic separation, the Fe grade of the concentrate can be further increased to 72.12%, and the contents of Al2O3 and SiO2 have no significant changes. The total recovery rate of Fe in the concentrate is 20.89%, and the purity of Fe3O4 is 99.67%. It can be seen that the Fe content increases slightly with the continuous addition of shaking table operations, but the contents of Al2O3 and SiO2 have basically no significant changes.
[0116] Comparative Example 3
[0117] Regarding the reverse flotation in step (3) of the above embodiment 1, the inventors have conducted a lot of research, including:
[0118] (1) Collector selection test
[0119] DDA, DDA-NaOL, DDA-SDBS, CTAB-NaOL, and CTAB-SDBS were selected as magnetite reverse flotation collectors. By comparing different collectors and their test indicators under different dosage conditions, the best agent for reverse flotation desiliconization was screened out (the mass ratio of cationic collector dodecylamine to anionic collector was 1:1 during the test). Jilin prospecting flotation machine (1L) was used as the flotation equipment, and natural pH (7.52) was used as the condition. The results are as follows:
[0120]
[0121] It can be seen that compared with flotation using mixed anion and cation collectors, directly using dodecylamine (DDA) as a magnetite reverse flotation collector can achieve better separation effects, so the collector of the present invention is preferably dodecylamine.
[0122] (2) Inhibitor selection test;
[0123] Starch is the most commonly used flotation depressant for iron ore flotation. Therefore, the inventors selected corn starch and carboxymethyl starch as depressants for magnetite and conducted reverse flotation tests when the dosage of dodecylamine was 100 g / t. The results are as follows:
[0124] As the dosage of corn starch as an inhibitor increased from 0g / t to 400g / t, the yield increased from 73.99% to 82.37%, and the recovery rate increased from 75.85% to 84.04%; while the Fe grade of the concentrate decreased from 71.26% to 70.91%, the Al2O3 content increased from 0.26% to 0.41%, and the SiO2 content increased from 0.28% to 0.46%. Therefore, although corn starch can increase the Fe recovery rate of the concentrate, it reduces the Fe grade of the concentrate, which is not conducive to subsequent operations;
[0125] As the dosage of inhibitor carboxymethyl starch increases from 0g / t to 400g / t, the yield increases from 73.99% to 80.95%, and the recovery increases from 75.85% to 82.65%; while the Fe grade of the concentrate decreases from 71.26% to 70.97%, the Al2O3 content increases from 0.26% to 0.38%, and the SiO2 content increases from 0.28% to 0.48%. When the dosage of carboxymethyl starch is 100g / t, the Fe grade of the concentrate increases by 0.06 percentage points, and the recovery increases by 1.01 percentage points, which is limited in the increase, so the present invention does not add inhibitors.
[0126] (3) Screening of flotation process parameters
[0127] 1) Effect of grinding fineness on flotation
[0128] Results: As the grinding fineness increased from -0.038mm (accounting for 25.39%) to 97.45%, the concentrate yield decreased from 73.99% to 46.47%, and the recovery rate decreased from 75.85% to 47.90%; while the concentrate Fe grade increased from 71.26% to 71.65%, the Al2O3 content decreased from 0.26% to 0.18%, and the SiO2 content decreased from 0.28% to 0.18%. When the grinding fineness was -0.038mm (accounting for 94.32%), the separation effect was better, the concentrate Fe grade was 71.63%, the Al2O3 and SiO2 grades were 0.18% and 0.17% respectively, and the recovery rate was 58.61%;
[0129] 2) Effect of pH on flotation
[0130] Results: When the pH value increased from 5.22 to 6.05, the concentrate yield did not change much as a whole, while the concentrate Fe grade showed a trend of gradual decrease, while the Al2O3 and SiO2 grades showed a trend of gradual increase. When the pH value was 6.05, the concentrate Fe grade was 71.72%, the Al2O3 and SiO2 grades were 0.17% and 0.16% respectively, and the recovery rate was 57.14%.
[0131] 3) Effect of pulp concentration on flotation
[0132] Results: As the pulp concentration increased from 15% to 36%, the concentrate yield increased from 50.12% to 58.48%, and the recovery rate increased from 51.76% to 60.28%; while the concentrate Fe grade decreased from 71.79% to 71.63%, the overall change of Al2O3 content was not large, and the SiO2 content increased from 0.16% to 0.21%. When the pulp concentration was 20%, the sorting index was better, at which time the concentrate Fe grade was 71.78%, the Al2O3 and SiO2 grades were 0.17%, 0.15%, and the recovery rate was 52.84%;
[0133] 4) Effect of DDA dosage on flotation
[0134] Results: As the amount of collector DDA increased from 60g / t to 140g / t, the concentrate yield decreased from 65.43% to 40.12%, and the recovery rate decreased from 67.44% to 41.47%; while the concentrate Fe grade increased from 71.62% to 71.83%, the Al2O3 content decreased from 0.23% to 0.18%, and the SiO2 content decreased from 0.19% to 0.14%. It can be seen that after the DDA dosage increased to 100g / t, the concentrate Fe grade was 71.78%, and the Al2O3 and SiO2 contents were 0.17% and 0.15%, respectively. After continuing to increase the DDA dosage, the concentrate grade did not change much;
[0135] 5) XFD flotation machine one coarse and one fine flotation process
[0136] Results: On the basis of roughing, a concentration operation was added, and the Fe grade of flotation concentrate continued to increase. When the concentration DDA dosage was 30g / t, the Fe grade of the concentrate was 71.82%, and the contents of Al2O3 and SiO2 were 0.17% and 0.14% respectively. When the concentration DDA dosage was increased to 50g / t, the separation index was better, and the Fe grade of the concentrate was 71.92%, and the contents of Al2O3 and SiO2 were 0.16% and 0.11% respectively.
[0137] 6) XFD flotation machine one rough two fine flotation process
[0138] Results: On the basis of one coarse and one fine flotation, one more concentration operation was added, and the Fe grade of the concentrate could be further increased to 71.94%, and the Al2O3 and SiO2 contents of the concentrate were 0.16% and 0.11% respectively.
[0139] 7) XFD flotation machine one rough three fine flotation process
[0140] Results: Adding one more concentration operation on the basis of one coarse and two fine flotation, the Fe grade of the concentrate can be further increased to 71.98%, and the Al2O3 and SiO2 contents of the concentrate are 0.16% and 0.10% respectively;
[0141] 8) XFD flotation machine one coarse four fine flotation process
[0142] Results: By adding one more concentration operation on the basis of one roughing and three fine flotation, the Fe grade of the concentrate can be further improved to 72.01%, and the Al2O3 and SiO2 contents of the concentrate have no obvious changes.
[0143] (4) Selection of flotation equipment
[0144] The conventional XFD flotation machine, MFC flotation column and Outotec's intelligent control flotation machine were tested respectively, and the results showed that Outotec's intelligent control flotation machine had the best effect.
[0145] (5) Flotation parameter screening of Outotec's intelligent control flotation machine:
[0146] 1) Effect of aeration volume on flotation
[0147] The influence of different aeration amounts on the flotation index of the intelligent control flotation machine was investigated at a stirring speed of 800r / min. The results showed that as the aeration amount increased, the concentrate yield showed a gradually decreasing trend; after the aeration amount increased from 6.0L / min to 10.0L / min, the Fe grade of the concentrate increased from 71.69% to 71.86%, and the Al2O3 and SiO2 contents decreased from 0.20% and 0.18% to 0.17% and 0.14%, respectively. After continuing to increase the aeration amount, the separation indexes were not significantly optimized;
[0148] 2) Effect of stirring speed on flotation
[0149] Results: With the increase of stirring speed, the concentrate yield showed a trend of gradual decrease; after the stirring speed increased from 600 to 1500r / min, the concentrate yield decreased from 59.83% to 35.23%, the Fe grade increased from 71.82% to 71.91%, and the Al2O3 and SiO2 contents decreased to 0.18% and 0.14%. When the stirring speed was 1000r / min, the concentrate index was better;
[0150] 3) One rough and one fine flotation process
[0151] On the basis of roughing, a concentration operation was added, and the Fe grade of flotation concentrate continued to increase. When the concentration DDA dosage was 20g / t, the Fe grade of the concentrate was 71.89%, and the Al2O3 and SiO2 contents were 0.17% and 0.14% respectively; when the concentration DDA dosage was increased to 30g / t, the Fe grade of the concentrate was 71.96%, and the Al2O3 and SiO2 contents were 0.17% and 0.14% respectively; the Fe grade of the concentrate did not change much when the DDA dosage was further increased;
[0152] 4) One rough and two fine flotation process
[0153] On the basis of the flotation column coarse and fine flotation, one more concentration operation is added, and the Fe grade of the concentrate can be further increased to 71.99%, and the Al2O3 and SiO2 contents of the concentrate are 0.17% and 0.13% respectively;
[0154] 5) One rough and three fine flotation process
[0155] By adding one more concentration operation on the basis of the first coarse and second fine flotation, the Fe grade of the concentrate can be further increased to 72.04%, and the Al2O3 and SiO2 contents of the concentrate are 0.16% and 0.12% respectively;
[0156] 6) One rough and four fine flotation process
[0157] By adding another concentration operation on the basis of one rough and three fine flotation, the Fe grade of the concentrate can be further increased to 72.05%, and the Al2O3 and SiO2 contents of the concentrate are 0.16% and 0.11% respectively.
[0158] (6) Desulfurization collector selection test
[0159] The slurry pH is 6.0, the dosage of pineneol is 2 drops as a fixed parameter, the dosage of collector is set at 50g / t, and the effect of collector type on desulfurization is investigated. The results are as follows:
[0160]
[0161] It can be seen that when ethyl xanthate is used as the collector, the yield of S tailings is 0.45%, the Fe grade of the concentrate is increased from 72.101% to 72.103% when entering the flotation, and the contents of Al2O3 and SiO2 have no obvious changes; when pentyl xanthate is used as the collector, the yield of S tailings is 0.93%, the Fe grade of the concentrate is increased from 72.101% to 72.106% when entering the flotation, and the contents of Al2O3 and SiO2 in the concentrate are reduced to 0.151% and 0.070%, respectively. It can be seen that the collection capacity of pentyl xanthate is due to ethyl xanthate and butyl xanthate.
[0162] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for efficiently separating iron ore concentrate, characterized in that: The method comprises in sequence a gravity separation step, a magnetic separation step, a reverse flotation step and an alkali leaching step.
2. The method for efficiently separating iron ore concentrate according to claim 1, characterized in that: The re-selection and screening step is carried out using a shaking table, and the ore is ground using a ball mill.
3. The method for efficiently separating iron ore concentrate according to claim 1, characterized in that: The magnetic separation steps are five-stage magnetic separation column separation-grinding-three-stage magnetic separation column re-separation.
4. The method for efficiently separating iron ore concentrate according to claim 3, characterized in that: The process parameters during magnetic column separation are as follows: rising water flow rate is 5.7L / min~18L / min, preferably 15.6L / min; current is 0.25A~1.25A, preferably 1.00A; feeding rate is 50g / min~200g / min, preferably 100g / min; slurry concentration is 15wt.%~30wt.%, preferably 20wt.%, and the fineness of the grinding is -0.038mm, accounting for 99.73%.
5. The method for efficiently separating iron ore concentrate according to claim 3, characterized in that: After the three-stage magnetic separation column is re-selected, a two-stage shaking table is performed.
6. A method for efficiently separating iron ore concentrate according to claim 2 or 5, characterized in that: The process parameters of the shaking table operation are: flushing water flow rate is 2.5L / min~15L / min, preferably 12.5L / min, ore feeding rate is 60g / min~240g / min, preferably 120g / min, and the inclination angle is set at 1°~3°, preferably 2°.
7. The method for efficiently separating iron ore concentrate according to claim 1, characterized in that: The reverse flotation steps sequentially include reverse flotation desulfurization, reverse flotation desiliconization roughing and reverse flotation desiliconization cleaning.
8. The method for efficiently separating iron ore concentrate according to claim 7, characterized in that: During the reverse flotation desulfurization, the pH is adjusted to 6.0, the desulfurization agent is 50g / t of amyl xanthate, and terpineol is added; the reverse flotation desiliconization roughing and reverse flotation desiliconization cleaning both use dodecylamine as the reverse flotation collector, the aeration volume is 5.0L / min-10.0L / min, preferably 8.0L / min, the stirring speed is 600r / min-1000r / min, preferably 800r / min, and the amount of dodecylamine used is 50g / t-90g / t, preferably 60g / t.
9. The method for efficiently separating iron ore concentrate according to claim 1, characterized in that: Fine grinding is performed before the alkali leaching step, and the particle size after grinding is about -10 μm, accounting for 98.65%.
10. The method for efficiently separating iron ore concentrate according to claim 1, characterized in that: The process parameters of the alkali leaching are: the alkali is NaOH, and its dosage is 40g / L to 80g / L, preferably 80g / L; the leaching temperature is 150°C to 180°C; the pressure is 0Mpa to 3Mpa; the stirring speed is 400r / min to 800r / min; and the reaction time is 3h to 4h.