Antibacterial flame-retardant three-layer co-extrusion BOPP (biaxially-oriented polypropylene) film and preparation method thereof
The antibacterial flame-retardant BOPP film prepared by three-layer coextrusion process uses the material composition and process processing of specific proportions to solve the problems of flammable and poor antibacterial properties of traditional BOPP films, achieving efficient flame-retardant and antibacterial effects, which is suitable for use in the form of materials with specific proportions. Widely used.
Patent Information
- Application Number
- CN202411035429.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Traditional BOPP films are flammable and produce smoke when burned, and have poor antibacterial performance, making it difficult to meet the market's demand for flame retardant and antibacterial functions.
The three-layer co-extrusion process is used to prepare antibacterial flame retardant BOPP film, in which the upper surface layer, antibacterial flame retardant layer and lower surface layer are composed of polypropylene, antibacterial agent, flame retardant filler, antibacterial agent and other materials with specific ratios. The melt coextrusion and stretching process are formed to ensure flame retardant and antibacterial properties.
It has achieved efficient antibacterial flame retardant effect, and the flame retardant level reaches V-0. Antibacterial agents have significant antibacterial effects on bacteria. The product is safe and non-toxic, and is suitable for mass production and application.
Smart Images

Figure CN118952797A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of BOPP film processing, and in particular to an antibacterial and flame-retardant three-layer co-extruded BOPP film and a preparation method thereof. Background Art
[0002] The production of biaxially oriented polypropylene film (BOPP) is to first make the melt of high molecular weight polypropylene into sheets or thick films through a narrow and long die, and then stretch it in two perpendicular directions (longitudinal and transverse) at a certain temperature and set speed in a special stretching machine at the same time or in steps, and then undergo appropriate cooling or heat treatment or special processing (such as corona, coating, etc.) to make a film. The mechanical properties of the BOPP film formed by biaxial stretching are significantly improved, and the transparency, thermal properties, barrier properties, etc. have undergone certain changes, which can better meet the needs of many fields and is currently the most widely used printing film.
[0003] Due to the molecular orientation of the stretching of BOPP film, the BOPP film has high physical stability, high mechanical strength, toughness and wear resistance, and has the advantages of light weight, non-toxicity, odorlessness, good printing performance, and good transparency. However, the limiting oxygen index (LOI) of polypropylene is relatively low, only about 18%, which is easy to burn, and a large amount of smoke will be generated during the combustion process, which poses a great safety hazard. In addition, people have higher and higher requirements for healthy living, and antibacterial products are becoming more and more popular. However, the traditional BOPP film for packaging itself has problems with air permeability and water permeability, and the antibacterial effect is poor, which makes it easy to be eroded by mold and microorganisms.
[0004] Therefore, it is in line with the market development trend to modify BOPP and its related products to make them flame retardant and antibacterial and to prepare antibacterial and flame retardant BOPP films with integrated flame retardant and antibacterial functions, and this has broad application prospects. Summary of the invention
[0005] In order to solve the above problems, the purpose of the present invention is to provide an antibacterial and flame-retardant three-layer co-extruded BOPP film and a preparation method thereof. On the basis of the original BOPP film production process and equipment, suitable antibacterial and flame-retardant additives are selected to achieve good antibacterial and flame-retardant effects, thereby solving the problem of poor antibacterial and flame-retardant properties of BOPP film during the research and development process.
[0006] The invention discloses an antibacterial flame-retardant three-layer co-extruded BOPP film, which consists of an upper surface layer, an antibacterial flame-retardant layer and a lower surface layer from top to bottom.
[0007] Furthermore, the upper surface layer, the antibacterial and flame-retardant layer, and the lower surface layer of the antibacterial and flame-retardant three-layer co-extruded BOPP film are respectively prepared by melt co-extrusion.
[0008] Furthermore, the upper surface layer is made of the following raw materials in mass fraction: 95% to 99% polypropylene (PP), 0.5% to 2.5% anti-adhesive agent, and 0.5% to 2.5% lubricant;
[0009] Furthermore, the antibacterial flame retardant layer is made of the following raw materials in mass fraction: 85% to 95% polypropylene (PP), 3.7% to 10.5% flame retardant filler, 1% to 3% antibacterial agent, 0.1% to 0.5% antioxidant, 0.1% to 0.5% compatibilizer, and 0.1% to 0.5% dispersant;
[0010] Furthermore, the lower surface layer is made of the following raw materials in mass fractions: 95% to 99% of polypropylene (PP), 0.5% to 2.5% of an anti-adhesive agent, and 0.5% to 2.5% of a lubricant.
[0011] Furthermore, the thickness of the antibacterial flame retardant three-layer co-extruded BOPP film is 40-45 μm, the thickness of the upper surface layer accounts for 2.5%-5% of the total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film, the thickness of the antibacterial flame retardant layer accounts for 90%-95% of the total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film, and the thickness of the lower surface layer accounts for 2.5%-5% of the total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film.
[0012] Furthermore, the PP in the upper surface layer, the antibacterial flame retardant layer and the lower surface layer is isotactic polypropylene.
[0013] Furthermore, the anti-adhesive agent in the upper surface layer and the lower surface layer is at least one of silicon dioxide, talc and kaolin.
[0014] Furthermore, the lubricant in the upper surface layer and the lower surface layer is one of vinyl bisstearamide (EBS), erucamide, oleamide and polyethylene wax.
[0015] Furthermore, the antioxidant in the antibacterial flame retardant layer is one or more of antioxidant 168, antioxidant 1010 and antioxidant 1330, the compatibilizer is one of ethylene acrylic acid copolymer (EAA), ethylene-ethyl acrylate copolymer (EEA), and ethylene-vinyl acetate copolymer (EVA), and the dispersant is polyethylene glycol.
[0016] Furthermore, the flame retardant filler in the antibacterial flame retardant layer has the following specific steps for preparing the flame retardant filler:
[0017] S1, weigh a certain amount of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol in a reaction kettle, react at 70-90°C for 8-10h, and cool to room temperature to obtain solution A;
[0018] S2, filtering and washing the solution A in sequence, and then drying at 50-70° C. for 12-14 hours to obtain a cobalt-based metal organic framework / ammonium polyphosphate type flame retardant filler;
[0019] Furthermore, the mass ratio of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate and anhydrous ethanol in step S1 is (15-20): (30-40): (50-60): (90-100): (15-20): (110-120).
[0020] Furthermore, the specific steps of the preparation method of the antibacterial agent are as follows:
[0021] (1) weighing a certain amount of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water in a reaction kettle, reacting at a temperature of 90-110° C. for 8-12 hours, filtering to obtain a solid precipitate, drying the solid precipitate at a temperature of 50-70° C. for 10-12 hours, and then calcining at a temperature of 110-140° C. for 16-20 hours to obtain diatomaceous earth / zinc oxide;
[0022] (2) A certain amount of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water are measured and placed in a reaction vessel, reacted at 80-100° C. for 10-12 hours, the reaction product is filtered, and the solid obtained after filtration is dried at 50-60° C. for 10-12 hours to obtain a diatomaceous earth / zinc oxide / silver chloride type antibacterial agent.
[0023] Furthermore, the mass ratio of diatomaceous earth, zinc chloride, potassium hydroxide and deionized water in step (1) is (35-40):(5-8):(10-16):(125-135).
[0024] Furthermore, the mass ratio of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate and deionized water in step (2) is (24-28): (11-14): (18-22): (100-120).
[0025] The present invention also provides a method for manufacturing an antibacterial flame-retardant three-layer co-extruded BOPP film, which specifically comprises the following steps:
[0026] (1) Mixing: Mix the raw material components of the upper surface layer, the antibacterial flame retardant layer and the lower surface layer in proportion, and disperse them evenly by a high-speed mixer;
[0027] (2) Extrusion: adding the uniformly dispersed raw materials of the antibacterial flame retardant layer to a main extruder for melt extrusion, filtering through a filter screen to obtain an antibacterial flame retardant layer melt; adding the raw materials of the upper surface layer to a first auxiliary extruder, and adding the raw materials of the lower surface layer to a second auxiliary extruder for melt extrusion, respectively, and filtering through a filter screen to obtain an upper surface layer melt and a lower surface layer melt, respectively;
[0028] (3) Casting: The upper surface layer melt, the antibacterial flame retardant layer melt, and the lower surface layer melt are extruded from the die lip of the three-layer structure extruder in order from top to bottom, and cast onto the surface of the chilled roller to form a cast sheet under the action of the chilled roller, the water bath, and the guide roller;
[0029] (4) Stretching: The cast film is drawn out and stretched longitudinally by the stretching rollers with different roller speeds in front and behind the longitudinal stretching machine and the heating roller in the middle; then it passes through the transverse stretching machine, clamps both sides of the film with chain clamps, moves forward along a gradually widening track, passes through the heating area and the shaping area, and the width of the film is increased;
[0030] (5) Traction and reeling: After edge trimming, thickness measurement and corona treatment, the film is rolled into a cylindrical film roll.
[0031] Furthermore, in step (2), the melt extrusion temperature of the main extruder is 225-235°C, the melt extrusion temperature of the first auxiliary extruder is 215°C-225°C, and the melt extrusion temperature of the second auxiliary extruder is 220°C-230°C;
[0032] Furthermore, in step (3), the surface temperature of the chilled roller is 15 to 35°C;
[0033] Furthermore, in step (4), the longitudinal stretching temperature is 65-75°C, and the transverse stretching temperature is 145-155°C;
[0034] Furthermore, in step (4), the longitudinal stretching ratio is 1.5-2.5 times, and the transverse stretching ratio is 6.5-7.5 times;
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) Highly effective antibacterial and flame retardant properties. The prepared diatomaceous earth / zinc oxide / silver chloride type antibacterial agent has a highly effective antibacterial effect on Escherichia coli and Staphylococcus aureus, and the antibacterial effect is significant; while the cobalt-based metal organic framework / ammonium polyphosphate type flame retardant filler has excellent flame retardant properties, and the vertical burning test (UL94) can reach V-0 level. The obtained product is safe and non-toxic, the preparation method is simple, the raw materials are easily available, and it can be mass-produced. It can be compounded with polymer materials to prepare packaging materials with antibacterial and flame retardant effects.
[0037] (2) The antibacterial mechanism of the antibacterial agent of the present invention is as follows: the antibacterial agent uses diatomaceous earth as a carrier. The silver chloride in diatomaceous earth / zinc oxide / silver chloride is positively charged when it meets water, and exhibits positive affinity when it meets negatively charged Escherichia coli, which facilitates inducing bacteria to aggregate on the surface of the material, and then releases Ag. +It destroys the cell membrane of E. coli, thus killing the bacteria. As an inorganic antibacterial agent, ZnO has high thermal stability and resistance to UV aging, and is one of the safest inorganic antibacterial agents. Diatomaceous earth-loaded ZnO releases more active oxygen under the same conditions, and has a better antibacterial effect. In summary, the synergistic antibacterial properties of diatomaceous earth / zinc oxide / silver chloride make it have excellent antibacterial properties.
[0038] (3) The flame retardant mechanism of the flame retardant filler of the present invention is as follows: the porous structure of the cobalt-based metal organic framework can limit the diffusion of the matrix from the inside to the combustion surface, thereby achieving the purpose of inhibiting combustion. In the solid phase, the heat-resistant cobalt-based metal organic framework acts as a thermal barrier, and its decomposition requires a large amount of heat. The porous metal oxide produced during the combustion process can not only delay the diffusion of heat, but also inhibit the release of the matrix from the solid phase to the combustion area. Ammonium polyphosphate can not only inhibit the volatilization of flammable substances and the formation of new free radicals, but also reduce the diffusion of oxygen, so ammonium polyphosphate plays a flame retardant role in both the solid phase and the gas phase. This synergistic effect makes the cobalt-based metal organic framework / ammonium polyphosphate type flame retardant filler have efficient flame retardant properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Schematic diagram of the structure of the antibacterial flame retardant three-layer co-extruded BOPP film of the present invention, in which: 1 is the upper surface layer, 2 is the antibacterial flame retardant layer, and 3 is the lower surface layer; DETAILED DESCRIPTION
[0040] In order to better understand the content of the present invention, the present invention will be further described below in conjunction with specific embodiments and drawings. The following embodiments are implemented based on the technology of the present invention, and detailed implementation methods and operating steps are given, but the protection scope of the present invention is not limited to the following embodiments.
[0041] In the following examples and comparative examples, the materials used are:
[0042] Isotactic polypropylene, Daqing Refining and Chemical Company of China National Petroleum Corporation; cobalt nitrate, Shandong Changyao New Materials Co., Ltd.; triethylamine, Shandong Polychemical Co., Ltd.; 4,4'-diaminodiphenylmethane, Shandong Chenyu Chemical Co., Ltd.; anhydrous ethanol, Shanghai Fangye Chemical Co., Ltd.; salicylaldehyde, Jinan Wenzhu Chemical Co., Ltd.; ammonium polyphosphate, Jiangsu Xinsu New Materials Co., Ltd.; zinc chloride, Shandong Desheng New Materials Co., Ltd.; diatomaceous earth, Chongqing Shihuan Mining Co., Ltd.; silver nitrate, Shandong Xuxiang Chemical Co., Ltd.; potassium chloride, Jinan Qinghai Chemical Co., Ltd.; silver nitrate, Shandong Xuxiang Chemical Co., Ltd.; antioxidants (antioxidant 168, antioxidant 1010, antioxidant 1330), BASF. Other raw materials not otherwise specified were purchased from commercial sources or prepared by conventional methods in the art.
[0043] Embodiment 1:
[0044] The antibacterial flame retardant three-layer co-extruded BOPP film described in this embodiment is composed of an upper surface layer, an antibacterial flame retardant layer, and a lower surface layer arranged from top to bottom, and the upper surface layer, the antibacterial flame retardant layer, and the lower surface layer are respectively prepared by melt co-extrusion.
[0045] The antibacterial flame retardant three-layer co-extruded BOPP film has the following components, calculated by mass: the upper surface layer comprises 95% isotactic polypropylene, 2.5% silica, and 2.5% EBS; the antibacterial flame retardant layer comprises 85% isotactic polypropylene, 10.5% flame retardant filler, 3% antibacterial agent, 0.5% antioxidant 168, 0.5% EAA, and 0.5% polyethylene glycol; the lower surface layer comprises 95% isotactic polypropylene, 2.5% silica, and 2.5% EBS.
[0046] The total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film is 40 μm, the thickness of the upper surface layer accounts for 5% of the total thickness, the thickness of the antibacterial flame retardant layer accounts for 90% of the total thickness, and the thickness of the lower surface layer accounts for 5% of the total thickness.
[0047] In this embodiment, the preparation method of the flame retardant filler in the antibacterial flame retardant layer comprises the following specific steps:
[0048] S1, taking a certain amount of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol and placing them in a reactor, reacting at 70°C for 8 hours, and cooling to room temperature after the reaction to obtain solution A, wherein the mass ratio of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol is 15:30:50:90:15:110;
[0049] S2, filtering and washing the solution A in sequence, and then drying at 50° C. for 12 h to obtain a cobalt-based metal organic framework / ammonium polyphosphate type flame retardant filler;
[0050] In this embodiment, the specific steps of the preparation method of the antibacterial agent are as follows:
[0051] (1) taking a certain amount of diatomaceous earth, zinc chloride, potassium hydroxide and deionized water and placing them in a reaction kettle, reacting them at 90° C. for 8 hours, filtering to obtain a solid precipitate, drying the solid precipitate at 50° C. for 10 hours, and then calcining at 110° C. for 16 hours to obtain diatomaceous earth / zinc oxide, wherein the mass ratio of diatomaceous earth, zinc chloride, potassium hydroxide and deionized water is 35:5:10:125;
[0052] (2) taking a certain amount of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate and deionized water obtained in step (1), placing them in a reaction vessel, reacting them at 80° C. for 10 h, filtering the reaction product, and drying the solid obtained after filtration at 50° C. for 10 h to obtain a diatomaceous earth / zinc oxide / silver chloride type antibacterial agent, wherein the mass ratio of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate and deionized water is 24:11:18:100.
[0053] The method for manufacturing the antibacterial flame-retardant three-layer co-extruded BOPP film in this embodiment specifically comprises the following steps:
[0054] (1) Mixing: The raw material components of the upper surface layer, the antibacterial flame retardant layer and the lower surface layer are mixed in proportion and dispersed evenly by a high-speed mixer;
[0055] (2) Extrusion: adding the uniformly dispersed raw materials of the antibacterial flame retardant layer to a main extruder for melt extrusion, filtering through a filter screen to obtain an antibacterial flame retardant melt; adding the raw materials of the upper surface layer to a first auxiliary extruder, and adding the raw materials of the lower surface layer to a second auxiliary extruder for melt extrusion, respectively, and then filtering through a filter screen to obtain an upper surface layer melt and a lower surface layer melt, respectively; wherein the melt extrusion temperature of the main extruder is 230° C., the melt extrusion temperature of the first auxiliary extruder is 220° C., and the melt extrusion temperature of the second auxiliary extruder is 225° C.;
[0056] (3) Casting: The upper surface layer melt, the antibacterial flame retardant layer melt, and the lower surface layer melt are extruded from the die lip of the three-layer structure extruder in order from top to bottom, and cast onto the surface of a chilled roller, the surface temperature of the chilled roller is 25° C., and a cast sheet is formed under the action of the chilled roller, a water bath, and a guide roller;
[0057] (4) Stretching: The cast film is drawn out and stretched longitudinally by the stretching rollers with different roller speeds in front and behind the longitudinal stretching machine and the heating roller in the middle; then it passes through the transverse stretching machine, clamps both sides of the film with chain clamps, moves forward along a gradually widening track, passes through the heating area and the shaping area, and the width of the film is increased; wherein the longitudinal stretching temperature is 70°C and the transverse stretching temperature is 150°C;
[0058] (5) Traction and reeling: After trimming, thickness measurement and corona treatment, the film is rolled into a cylindrical film roll, in which the longitudinal stretching ratio is 1.5 times and the transverse stretching ratio is 6.5 times.
[0059] Embodiment 2:
[0060] The antibacterial flame retardant three-layer co-extruded BOPP film described in this embodiment is composed of an upper surface layer, an antibacterial flame retardant layer, and a lower surface layer arranged from top to bottom, and the upper surface layer, the antibacterial flame retardant layer, and the lower surface layer are respectively prepared by melt co-extrusion.
[0061] The antibacterial flame retardant three-layer co-extruded BOPP film has the following components, calculated by mass: the upper surface layer comprises 96% isotactic polypropylene, 2% silica, and 2% EBS; the antibacterial flame retardant layer comprises 87.5% isotactic polypropylene, 8.8% flame retardant filler, 2.5% antibacterial agent, 0.4% antioxidant 168, 0.4% EAA, and 0.4% polyethylene glycol; the lower surface layer comprises 96% isotactic polypropylene, 2% silica, and 2% EBS.
[0062] The total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film is 40 μm, the thickness of the upper surface layer accounts for 5% of the total thickness, the thickness of the antibacterial flame retardant layer accounts for 90% of the total thickness, and the thickness of the lower surface layer accounts for 5% of the total thickness.
[0063] In this embodiment, the preparation method of the flame retardant filler in the antibacterial flame retardant layer comprises the following specific steps:
[0064] S1, weigh a certain amount of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol and place them in a reactor, react at 75°C for 8.5 hours, and cool to room temperature after the reaction to obtain solution A, wherein the mass ratio of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol is 16:32:52:92:16:112;
[0065] S2, filtering and washing the solution A in sequence, and then drying at 55° C. for 12.5 hours to obtain a cobalt-based metal organic framework / ammonium polyphosphate type flame retardant filler;
[0066] In this embodiment, the specific steps of the preparation method of the antibacterial agent are as follows:
[0067] (1) taking a certain amount of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water and placing them in a reactor, reacting them at 95° C. for 8.5 hours, filtering to obtain a solid precipitate, drying the solid precipitate at 55° C. for 10.5 hours, and then calcining at 110° C. for 17 hours to obtain diatomaceous earth / zinc oxide, wherein the mass ratio of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water is 36:6:12:130;
[0068] (2) A certain amount of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water obtained in step (1) are measured and placed in a reaction vessel, reacted at 85° C. for 10.5 hours, the reaction product is filtered, and the solid obtained after filtration is dried at 55° C. for 10.5 hours to obtain a diatomaceous earth / zinc oxide / silver chloride type antibacterial agent, wherein the mass ratio of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water is 25:12:19:112.
[0069] The method for manufacturing the antibacterial and flame-retardant three-layer co-extruded BOPP film in this embodiment is the same as that in Example 1.
[0070] Embodiment 3:
[0071] The antibacterial flame retardant three-layer co-extruded BOPP film described in this embodiment is composed of an upper surface layer, an antibacterial flame retardant layer, and a lower surface layer arranged from top to bottom, and the upper surface layer, the antibacterial flame retardant layer, and the lower surface layer are respectively prepared by melt co-extrusion.
[0072] The antibacterial and flame-retardant three-layer co-extruded BOPP film has the following components, calculated by mass: the upper surface layer comprises 97% isotactic polypropylene, 1.5% silica, and 1.5% EBS; the antibacterial and flame-retardant layer comprises 90% isotactic polypropylene, 7.1% flame-retardant filler, 2% antibacterial agent, 0.3% antioxidant 168, 0.3% EAA, and 0.3% polyethylene glycol; the lower surface layer comprises 97% isotactic polypropylene, 1.5% silica, and 1.5% EBS.
[0073] The total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film is 40 μm, the thickness of the upper surface layer accounts for 5% of the total thickness, the thickness of the antibacterial flame retardant layer accounts for 90% of the total thickness, and the thickness of the lower surface layer accounts for 5% of the total thickness.
[0074] In this embodiment, the preparation method of the flame retardant filler in the antibacterial flame retardant layer comprises the following specific steps:
[0075] S1, measuring a certain amount of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol and placing them in a reactor, reacting at 80°C for 9 hours, and cooling to room temperature after the reaction to obtain solution A, wherein the mass ratio of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol is 18:35:55:95:18:115;
[0076] S2, filtering and washing the solution A in sequence, and then drying at 60° C. for 13 h to obtain a cobalt-based metal organic framework / ammonium polyphosphate type flame retardant filler;
[0077] In this embodiment, the specific steps of the preparation method of the antibacterial agent are as follows:
[0078] (1) taking a certain amount of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water and placing them in a reactor, reacting them at 100° C. for 10 hours, filtering to obtain a solid precipitate, drying the solid precipitate at 60° C. for 11 hours, and then calcining at 120° C. for 18 hours to obtain diatomaceous earth / zinc oxide, wherein the mass ratio of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water is 37:7:15:130;
[0079] (2) taking a certain amount of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water obtained in step (1), placing them in a reaction vessel, reacting at 90° C. for 11 h, filtering the reaction product, and drying the solid obtained after filtration at 55° C. for 11 h to obtain a diatomaceous earth / zinc oxide / silver chloride type antibacterial agent, wherein the mass ratio of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water is 26:13:20:110.
[0080] The method for manufacturing the antibacterial and flame-retardant three-layer co-extruded BOPP film in this embodiment is the same as that in Example 1.
[0081] Embodiment 4:
[0082] The antibacterial flame retardant three-layer co-extruded BOPP film described in this embodiment is composed of an upper surface layer, an antibacterial flame retardant layer, and a lower surface layer arranged from top to bottom, and the upper surface layer, the antibacterial flame retardant layer, and the lower surface layer are respectively prepared by melt co-extrusion.
[0083] The antibacterial flame retardant three-layer co-extruded BOPP film has the following components, calculated by mass: the upper surface layer comprises 98% isotactic polypropylene, 1% silica, and 1% EBS; the antibacterial flame retardant layer comprises 92.5% isotactic polypropylene, 5.4% flame retardant filler, 1.5% antibacterial agent, 0.2% antioxidant 168, 0.2% EAA, and 0.2% polyethylene glycol; the lower surface layer comprises 98% isotactic polypropylene, 1% silica, and 1% EBS.
[0084] The total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film is 40 μm, the thickness of the upper surface layer accounts for 5% of the total thickness, the thickness of the antibacterial flame retardant layer accounts for 90% of the total thickness, and the thickness of the lower surface layer accounts for 5% of the total thickness.
[0085] In this embodiment, the preparation method of the flame retardant filler in the antibacterial flame retardant layer comprises the following specific steps:
[0086] S1, measuring a certain amount of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol and placing them in a reactor, reacting at 85°C for 9.5 hours, and cooling to room temperature after the reaction to obtain solution A, wherein the mass ratio of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol is 15:40:55:100:20:115;
[0087] S2, filtering and washing the solution A in sequence, and then drying at 65° C. for 13.5 h to obtain a cobalt-based metal organic framework / ammonium polyphosphate type flame retardant filler;
[0088] In this embodiment, the specific steps of the preparation method of the antibacterial agent are as follows:
[0089] (1) taking a certain amount of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water and placing them in a reaction kettle, reacting them at 105° C. for 11 hours, filtering to obtain a solid precipitate, drying the solid precipitate at 65° C. for 11.5 hours, and then calcining at 130° C. for 19 hours to obtain diatomaceous earth / zinc oxide, wherein the mass ratio of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water is 35:8:15:130;
[0090] (2) A certain amount of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water obtained in step (1) were measured and placed in a reaction vessel, reacted at 95° C. for 11.5 hours, the reaction product was filtered, and the solid obtained after filtration was dried at 55° C. for 11.5 hours to obtain a diatomaceous earth / zinc oxide / silver chloride type antibacterial agent, wherein the mass ratio of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water was 27:14:21:115.
[0091] The method for manufacturing the antibacterial and flame-retardant three-layer co-extruded BOPP film in this embodiment is the same as that in Example 1.
[0092] Embodiment 5:
[0093] The antibacterial flame retardant three-layer co-extruded BOPP film described in this embodiment is composed of an upper surface layer, an antibacterial flame retardant layer, and a lower surface layer arranged from top to bottom, and the upper surface layer, the antibacterial flame retardant layer, and the lower surface layer are respectively prepared by melt co-extrusion.
[0094] The antibacterial and flame-retardant three-layer co-extruded BOPP film has the following components, calculated by mass: the upper surface layer comprises 99% isotactic polypropylene, 0.5% silica, and 0.5% EBS; the antibacterial and flame-retardant layer comprises 95% isotactic polypropylene, 3.7% flame-retardant filler, 1% antibacterial agent, 0.1% antioxidant 168, 0.1% EAA, and 0.1% polyethylene glycol; and the lower surface layer comprises 99% isotactic polypropylene, 0.5% silica, and 0.5% EBS.
[0095] The total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film is 40 μm, the thickness of the upper surface layer accounts for 5% of the total thickness, the thickness of the antibacterial flame retardant layer accounts for 90% of the total thickness, and the thickness of the lower surface layer accounts for 5% of the total thickness.
[0096] In this embodiment, the preparation method of the flame retardant filler in the antibacterial flame retardant layer comprises the following specific steps:
[0097] S1, taking a certain amount of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol and placing them in a reactor, reacting at 90°C for 10 hours, and cooling to room temperature after the reaction to obtain solution A, wherein the mass ratio of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol is 15:40:60:100:20:120;
[0098] S2, filtering and washing the solution A in sequence, and then drying at 70° C. for 14 h to obtain a cobalt-based metal organic framework / ammonium polyphosphate type flame retardant filler;
[0099] In this embodiment, the specific steps of the preparation method of the antibacterial agent are as follows:
[0100] (1) taking a certain amount of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water and placing them in a reaction kettle, reacting them at 110° C. for 12 hours, filtering to obtain a solid precipitate, drying the solid precipitate at 70° C. for 12 hours, and then calcining at 140° C. for 20 hours to obtain diatomaceous earth / zinc oxide, wherein the mass ratio of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water is 40:5:15:125;
[0101] (2) taking a certain amount of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water obtained in step (1), placing them in a reaction vessel, reacting them at 100° C. for 12 h, filtering the reaction product, and drying the solid obtained after filtration at 60° C. for 12 h to obtain a diatomaceous earth / zinc oxide / silver chloride type antibacterial agent, wherein the mass ratio of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water is 25:12:20:120.
[0102] The method for manufacturing the antibacterial and flame-retardant three-layer co-extruded BOPP film in this embodiment is the same as that in Example 1.
[0103] Comparative Example 1:
[0104] According to the structural composition of the antibacterial flame retardant three-layer co-extruded BOPP film in Example 1, the antibacterial flame retardant layer in this comparative example is made of the following raw materials in mass fraction: 98.5% isotactic polypropylene, 0.5% antioxidant, 0.5% compatibilizer, and 0.5% dispersant; the rest is the same as in Example 1.
[0105] The method for manufacturing the antibacterial and flame-retardant three-layer co-extruded BOPP film in this comparative example is the same as that in Example 1.
[0106] Comparative Example 2:
[0107] According to the structural composition of the antibacterial flame retardant three-layer co-extruded BOPP film in Example 1, the antibacterial flame retardant layer in this comparative example is made of the following raw materials in mass fraction: 88% isotactic polypropylene, 10.5% flame retardant filler, 0.5% antioxidant, 0.5% compatibilizer, and 0.5% dispersant; the rest is the same as in Example 1.
[0108] The method for manufacturing the antibacterial and flame-retardant three-layer co-extruded BOPP film in this comparative example is the same as that in Example 1.
[0109] Comparative Example 3:
[0110] According to the structural composition of the antibacterial flame retardant three-layer co-extruded BOPP film in Example 1, the antibacterial flame retardant layer in this comparative example is made of the following raw materials in mass fraction: 95.5% isotactic polypropylene, 3% antibacterial agent, 0.5% antioxidant, 0.5% compatibilizer, and 0.5% dispersant; the rest is the same as in Example 1.
[0111] The method for manufacturing the antibacterial and flame-retardant three-layer co-extruded BOPP film in this comparative example is the same as that in Example 1.
[0112] The performance of the antibacterial flame retardant three-layer co-extruded BOPP films prepared in Examples 1-5 and Comparative Examples 1-3 was tested, and the test results are shown in Table 1:
[0113] Table 1 Performance test results of the antibacterial flame retardant three-layer co-extruded BOPP films in Examples 1-5 and Comparative Examples 1-3
[0114]
[0115] As can be seen from Table 1, compared with Comparative Examples 1 and 2, Examples 1-5 have excellent antibacterial properties, and the antibacterial rate against Staphylococcus aureus can reach more than 99%, and the antibacterial rate against Escherichia coli can reach more than 98%; compared with Comparative Examples 1 and 3, Examples 1-5 have excellent flame retardant properties, and the flame retardant grade can reach V-0. In summary, the antibacterial flame retardant BOPP film prepared by the method provided by the present invention has excellent antibacterial and flame retardant properties, and can be extended to the application field of antibacterial flame retardant BOPP film.
[0116] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. An antibacterial flame retardant three-layer co-extruded BOPP film, It is characterized in that The invention is composed of an upper surface layer, an antibacterial flame retardant layer and a lower surface layer, wherein the upper surface layer, the antibacterial flame retardant layer and the lower surface layer are respectively prepared by melt co-extrusion; the antibacterial flame retardant layer is made of the following raw materials in mass fraction: 85% to 95% of polypropylene, 3.7% to 10.5% of flame retardant filler, 1% to 3% of antibacterial agent, 0.1% to 0.5% of antioxidant, 0.1% to 0.5% of compatibilizer and 0.1% to 0.5% of dispersant.
2. The antibacterial flame retardant three-layer co-extruded BOPP film according to claim 1, It is characterized in that The upper surface layer is made of the following raw materials in mass fraction: 95% to 99% polypropylene, 0.5% to 2.5% anti-adhesive agent, and 0.5% to 2.5% lubricant; the lower surface layer is made of the following raw materials in mass fraction: 95% to 99% polypropylene, 0.5% to 2.5% anti-adhesive agent, and 0.5% to 2.5% lubricant.
3. The antibacterial flame retardant three-layer co-extruded BOPP film according to claim 1, It is characterized in that The thickness of the antibacterial flame retardant three-layer co-extruded BOPP film is 40-45 μm, the thickness of the upper surface layer accounts for 2.5%-5% of the total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film, the thickness of the antibacterial flame retardant layer accounts for 90%-95% of the total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film, and the thickness of the lower surface layer accounts for 2.5%-5% of the total thickness of the antibacterial flame retardant three-layer co-extruded BOPP film.
4. The antibacterial flame retardant three-layer co-extruded BOPP film according to claim 2, It is characterized in that The polypropylene in the upper surface layer and the lower surface layer is isotactic polypropylene, the anti-adhesive agent is at least one of silicon dioxide, talc and kaolin, and the lubricant is one of vinyl bisstearamide, erucamide, oleamide and polyethylene wax.
5. The antibacterial flame retardant three-layer co-extruded BOPP film according to claim 1, It is characterized in that The polypropylene in the antibacterial flame retardant layer is isotactic polypropylene, the antioxidant is one or more of antioxidant 168, antioxidant 1010 and antioxidant 1330, the compatibilizer is one of ethylene acrylic acid copolymer, ethylene-ethyl acrylate copolymer, and ethylene-vinyl acetate copolymer, and the dispersant is polyethylene glycol.
6. The antibacterial flame retardant three-layer co-extruded BOPP film according to claim 1, It is characterized in that The flame retardant filler in the antibacterial flame retardant layer has the following specific steps for preparing the flame retardant filler: S1, weigh a certain amount of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol in a reaction kettle, react at 70-90°C for 8-10h, and cool to room temperature to obtain solution A, wherein the mass ratio of cobalt nitrate, triethylamine, 4,4'-diaminodiphenylmethane, salicylaldehyde, ammonium polyphosphate, and anhydrous ethanol is (15-20): (30-40): (50-60): (90-100): (15-20): (110-120); S2, filtering and washing the solution A in sequence, and then drying at 50-70° C. for 12-14 hours to obtain a cobalt-based metal organic framework / ammonium polyphosphate type flame retardant filler.
7. The antibacterial flame retardant three-layer co-extruded BOPP film according to claim 1, It is characterized in that The specific steps of the preparation method of the antibacterial agent are as follows: (1) weighing a certain amount of diatomaceous earth, zinc chloride, potassium hydroxide, and deionized water in a reaction kettle, reacting at a temperature of 90-110° C. for 8-12 hours, filtering to obtain a solid precipitate, drying the solid precipitate at a temperature of 50-70° C. for 10-12 hours, and then calcining at a temperature of 110-140° C. for 16-20 hours to obtain diatomaceous earth / zinc oxide; (2) A certain amount of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate, and deionized water are measured and placed in a reaction vessel, reacted at 80-100° C. for 10-12 hours, the reaction product is filtered, and the solid obtained after filtration is dried at 50-60° C. for 10-12 hours to obtain a diatomaceous earth / zinc oxide / silver chloride type antibacterial agent.
8. The method for preparing the antibacterial flame retardant three-layer co-extruded BOPP film according to any one of claims 1 to 7, It is characterized in that The specific steps include: (1) Mixing: Mix the raw material components of the upper surface layer, the antibacterial flame retardant layer and the lower surface layer in proportion, and disperse them evenly by a high-speed mixer; (2) Extrusion: adding the uniformly dispersed raw materials of the antibacterial flame retardant layer to a main extruder for melt extrusion, filtering through a filter screen to obtain an antibacterial flame retardant layer melt; adding the raw materials of the upper surface layer to a first auxiliary extruder, and adding the raw materials of the lower surface layer to a second auxiliary extruder for melt extrusion, respectively, and filtering through a filter screen to obtain an upper surface layer melt and a lower surface layer melt, respectively; (3) Casting: The upper surface layer melt, the antibacterial flame retardant layer melt, and the lower surface layer melt are extruded from the die lip of the three-layer structure extruder in order from top to bottom, and cast onto the surface of the chilled roller to form a cast sheet under the action of the chilled roller, the water bath, and the guide roller; (4) Stretching: The cast film is drawn out and stretched longitudinally by the stretching rollers with different roller speeds in front and behind the longitudinal stretching machine and the heating roller in the middle; then it passes through the transverse stretching machine, clamps both sides of the film with chain clamps, moves forward along a gradually widening track, passes through the heating area and the shaping area, and the width of the film is increased; (5) Traction and reeling: After edge trimming, thickness measurement and corona treatment, the film is rolled into a cylindrical film roll.
9. The preparation method according to claim 8, It is characterized in that The mass ratio of diatomaceous earth, zinc chloride, potassium hydroxide and deionized water in step (1) is (35-40): (5-8): (10-16): (125-135); the mass ratio of diatomaceous earth / zinc oxide, potassium chloride, silver nitrate and deionized water in step (2) is (24-28): (11-14): (18-22): (100-120).
10. The preparation method according to claim 8, It is characterized in that In step (2), the melt extrusion temperature of the main extruder is 225-235°C, the melt extrusion temperature of the first auxiliary extruder is 215°C-225°C, and the melt extrusion temperature of the second auxiliary extruder is 220°C-230°C; in step (3), the surface temperature of the chilled roller is 15-35°C; in step (4), the longitudinal stretching temperature is 65-75°C, the transverse stretching temperature is 145-155°C, the longitudinal stretching ratio is 1.5-2.5 times, and the transverse stretching ratio is 6.5-7.5 times.
Citation Information
Patent Citations
Antibacterial flame-retardant BOPP (biaxially-oriented polypropylene) film and preparation method thereof
CN114211722A
Cited By
Pearlised film with flame-retardant and antibacterial functions as well as preparation method and application of pearlised film
CN120699299A