Preparation method of double-layer carbon-coated spherical nano lithium iron phosphate positive electrode material

Through the preparation method of double-layer carbon-covered spherical nano lithium iron phosphate positive electrode material, the problems of low-temperature performance and high specific surface area of ​​lithium iron phosphate materials are solved, and high structural stability and low-cost processing performance are improved, which significantly improves the Electrolyte transfer and power performance.

CN118954465APending Publication Date: 2024-11-15NANTONG RESHINE NEW MATERIAL CO LTD +1

Patent Information

Application Number
CN202411130631.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The poor low-temperature performance and high specific surface area of ​​lithium iron phosphate positive electrode materials lead to poor processing performance and high cost.

Method used

The preparation method of double-layer carbon-coated spherical nano lithium iron phosphate positive electrode material is adopted, and the porous mesh structure is formed through primary sintering, and secondary carbon coating is subsequently carried out, and low-cost double-layer carbon coating is achieved by filtration and vibration drying. Reduce specific surface area and improve structural stability and processing performance.

Benefits of technology

It significantly improves the circulation and processing performance of the material, reduces costs, increases screening and iron removal capacity, improves the electrolyte transmission and power performance, and solves the processing problem of difficult dispersion of nanomaterials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954465A_ABST
    Figure CN118954465A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of a production process of a lithium battery positive electrode material, and particularly discloses a preparation method of a double-layer carbon-coated spherical nano lithium iron phosphate positive electrode material. Comprising the following steps: 1) primary sintering: mixing an iron source, a lithium source, an additive and a first part of carbon source with a solvent to form primary mixed slurry, grinding and drying, and performing primary sintering to obtain a porous and stable grid structure primary sintered material; and 2) secondary sintering: mixing the primary sintering material with a second part of the carbon source and the solvent to obtain secondary mixed slurry, and carrying out secondary sintering after filter pressing and drying. A lithium iron phosphate precursor with a stable structure and a net structure is prepared by regulating and controlling the addition amount of a carbon source and performing primary sintering, then double-layer coating of carbon is realized through secondary wet coating, and sanding and spray drying equipment is not needed in the secondary wet coating, so that the number of small particles in a material system is remarkably reduced, the specific surface of the material is smaller, and the specific surface area of the material is smaller. And meanwhile, the cost can be obviously reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium battery positive electrode material production process, and in particular to a method for preparing a double-layer carbon-coated spherical nano lithium iron phosphate positive electrode material. Background Art

[0002] There are many types of positive electrode materials for lithium-ion batteries, including ternary positive electrode materials, lithium iron phosphate, lithium manganese oxide, etc. Among them, ternary positive electrode materials are expensive and have poor safety due to the presence of rare metal elements such as nickel and cobalt. Phosphate positive electrode materials such as lithium iron phosphate have the advantages of high safety, long cycle and low cost, and the market capacity is constantly increasing. However, lithium iron phosphate itself has a low energy density and poor low-temperature performance, and its application in cold regions is limited.

[0003] In order to solve the problem of poor low-temperature performance of lithium iron phosphate materials, the industry usually adopts nano-processing methods, including the use of liquid phase methods, so that the primary particles of the material are reduced to below 200nm. However, the conventional process usually puts all the raw materials into the batching at one time, and then mixes and sands them. In order to achieve nano-processing, it takes a long time to grind, and then sinter. After sintering, the material is air-flow crushed. Since the primary particles are very small, the crushing capacity of this material is very low, and the viscosity of the material increases after crushing, the fluidity becomes worse, the subsequent screening capacity is very low, the iron removal effect is very poor, and the cost is now increased. In addition, the specific surface area of ​​this material will be very large, and the processing performance of the slurry is very poor when batching at the battery end, which affects the preparation of the pole piece.

[0004] In the Chinese patent application CN202211516678.6, a lithium iron phosphate composite positive electrode material and its preparation method and application are disclosed, and the preparation method comprises the following steps: mixing an iron source, a phosphorus source, a lithium source and a primary carbon source to obtain a precursor; the primary carbon source comprises a combination of at least two carbon-containing substances; sintering the precursor once to obtain an intermediate; mixing the intermediate with a secondary carbon source and performing secondary sintering to obtain the lithium iron phosphate composite positive electrode material. The present invention makes the obtained lithium iron phosphate composite positive electrode material have excellent electrochemical properties through the design of raw materials and process routes and their synergistic effect, especially in terms of conductivity and rate performance. The preparation method has a simple process, a wide range of raw materials, no expensive and complex instruments and equipment, and no harsh reaction conditions. It is easy to achieve large-scale industrial production and has broad industrialization prospects. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the prior art and propose a method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material, comprising: A method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material, characterized in that it comprises the steps of: 1) Primary sintering: The iron source, lithium source, additive and the first part of carbon source are mixed with a solvent to form a primary mixed slurry, and the slurry is ground, dried and then sintered to obtain a porous and structurally stable grid structure primary sintered material. The D50 of the slurry after grinding is 0.15-0.6 μm, and the primary sintered material has a mesh structure. Compared with conventional processes, it has higher structural stability, can ensure that the structure is not broken in subsequent processing, is more conducive to the transmission of the electrolyte, and improves the processing performance of the material and the lithium ion diffusion rate.

[0006] Only part of the carbon source is added during the first batching, so that the residual lithium of the material after the first sintering is between 0.4 and 1.0, and the material after the first sintering becomes porous (see Figure 1 ), a stable network structure is formed between the primary particles; then the primary sintered material is evenly mixed with the second part of the carbon source and water, and the solvent containing the carbon source is adsorbed into the interior and surface of the particles by utilizing the porous characteristics of the primary sintered material to achieve secondary carbon coating, and then a secondary carbon-coated porous lithium iron phosphate positive electrode material is obtained after sintering.

[0007] 2) Secondary sintering: the primary sintered material is mixed with the second part of the carbon source and the solvent to obtain a secondary mixed slurry, the secondary mixed slurry is filtered and then dried, and then secondary sintered after drying to obtain a secondary sintered material.

[0008] As mentioned above, the network structure between the primary particles after the first sintering is not destroyed during the second carbon coating, which ensures the structural stability of the material particles while achieving wet carbon coating. The specific surface area of ​​the product is significantly reduced, and the subsequent processing performance of the product is significantly improved.

[0009] The filter press can be carried out using a plate and frame vertical or horizontal filter press or other forms of filtering equipment, such as a centrifuge. During the filter press, the moisture content is controlled according to the content of the carbon source in the configured slurry to ensure that the residual amount of the carbon source between drying batches is controllable; the filtrate after the filter press can be reused.

[0010] Preferably, during the primary sintering, the temperature is first raised to the sintering temperature at a rate of 2-5°C / min, and then maintained at the sintering temperature for 3-15 hours, and the sintering temperature is between 300-750°C.

[0011] Preferably, during the secondary sintering, the temperature is first raised to the sintering temperature at a rate of 2-5°C / min, and then kept at the sintering temperature for 3-15 hours, and the sintering temperature is between 500-850°C.

[0012] Preferably, the iron source is one or more of iron phosphate, oxalate, carbonate and oxide, and the lithium source is one or more of lithium carbonate, lithium phosphate and lithium dihydrogen phosphate.

[0013] Preferably, the carbon source is one or more of glucose, sucrose, starch, and polyethylene glycol.

[0014] Preferably, in order to improve the performance of the positive electrode material, an additive is usually added during the batching, and the additive is an oxalate, phosphate, oxide or carbonate of a metal element. The metal element is one or more of Mg, Ti, V, Nb, W, Mo, Ni and Co.

[0015] Preferably, the secondary sintered material is screened and iron removed to obtain a spherical lithium iron phosphate material, the particle size range D50 of the spherical structure is 5-30 μm, and the material ratio is 8.0-14.0 μm. 2 / g, and the carbon content is 0.8%~2.0%. The obtained lithium iron phosphate positive electrode material is spherical, and is a secondary particle formed by the union of primary particles. The primary particles are interconnected in a network shape at the microscopic level, and have better structural stability, double-layer carbon coating and low specific surface area.

[0016] Beneficial effects of the present invention: On the basis of existing technologies, by optimizing the synthesis process of lithium iron phosphate materials, we simultaneously completed the preparation of double-layer carbon-coated, spheroidized, and nano-sized lithium iron phosphate products with high structural stability. The spheroidization method solved the processing problem of nanomaterials that are difficult to disperse. At the same time, the spherical primary particles are about 200nm, achieving nano-size appearance. The surface coating effect is further optimized by double-layer carbon coating, and the cycle performance of the material is significantly improved.

[0017] Moreover, by regulating the amount of carbon source added, a lithium iron phosphate precursor with a stable network structure is prepared by sintering once, and then a double-layer carbon coating is achieved through secondary wet coating. In addition, sand milling and spray drying equipment are not required in the secondary wet coating, and only filter pressing and vibration drying are used to complete the preparation of double-layer carbon-coated products in a low-cost manner. No crushing is required in the later stage, and the production capacity of screening, iron removal and guarantee is significantly increased, and the processing energy consumption is less. In addition, since the secondary carbon coating does not use grinding, the number of small particles in the material system is significantly reduced, the material has a smaller specific surface area, is easier to process, and the cost can be significantly reduced.

[0018] In addition, the material has a micron-scale spherical structure and good fluidity, so it does not need to be crushed, and the screening and iron removal capacity of the material will be significantly increased. At the battery cell level, due to the improved fluidity of the material, the processability and solid content of the material pulping will be significantly improved. At the same time, the porous structure of the material at the microscopic level is more conducive to the transmission of the electrolyte, and the power performance will be significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1This is a process flow chart of the preparation of the double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material of the present invention; Figure 2 This is a SEM morphology image of the material after the first sintering in Example 1 of the present invention. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0021] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0022] Embodiment 1: Step 1, 25 kg of lithium carbonate, 100 kg of iron phosphate, 6.0 kg of glucose, 1.0 kg of titanium dioxide, and 135 kg of water are mixed evenly to obtain a primary mixture.

[0023] Step 2: The primary mixed material is introduced into a sand mill for coarse grinding (zirconium bead diameter 0.6mm), and the primary grinding particle size D50 = 1.3μm; then introduced into a sand mill for fine grinding (zirconium bead diameter 0.3mm), and the grinding particle size D50 = 0.35μm; then spray drying is performed, and the spray drying air inlet temperature is 250℃ and the air outlet temperature is 90℃; then sintering is performed under inert atmosphere protection conditions, and the temperature is raised to 650℃ at a speed of 3℃ / min, and the temperature is kept for 7 hours, and finally cooled to obtain the primary sintered material. The material after the primary sintering becomes porous, refer to the attached Figure 1 As shown, a stable network structure is formed between the primary particles.

[0024] Step 3, 100 kg of the primary sintering material, 6.0 kg of glucose, and 110 kg of water are mixed and stirred evenly to obtain a secondary mixture.

[0025] Step 4, filter the secondary mixed material through a filter press to obtain a filter cake with a moisture content of 10%; then dry the filter cake through a vibration dryer to obtain a dry material with good fluidity, raise the temperature to 700°C at a rate of 3°C / min, keep warm for 7 hours, and finally cool down to obtain a secondary sintering material.

[0026] Step 5, sieving the secondary sintered material to remove iron, and obtaining the lithium iron phosphate positive electrode material of Example 1.

[0027] Embodiment 2: Step 1, 25 kg of lithium carbonate, 100 kg of iron phosphate, 7.0 kg of glucose, 1.0 kg of titanium dioxide, and 135 kg of water are mixed evenly to obtain a primary mixture.

[0028] Step 2, introducing the primary mixture into a sand mill for coarse grinding (zirconium bead diameter 0.6mm), the primary grinding particle size D50 = 1.3μm; then introducing it into a sand mill for fine grinding (zirconium bead diameter 0.3mm), the grinding particle size D50 = 0.35μm; then spray drying, the spray drying air inlet temperature is 250℃, and the air outlet temperature is 90℃; then sintering is carried out under inert atmosphere protection conditions, rising to 650℃ at a speed of 3℃ / min, keeping warm for 7 hours, and finally cooling to obtain a primary sintered material.

[0029] Step 3, 100 kg of the primary sintering material, 5.0 kg of glucose, and 110 kg of water are mixed and stirred evenly to obtain a secondary mixture.

[0030] Step 4, filter the secondary mixed material through a filter press to obtain a filter cake with a moisture content of 10%; then dry the filter cake through a vibration dryer to obtain a dry material with good fluidity, raise the temperature to 700°C at a rate of 3°C / min, keep warm for 7 hours, and finally cool down to obtain a secondary sintering material.

[0031] Step 5, sieving the secondary sintered material to remove iron, and obtaining the lithium iron phosphate positive electrode material of Example 2.

[0032] Embodiment 3: Step 1, 25 kg of lithium carbonate, 100 kg of iron phosphate, 8.0 kg of glucose, 1.0 kg of titanium dioxide, and 135 kg of water are mixed evenly to obtain a primary mixture.

[0033] Step 2, introducing the primary mixture into a sand mill for coarse grinding (zirconium bead diameter 0.6mm), the primary grinding particle size D50 = 1.3μm; then introducing it into a sand mill for fine grinding (zirconium bead diameter 0.3mm), the grinding particle size D50 = 0.35μm; then spray drying, the spray drying air inlet temperature is 250℃, and the air outlet temperature is 90℃; then sintering is carried out under inert atmosphere protection conditions, rising to 650℃ at a speed of 3℃ / min, keeping warm for 7 hours, and finally cooling to obtain a primary sintered material.

[0034] Step 3, 100 kg of the primary sintering material, 4.0 kg of glucose, and 110 kg of water are mixed and stirred evenly to obtain a secondary mixture.

[0035] Step 4, filter the secondary mixed material through a filter press to obtain a filter cake with a moisture content of 10%; then dry the filter cake through a vibration dryer to obtain a dry material with good fluidity, raise the temperature to 700°C at a rate of 3°C / min, keep warm for 7 hours, and finally cool down to obtain a secondary sintering material.

[0036] Step 5, sieving the secondary sintered material to remove iron, and obtaining the lithium iron phosphate positive electrode material of Example 3.

[0037] Comparative Example 1: Step 11, 25 kg of lithium carbonate, 100 kg of iron phosphate, 7.0 kg of glucose, 1.0 kg of titanium dioxide, and 135 kg of water are mixed evenly to obtain a primary mixture.

[0038] Step 22, introduce the primary mixture into a sand mill for coarse grinding (zirconium bead diameter 0.6mm), the primary grinding particle size D50 = 1.3μm; then introduce it into a sand mill for fine grinding (zirconium bead diameter 0.3mm), the grinding particle size D50 = 0.35μm; then spray drying, the spray drying air inlet temperature is 250℃, and the air outlet temperature is 90℃; then sintering is carried out under inert atmosphere protection conditions, rising to 650℃ at a speed of 3℃ / min, keeping warm for 7 hours, and finally cooling to obtain a primary sintered material.

[0039] Step 4, the material is subjected to air flow pulverization and sieving to remove iron, so as to obtain the lithium iron phosphate positive electrode material of Comparative Example 1.

[0040] The performance of the lithium iron phosphate positive electrode materials prepared in the above embodiment and the comparative example was tested and compared, and the results are shown in Table 1 below:

[0041] The lithium iron phosphate positive electrode material prepared in the embodiment of the present invention has electrical properties comparable to those of mainstream products in the industry, and has low specific surface area, low powder resistance and excellent processing performance. At the same time, due to the innovative application of processing equipment, the processing cost of the material is significantly reduced.

[0042] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material, characterized in that: Includes steps: 1) Primary sintering: The iron source, lithium source, additives and the first part of the carbon source are mixed with a solvent to form a primary mixed slurry, and the slurry is ground and dried before primary sintering to obtain a porous and structurally stable grid structure primary sintered material. The D50 of the ground slurry is 0.15-0.6 μm. 2) Secondary sintering: the primary sintered material is mixed with the second part of the carbon source and the solvent to obtain a secondary mixed slurry, the secondary mixed slurry is filtered and then dried, and then secondary sintered after drying to obtain a secondary sintered material.

2. The method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material according to claim 1, characterized in that: During the primary sintering, the temperature is first raised to the sintering temperature at a rate of 2-5°C / min, and then kept at the sintering temperature for 3-15 hours. The sintering temperature is between 300-750°C.

3. The method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material according to claim 1, characterized in that: During the secondary sintering, the temperature is first raised to the sintering temperature at a rate of 2-5°C / min, and then kept at the sintering temperature for 3-15 hours. The sintering temperature is between 500-850°C.

4. The method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material according to claim 1, characterized in that: The iron source is one or more of iron phosphate, oxalate, carbonate and oxide, and the lithium source is one or more of lithium carbonate, lithium phosphate and lithium dihydrogen phosphate.

5. The method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material according to claim 1, characterized in that: The carbon source is, for example, one or more of glucose, sucrose, starch, and polyethylene glycol.

6. The method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material according to claim 1, characterized in that: The additive is oxalate, phosphate, oxide or carbonate of the metal element.

7. The method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material according to claim 6, characterized in that: The metal element is one or more of Mg, Ti, V, Nb, W, Mo, Ni, and Co.

8. The method for preparing a double-layer carbon-coated spherical nano-lithium iron phosphate positive electrode material according to claim 1, characterized in that: The secondary sintered material is screened and iron removed to obtain a spherical lithium iron phosphate material. The particle size range of the spherical structure D50: 5~30μm, and the material ratio is 8.0~14.0m 2 / g, carbon content is 0.8%~2.0%.

Citation Information

Patent Citations

  • Preparation method of spherical lithium iron phosphate

    CN102013484A

  • Carbon-coated lithium iron phosphate and preparation method therefor, and lithium ion battery

    CN107240696A

  • Carbon-coated lithium iron phosphate process, and prepared carbon-coated lithium iron phosphate and application thereof

    CN110380025A

  • Preparation method of low-cost high-capacity spherical lithium iron phosphate

    CN116639673A

  • Method for preparing carbon-coated lithium iron phosphate material from ferrous phosphate

    US20230080632A1

Cited By

  • Double-layer carbon-coated lithium iron phosphate positive electrode material, preparation method thereof and battery

    CN120637372A

  • Multi-layer coated lithium manganese iron phosphate material as well as preparation method and application thereof

    CN121269664A

  • A multilayer coated lithium manganese iron phosphate material, its preparation method and application