Biomass-based activated carbon as well as physical and chemical synergistic activation preparation method and application

By employing a physicochemical synergistic activation method, combined with high-temperature activation using phosphoric acid and water vapor, the problems of low mesoporous content and poor adsorption performance of activated carbon were solved, resulting in the preparation of high-performance biomass-based activated carbon for application in the adsorption field.

CN118954507APending Publication Date: 2024-11-15NORTHWEST UNIV

Patent Information

Application Number
CN202410984269.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing technologies for preparing activated carbon suffer from problems such as low mesoporous content and poor adsorption performance.

Method used

A physicochemical synergistic activation method was adopted. After impregnating the precursor raw materials in a phosphoric acid aqueous solution, primary and secondary activation were carried out in a tube furnace. High-temperature activation was performed using the combination of N2 and water vapor. Subsequently, residues were removed by washing with HCl, thus preparing biomass-based activated carbon with large specific surface area, high mesoporous content, and good adsorption performance.

Benefits of technology

Activated carbon materials with a specific surface area as high as 2310 m2/g, a methylene blue adsorption value as high as 795 mg/g, a methyl orange adsorption value as high as 498 mg/g, and an iodine adsorption value as high as 1553 mg/g were prepared, significantly improving the adsorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954507A_ABST
    Figure CN118954507A_ABST
Patent Text Reader

Abstract

The invention discloses biomass-based activated carbon as well as a physical and chemical synergistic activation preparation method and application thereof, and belongs to the technical field of activated carbon. The chemical activation method adopts phosphoric acid activation, the physical activation method adopts an activation method of simultaneously introducing N2 and water vapor, the activated carbon material with large specific surface area, high mesoporous rate and good adsorption performance is prepared after high-temperature activation, and the phosphoric acid can permeate into the raw materials in the activation treatment process, so that in the follow-up water vapor activation process, the adsorption performance of the activated carbon material is greatly improved. Under the combined action of phosphoric acid and water vapor, more pore channels can be generated, so that pores of the material are richer. The prepared activated carbon has a good adsorption effect on methylene blue, methyl orange and iodine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of activated carbon preparation, and specifically relates to a biomass-based activated carbon and a physical and chemical synergistic activation preparation method and application. Background Art

[0002] Activated carbon is a material rich in carbon and can be prepared from coal, various organic wastes such as agricultural waste, forestry waste and urban sludge. It has the advantages of wide sources, low price, high carbon content, high cation exchange capacity, rich surface functional groups, large specific surface area and stable structure. It is widely used in adsorption, separation, catalysis and other fields.

[0003] At present, the most commonly used activation methods for carbon materials are physical activation and chemical activation. Physical activation refers to the process of introducing CO into the reactor at a certain temperature (800-1000℃) to activate biochar. 2 , water vapor or a small amount of air and other gases to activate and form activated carbon with a porous structure. The mechanism of physical activation is to achieve the purpose of pore formation by reacting oxidizing gas with carbon material and consuming carbon atoms; chemical activation refers to the process of mixing biomass raw materials or biochar precursors with chemical activators and then activating them at a certain temperature (400-850°C). For example, a Chinese patent (CN101332992A) discloses a method for preparing biomass-based activated carbon using zinc chloride activation. The raw materials are impregnated and activated with zinc chloride to prepare tung shell-based activated carbon with a specific surface area of ​​1602m 2 / g, methylene blue adsorption value 300mg / g activated carbon. Chinese patent (CN111232977A) discloses a method for preparing biomass-based activated carbon by phosphoric acid activation, wherein the raw material is impregnated and activated with phosphoric acid at a ratio of 1:2 to prepare straw-based activated carbon with a specific surface area of ​​1068m 2 / g of activated carbon. However, whether it is physical activation or chemical activation, there are low mesoporosity and poor adsorption performance in the process of preparing activated carbon. It is necessary to explore the use of raw materials in new preparation methods and under different conditions to prepare activated carbon materials, so as to effectively improve the adsorption effect of activated carbon.

[0004] In addition, fruit trees are planted in many places, and a huge number of branches are pruned every year at a low price. In addition, the content of lignin and cellulose in the branches of fruit trees is higher than that of other trees, resulting in a high fixed carbon content and a good pore structure. It is a very excellent and cheap raw material for making activated carbon. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and to provide a biomass-based activated carbon and a physical and chemical synergistic activation preparation method and application to solve the problems of low mesoporosity and poor adsorption performance in the process of preparing activated carbon in the prior art.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing biomass-based activated carbon by physical and chemical synergistic activation, comprising the following steps:

[0008] Step 1, immersing the precursor raw material in a phosphoric acid aqueous solution, adding a catalyst for reaction, and drying the immersed precursor raw material powder to obtain a process powder;

[0009] Step 2: Place the process powder in a tube furnace for heat preservation and perform primary activation. During the primary activation process, N 2 ; Then simultaneously pass N 2 and water vapor, heat preservation for secondary activation, and obtain the activated material after cooling; the primary activation temperature is 400-500°C, and the primary activation heat preservation time is 0.5-1h;

[0010] Step 3, washing, filtering and drying the activated material to obtain activated carbon material.

[0011] A further improvement of the present invention is:

[0012] Preferably, in step 1, the precursor material is crushed wood, and the catalyst is a sulfuric acid solution.

[0013] Preferably, in step 1, the mixing mass ratio of the precursor raw material and the phosphoric acid aqueous solution is 1:1 to 1:3; and the added amount of the catalyst is 2 to 6 wt % of the total mass of the precursor raw material powder and the phosphoric acid aqueous solution.

[0014] Preferably, in step 1, the immersion time is 12 to 36 hours, the immersion temperature is room temperature, and the drying temperature is 100°C.

[0015] Preferably, in step 2, during the primary activation process, N 2 The flow rate was 30 mL / min.

[0016] Preferably, in step 2, the secondary activation temperature is 750-950° C., and the holding time is 0.5-1 h.

[0017] Preferably, in step 3, the activated material is placed in 1 mol / L HCl, washed in a water bath at 50° C., washed with distilled water until neutral, and filtered.

[0018] Preferably, in step 3, the washing temperature is 50°C and the drying temperature is 80°C.

[0019] A biomass-based activated carbon prepared by any one of the above preparation methods.

[0020] Preferably, the biomass-based activated carbon is used to adsorb methylene blue, methyl orange and iodine.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention provides a method for preparing biomass activated carbon by a physical and chemical synergistic activation method, comprising the following steps: (1) crushing a precursor raw material and placing it in a phosphoric acid aqueous solution and a catalyst for immersion, and then drying the impregnated precursor raw material powder; (2) placing the precursor raw material powder dried in step (1) in a tube furnace at N 2 The temperature was raised to the primary activation temperature under the atmosphere, kept warm, and then N 2 and water vapor, continue to heat to the secondary activation temperature, keep the temperature, cool down, and take out the activated material; (3) wash the material activated by step (2), filter it by suction; dry the filtered material to obtain a biomass-based activated carbon material. In the present invention, the chemical activation method uses phosphoric acid activation, and the physical activation method uses N 2 The activation method of introducing water vapor simultaneously, after high temperature activation, an activated carbon material with large specific surface area, high mesoporosity and good adsorption performance is prepared. The adsorption value of methylene blue is as high as 795 mg / g, the adsorption value of methyl orange is as high as 498 mg / g, the adsorption value of iodine can be as high as 1553 mg / g, and the BET specific surface area can reach 2310m 2 / g. The methylene blue, methyl orange adsorption value, iodine adsorption value and specific surface area of ​​activated carbon materials prepared by single physical activation method and single chemical activation method using coal as raw material are higher. This method effectively increases the specific surface area of ​​activated carbon and improves the adsorption performance of activated carbon. The preparation method has low cost and simple process. The prepared material has high mesoporosity and good adsorption performance, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A flow chart for preparation.

[0024] Figure 2 This is the SEM image of the activated carbon in Example 8.

[0025] Figure 3 N is the N of the activated carbon sample prepared in Example 8 2 Adsorption-desorption curves and pore size distribution curves.

[0026] Among them, (a) is N 2 (a) is the adsorption-desorption curve; (b) is the pore size distribution curve.

[0027] Figure 4 This is a comparison chart of the adsorption values ​​of Example 8 at different initial concentrations of methylene blue.

[0028] Figure 5 The figure is a comparison chart of the adsorption values ​​of 800 mg / L methylene blue of Example 8, Comparative Example 1 and Comparative Example 2 at different dosages.

[0029] Figure 6 It is a comparison chart of the adsorption values ​​of 800 mg / L methylene blue at different times when the dosage is 1 g / L for Example 8, Comparative Example 1 and Comparative Example 2.

[0030] Figure 7 This is a comparison chart of the adsorption values ​​of Example 8 at different initial methyl orange concentrations.

[0031] Figure 8 This is a comparison chart of the adsorption values ​​of 500 mg / L methyl orange at different dosages for Example 8, Comparative Example 1 and Comparative Example 2.

[0032] Fig. 9 This is a comparison chart of the methyl orange adsorption values ​​of Example 8, Comparative Example 1 and Comparative Example 2 at different times for 500 mg / L methyl orange when the dosage is 1 g / L. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:

[0034] See also Figure 1 The present invention discloses a method for preparing biomass-based activated carbon by physical and chemical synergistic activation. The specific preparation method comprises the following steps:

[0035] Step 1: immerse the precursor raw material powder in a phosphoric acid aqueous solution, add a small amount of catalyst, and then dry the immersed precursor raw material powder.

[0036] In step 1), the mass ratio of the precursor raw material powder to the phosphoric acid aqueous solution is 1:1 to 1:3, and the amount of the added catalyst is 2 to 6 wt % of the total mass of the precursor raw material powder and the phosphoric acid aqueous solution.

[0037] As a preferred solution, the mass ratio of the chemical activator to the precursor raw material powder is 1:2, and a catalyst with a mass fraction of 4% is added.

[0038] In step 1), the precursor raw material is obtained by crushing trees, specifically, breaking branches into branches of about 3 cm, drying at 80° C., and crushing through an 80-mesh sieve.

[0039] In step 1), the phosphoric acid aqueous solution is a phosphoric acid solution with a mass fraction of 30% to 50%, the catalyst is a 40% sulfuric acid solution, and the phosphoric acid aqueous solution is used as a chemical activator solution.

[0040] As a preferred solution, the chemical activator is a 40% phosphoric acid aqueous solution.

[0041] In step 1), the immersion time is 12 to 36 hours, and the immersion is carried out at room temperature.

[0042] As a preferred solution, the immersion time is 24 hours.

[0043] In step 1), the drying temperature is 100°C.

[0044] 2) placing the precursor raw material powder dried in step 1) in a tube furnace at N 2 The temperature was raised to the primary activation temperature under the atmosphere and kept at the set time. After the holding time was completed, N 2 and water vapor, continue to heat up to the secondary activation temperature, keep warm for the set time two, then cool down, and take out the activated material when the temperature drops below 50℃.

[0045] In step 2), N 2 The flow rate was 30 mL / min.

[0046] In step 2), the second heating is conducted while N 2 and water vapor, from N 2 First, pass it into a three-necked flask filled with boiling water, then N 2 The water vapor is carried into the tube furnace at the same time.

[0047] In step 2), the first activation temperature is 400-500°C, and the set time 1 is 0.5-1h; the second activation temperature is 750-950°C, and the set time 2 is 0.5-1h;

[0048] As a preferred solution, the first activation temperature is 450°C; the second activation temperature is 850°C.

[0049] In step 2), the heating rate of the tube furnace is 5°C / min.

[0050] 3) Washing, filtering and drying the material activated in step 2) to obtain an activated carbon material.

[0051] In step 3), the washing is performed with 1 mol / L HCl in a 50°C water bath, and then washed with distilled water until neutral, and filtered. In step 3), the washing temperature is 50°C; the drying temperature is 80°C.

[0052] During the above-mentioned treatment process of step 1 and step 2, the ionization of phosphoric acid causes the polymer in the precursor material to swell, peptize and dissolve, so that water vapor can penetrate well into the raw material in the subsequent primary activation process, so that it is heated evenly, and activated carbon can be obtained at a lower primary activation temperature (450-600°C) and a shorter activation time (0.5-1.5h). In addition, during the heating process, the thermal evaporation of phosphoric acid will form a cavity structure inside the adsorption material, thereby increasing the distance between carbon microcrystals, making the material more porous, and increasing some acidic active functional groups, so that the adsorption sites of activated carbon are increased.

[0053] The main mechanism of water vapor activation is that water vapor enters the carbon pores and reacts with carbon to produce gas. Some carbon atoms evaporate after the reaction, resulting in pores. The volatilized gas etches the pore wall again, thereby producing more pores. The biomass activated carbon obtained by water vapor activation is mainly micropores. With the increase of activation time, water vapor tends to widen the micropores during the activation process, thereby producing a pore structure change from micropores to mesopores and even to macropores.

[0054] The activated carbon obtained by water vapor activation has less ash content, general pore development, mainly micropores, and low yield. The activated carbon obtained by phosphoric acid activation has developed pores, mostly mesopores, and a high yield, but the required post-processing stage is more cumbersome, and there is more ash and residual phosphoric acid. The activated carbon obtained by phosphoric acid-water vapor combined activation combines the advantages of both and successfully avoids most of their disadvantages. The activated carbon activated by phosphoric acid has a more mesoporous structure and some residual phosphoric acid. After water vapor activation, its microporous structure is supplemented, making the pore structure richer. At the same time, water vapor has a certain washing effect on the residual phosphoric acid, which can remove most of the residual phosphoric acid. The amount of HCl used in the final washing product can be reduced.

[0055] Furthermore, the prepared activated carbon is washed with HCl to remove the remaining phosphates and some residual ash, which block part of the pores of the carbon. Removing these components can obtain a more developed pore structure and greatly increase the active sites on the adsorbent surface.

[0056] Example 1

[0057] Weigh 10 g of the dried precursor powder and mix it with 10 mL of 30% phosphoric acid aqueous solution, add 2 wt% sulfuric acid, soak for 12 h, and then dry at 100 °C for later use. 2 Under the condition (N 2 The temperature was raised to 400°C at a rate of 5°C / min and kept at this temperature for 1 h, and then N 2 and water vapor (in N2 As carrier gas, it carries water vapor into the tube furnace, N 2 The flow rate was 30 mL / min), and the temperature was continued to rise to 750°C at a rate of 5°C / min for 1 h. After the activation, the temperature was lowered, and N was continuously introduced during the process. 2 . When the furnace temperature drops to 50°C, take out the activated sample. Wash the activated sample with 1mol / L HCl in a 50°C water bath for 30 minutes, then wash with deionized water until neutral, and then filter. Dry the filtered material in an oven (80°C). After the dried sample is cooled to room temperature, weigh it, put it in a ziplock bag, and test its performance.

[0058] Example 2

[0059] Weigh 10 g of the dried precursor powder and mix it with 20 mL of 40% phosphoric acid aqueous solution, add 2 wt% sulfuric acid, soak for 12 h, and then dry at 100 °C for later use. 2 Under the condition (N 2 The temperature was raised to 400°C at a rate of 5°C / min and kept at this temperature for 1 h. Then, N 2 and water vapor conditions (N 2 The flow rate was 30 mL / min, N 2 First pass into a three-necked flask, then N 2 Carry water vapor into the tube furnace to simultaneously introduce N 2 and water vapor), and then continue to heat to 750℃ at a rate of 5℃ / min, and maintain the activation time for 1h. After the activation is completed, the temperature is lowered, and N is continuously introduced during the entire cooling process. 2 . When the furnace temperature drops to about 50℃, take out the activated sample. Stir the activated sample with 1mol / L HCl in a 50℃ water bath for 30min, then wash it with deionized water until it is neutral, and then filter it. Dry the filtered material in an oven at 80℃. After the dried sample cools to room temperature, weigh it, put it in a ziplock bag, and test its performance.

[0060] Example 3

[0061] Weigh 10 g of the dried precursor powder and mix it with 20 mL of 40% phosphoric acid aqueous solution, add 2 wt% sulfuric acid, soak for 12 h, and then dry at 100 °C for later use. 2 Under the condition (N 2 The temperature was raised to 400°C at a rate of 5°C / min and kept at this temperature for 1 h. Then, N 2 and water vapor conditions (N2 The flow rate was 30 mL / min, N 2 First pass into a three-necked flask, then N 2 Carry water vapor into the tube furnace to simultaneously introduce N 2 and water vapor), and then continue to heat to 800℃ at a rate of 5℃ / min, and maintain the activation time for 1h. After the activation is completed, the temperature is lowered, and N is continuously introduced during the entire cooling process. 2 . When the furnace temperature drops to about 50℃, take out the activated sample. Stir the activated sample with 1mol / L HCl in a 50℃ water bath for 30min, then wash it with deionized water until it is neutral, and then filter it. Dry the filtered material in an oven at 80℃. After the dried sample cools to room temperature, weigh it, put it in a ziplock bag, and test its performance.

[0062] Example 4

[0063] Weigh 10 g of the dried precursor raw material powder and mix it with 20 mL of 40% phosphoric acid aqueous solution, add 4 wt% sulfuric acid, soak for 24 h, and then dry at 100 °C for later use. Put the material into a tube furnace and pass N 2 Under the condition (N 2 The temperature was raised to 400°C at a rate of 5°C / min and kept at this temperature for 1 h. Then, N 2 and water vapor conditions (N 2 The flow rate was 30 mL / min, N 2 First pass into a three-necked flask, then N 2 Carry water vapor into the tube furnace to simultaneously introduce N 2 and water vapor), and then continue to heat to 800℃ at a rate of 5℃ / min, and maintain the activation time for 1h. After the activation is completed, the temperature is lowered, and N is continuously introduced during the entire cooling process. 2 . When the furnace temperature drops to about 50℃, take out the activated sample. Wash the activated material with 1mol / L HCl in a 50℃ water bath for 30min, then wash with deionized water until neutral, and then filter. Dry the filtered material in an oven at 80℃. After the dried sample cools to room temperature, weigh it, put it in a ziplock bag, and test its performance.

[0064] Example 5

[0065] Weigh 10 g of the dried precursor raw material powder and mix it with 20 mL of 40% phosphoric acid aqueous solution, add 4 wt% sulfuric acid, soak for 24 h, and then dry at 100 °C for later use. Put the material into a tube furnace and pass N 2 Under the condition (N 2The temperature was raised to 450°C at a rate of 5°C / min and kept at this temperature for 1 h. Then, N 2 and water vapor conditions (N 2 The flow rate was 30 mL / min, N 2 First pass into a three-necked flask, then N 2 Carry water vapor into the tube furnace to simultaneously introduce N 2 and water vapor), and then continue to heat to 850℃ at a rate of 5℃ / min, and maintain the activation time for 1h. After the activation is completed, the temperature is lowered, and N is continuously introduced during the entire cooling process. 2 . When the furnace temperature drops to about 50℃, take out the activated sample. Stir the activated sample with 1mol / L HCl in a 50℃ water bath for 30min, then wash it with deionized water until it is neutral, and then filter it. Dry the filtered material in an oven at 80℃. After the dried sample cools to room temperature, weigh it, put it in a ziplock bag, and test its performance.

[0066] Example 6

[0067] Weigh 10 g of the dried precursor powder and mix it with 30 mL of 50% phosphoric acid aqueous solution, add 6% sulfuric acid, soak for 36 hours, and then dry at 100 °C for later use. 2 Under the condition (N 2 The temperature was raised to 500°C at a rate of 5°C / min and kept at this temperature for 1 h. Then, N 2 and water vapor conditions (N 2 The flow rate was 30 mL / min, N 2 First pass into a three-necked flask, then N 2 Carry water vapor into the tube furnace to simultaneously introduce N 2 and water vapor), and then continue to heat to 850℃ at a rate of 5℃ / min, and maintain the activation time for 1h. After the activation is completed, the temperature is lowered, and N is continuously introduced during the entire cooling process. 2 . When the furnace temperature drops to about 50℃, take out the activated sample. Stir the activated sample with 1mol / L HCl in a 50℃ water bath for 30min, then wash it with deionized water until it is neutral, and then filter it. Dry the filtered material in an oven at 80℃. After the dried sample cools to room temperature, weigh it, put it in a ziplock bag, and test its performance.

[0068] Example 7

[0069] Weigh 10 g of the dried precursor powder and mix it with 20 mL of 40% phosphoric acid aqueous solution, add 4% sulfuric acid, soak for 24 h, and then dry at 100 °C for later use. 2 Under the condition (N 2 The temperature was raised to 550°C at a rate of 5°C / min and kept at this temperature for 1 h, and then N 2 and water vapor conditions (N 2 The flow rate was 30 mL / min, N 2 First pass into a three-necked flask, then N 2 Carry water vapor into the tube furnace to simultaneously introduce N 2 and water vapor), and then continue to heat to 900℃ at a rate of 5℃ / min, and maintain the activation time for 1h. After the activation is completed, the temperature is lowered, and N2 is continuously introduced during the entire cooling process. 2 . When the furnace temperature drops to about 50℃, take out the activated sample. Stir the activated sample with 1mol / L HCl in a 50℃ water bath for 30min, then wash it with deionized water until it is neutral, and then filter it. Dry the filtered material in an oven at 80℃. After the dried sample cools to room temperature, weigh it, put it in a ziplock bag, and test its performance.

[0070] Example 8

[0071] Weigh 10 g of the dried precursor powder and mix it with 20 mL of 40% phosphoric acid aqueous solution, add 4% sulfuric acid, soak for 24 h, and then dry at 100 °C for later use. 2 Under the condition (N 2 The temperature was raised to 450°C at a rate of 5°C / min and kept at this temperature for 1 h. Then, N 2 and water vapor conditions (N 2 The flow rate was 30 mL / min, N 2 First pass into a three-necked flask, then N 2 Carry water vapor into the tube furnace to simultaneously introduce N 2 and water vapor), and then continue to heat to 950℃ at a rate of 5℃ / min, and maintain the activation time for 1h. After the activation is completed, the temperature is lowered, and N is continuously introduced during the entire cooling process. 2. When the furnace temperature drops to about 50℃, take out the activated sample. Stir the activated sample with 1mol / L HCl in a 50℃ water bath for 30min, then wash it with deionized water until it is neutral, and then filter it. Dry the filtered material in an oven at 80℃. After the dried sample cools to room temperature, weigh it, put it in a ziplock bag, and test its performance.

[0072] Figure 2 The SEM image of the activated carbon prepared in this example shows that the prepared activated carbon has a relatively developed pore structure and the pores are evenly distributed. This is because the swelling effect of phosphoric acid and the rapid diffusion rate of water vapor allow it to penetrate deeply into the material, activate it evenly, and inhibit tar formation, so that the activated carbon maintains a good pore structure.

[0073] Figure 3 N is the N of the activated carbon sample prepared in this example 2 Adsorption-desorption curve and pore size distribution curve. Its nitrogen adsorption-desorption curve is type IV, and has an obvious H4 type hysteresis loop, which is a significant feature of mesoporous carbon materials. From the pore size distribution curve, it can be seen that its pore size distribution is concentrated, mainly composed of mesopores of 0.5nm to 2.5nm, which is consistent with the results of the adsorption-desorption isotherm analysis.

[0074] Figure 4 The adsorption comparison diagram of different initial concentrations of methylene blue in this example is shown in the figure. It can be seen from the figure that the adsorption of methylene blue by activated carbon increases with the increase of the concentration of methylene blue, and the maximum can reach 850 mg / L.

[0075] Figure 5 The following is a comparison diagram of the adsorption of 800 mg / L methylene blue by this embodiment and two comparative examples at different dosages. It can be seen from the figure that the adsorption effect of methylene blue is best when the dosage is 1.0 g / L.

[0076] Figure 6 The adsorption comparison diagram of 800 mg / L methylene blue at different time for this embodiment and two comparative examples when the dosage is 1.0 g / L. It can be seen from the figure that the adsorption effect of this embodiment on 800 mg / L methylene blue is much greater than that of the two comparative examples, indicating that the physical and chemical synergistic activation increases the adsorption effect on methylene blue.

[0077] Figure 7 The adsorption comparison diagram of this embodiment at different initial concentrations of methyl orange is shown in the figure. It can be seen from the figure that the adsorption of methylene blue by activated carbon increases with the increase of methyl orange concentration, and the maximum value can reach 485 mg / L.

[0078] Figure 8The following is a comparison chart of the adsorption of 500 mg / L methyl orange by this embodiment and two comparative examples at different dosages. It can be seen from the figure that the adsorption effect of methyl orange is best when the dosage is 1.0 g / L.

[0079] Fig. 9 The figure is a comparison of the adsorption of 500 mg / L methyl orange at different times by the embodiment and two comparative examples when the dosage is 1.0 g / L. It can be seen from the figure that the adsorption effect of the embodiment on 500 mg / L methyl orange is much greater than that of the two comparative examples, indicating that the physical and chemical synergistic activation increases the adsorption effect on methylene blue.

[0080] Comparative Example 1

[0081] Biomass activated carbon was prepared by physical activation method: 10 g of precursor raw material powder was weighed and placed in a tube furnace, and N 2 (N 2 The temperature was raised to 750°C at a rate of 5°C / min, and N 2 and water vapor (N 2 The flow rate was 30 mL / min, N 2 First pass into a three-necked flask, then N 2 Carry water vapor into the tube furnace to simultaneously introduce N 2 and water vapor), and then continue to heat up to 950℃ and maintain the activation time for 1h. After the activation, stop heating and start cooling. After it drops to 750℃, only N 2 . When the furnace temperature drops to 50℃, take out the sample. Stir the activated material with 1mol / L hydrochloric acid in a 50℃ water bath for 30min, then wash with distilled water until neutral, and filter. Dry the filtered material in an oven at 80℃. After the dried sample cools to room temperature, weigh it, then put it into a ziplock bag and test the performance of the sample.

[0082] Comparative Example 2

[0083] The biomass activated carbon was prepared by chemical activation method: 10 g of precursor raw material powder was weighed and impregnated with 20 mL of 40% phosphoric acid aqueous solution for 24 h, and then dried at 100 °C. The dried material was placed in a tube furnace at N 2 (N 2In an atmosphere with a flow rate of 30mL / min), heat up to the activation temperature of 450℃ at a rate of 5℃ / min, and maintain the activation time for 1h. When the activation is completed, stop heating and start cooling. When the furnace temperature drops to 50℃, take out the sample. Stir the activated material with 1mol / L hydrochloric acid in a 50℃ water bath for 30min, then wash with distilled water until neutral, and filter. Dry the filtered sample in an oven at 80℃. After the dried sample is cooled to room temperature, weigh its mass, then put it into a ziplock bag, and test the performance of the sample.

[0084] Performance Testing

[0085] In order to study the adsorption performance of biomass-based activated carbon prepared by physical and chemical synergistic activation method, the adsorption values ​​of iodine, methylene blue and methyl orange were determined. The steps of methylene blue adsorption are as follows:

[0086] 1. Weigh 0.05g, 0.10g, 0.15g, and 0.20g of biomass-based activated carbon prepared by physical and chemical synergistic activation method, and add them into 100mL of 800mg / L methylene blue solution respectively.

[0087] 2. Use a constant temperature oscillator to oscillate at a certain speed for a certain period of time at room temperature and then filter.

[0088] 3. Measure the absorbance of the filtrate at the maximum absorption wavelength and calculate the methylene blue adsorption value of the biomass-based activated carbon.

[0089] 4. Carry out the same experiment on biomass-based activated carbon prepared by single physical and chemical activation methods, repeat steps 1 to 3, and compare the differences in experimental data on the adsorption of methylene blue by biomass-based activated carbon prepared by physical activation, chemical activation, and physicochemical synergistic activation.

[0090] 5. Add 0.10 g of biomass-based activated carbon prepared by the physical and chemical synergistic activation method into 100 mL of 600 mg / L, 700 mg / L, 800 mg / L, and 900 mg / L methylene blue solutions, respectively.

[0091] 6. Use a constant temperature oscillator to oscillate at a certain speed for a certain period of time at room temperature and then filter.

[0092] 7. Measure the absorbance of the filtrate at the maximum absorption wavelength, and calculate the methylene blue adsorption value of biomass-based activated carbon prepared by the physical and chemical synergistic activation method under different methylene blue concentrations as time changes.

[0093] In order to study the adsorption performance of biomass-based activated carbon prepared by physical and chemical synergistic activation method, the iodine adsorption value, methylene blue and methyl orange adsorption value were determined. The methyl orange adsorption steps are as follows:

[0094] 8. Use 500 mg / L methyl orange solution to perform the above operations 1 to 3. Compare the differences in experimental data of biomass-based activated carbon adsorbing methyl orange prepared by physical activation, chemical activation and physical and chemical synergistic activation.

[0095] Results and Analysis

[0096] Methylene blue adsorption

[0097]

[0098] Methyl orange adsorption

[0099]

[0100] It can be seen from the above table that under different activated carbon addition conditions, the adsorption values ​​of biomass-based activated carbon prepared by the physical and chemical synergistic activation method for methylene blue and methyl orange are higher than those of activated carbon activated by single physical or chemical activation.

[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing biomass-based activated carbon by physical and chemical synergistic activation, characterized in that: The following steps are involved: Step 1, immersing the precursor raw material in a phosphoric acid aqueous solution, adding a catalyst for reaction, and drying the immersed precursor raw material powder to obtain a process powder; Step 2, placing the process powder in a tube furnace for primary activation, introducing N2 during the primary activation; then introducing N2 and water vapor at the same time, and maintaining the temperature for secondary activation, and obtaining the activated material after cooling; the primary activation temperature is 400-500°C, and the primary activation insulation time is 0.5-1h; Step 3, washing, filtering and drying the activated material to obtain activated carbon material.

2. The method for preparing biomass-based activated carbon by physical and chemical synergistic activation according to claim 1, characterized in that: In step 1, the precursor material is crushed wood, and the catalyst is sulfuric acid solution.

3. The method for preparing biomass-based activated carbon by physical and chemical synergistic activation according to claim 1, characterized in that: In step 1, the mixing mass ratio of the precursor raw material and the phosphoric acid aqueous solution is 1:1 to 1:3; the added amount of the catalyst is 2 to 6 wt % of the total mass of the precursor raw material powder and the phosphoric acid aqueous solution.

4. The method for preparing biomass-based activated carbon by physical and chemical synergistic activation according to claim 1, characterized in that: In step 1, the immersion time is 12 to 36 hours, the immersion temperature is room temperature, and the drying temperature is 100°C.

5. The method for preparing biomass-based activated carbon by physical and chemical synergistic activation according to claim 1, characterized in that: In step 2, during the primary activation process, the N2 introduction rate was 30 mL / min.

6. The method for preparing biomass-based activated carbon by physical and chemical synergistic activation according to claim 1, characterized in that: In step 2, the secondary activation temperature is 750-950° C., and the holding time is 0.5-1 h.

7. The method for preparing biomass-based activated carbon by physical and chemical synergistic activation according to claim 1, characterized in that: In step 3, the activated material is placed in 1 mol / L HCl, washed in a water bath at 50° C., washed with distilled water until neutral, and filtered.

8. The method for preparing biomass-based activated carbon by physical and chemical synergistic activation according to claim 7, characterized in that: In step 3, the washing temperature is 50°C and the drying temperature is 80°C.

9. A biomass-based activated carbon prepared by the preparation method according to any one of claims 1 to 8.

10. An application of the biomass-based activated carbon according to claim 9, characterized in that: The biomass-based activated carbon is used for adsorbing methylene blue, methyl orange and iodine.

Citation Information

Patent Citations

  • Method for preparing active carbon by taking biomass pyrolytic carbon as raw material

    CN104003387A

  • Method for preparing high specific surface area activated carbon through rapid activation under fluidization

    US20180362350A1

Cited By

  • High-purity composite carbon adsorption material as well as preparation method and application thereof

    CN120001336A

  • Biomass-based activated carbon and preparation method thereof

    CN120364695A

  • Process for removing pollutants in industrial aquaculture tail water of penaeus vannamei boone

    CN121225835A