Anhydrous gypsum board and preparation method thereof

By using anhydrous gypsum, exciter and pulp, the hydration rate and solidification time are adjusted, and the toughness and water resistance of gypsum board are solved, achieving high-strength, fire resistance and cost-effective preparation of anhydrous gypsum board.

CN118955079APending Publication Date: 2024-11-15ZHENGZHOU SUNDY BUILDING TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411099093.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing gypsum board has poor toughness and poor water resistance, which leads to easy breakage and moisture-absorbing, and the cost increases to improve waterproofing effect is not ideal.

Method used

Anhydrous gypsum is used as the main raw material, and the excitant, retarder and pulp are added. Anhydrous gypsum board is prepared through pulping, blanking, pressing and drying processes, adjusting the hydration rate and solidification time, and improving the toughness and water resistance of the board. .

Benefits of technology

The high strength, good moisture resistance, excellent fire resistance and dimensional stability of waterless gypsum board are achieved, reducing costs, and improving the nail grip and toughness of the board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004988872110000061
    Figure BDA0004988872110000061
  • Figure BDA0004988872110000071
    Figure BDA0004988872110000071
  • Figure BDA0004988872110000072
    Figure BDA0004988872110000072
Patent Text Reader

Abstract

The invention discloses an anhydrous gypsum board and a preparation method thereof, and relates to the technical field of building materials, and the anhydrous gypsum board is prepared by adding water into the following raw materials in parts by weight: 300-700 parts of anhydrous gypsum, 300-700 parts of an exciting agent, 80-120 parts of paper pulp and 0.5-3 parts of a retarder. The preparation method comprises the following steps: putting the anhydrite, the exciting agent, the paper pulp, the retarder and the water into a stirrer, and uniformly stirring to prepare slurry; redundant water in the prepared slurry is pumped out; uniformly spreading the slurry, uniformly coating the slurry on a rotating cylindrical roller, and cutting off by using a knife after the roller rotates for multiple circles, so as to obtain a plate blank; the plate blanks are stacked, and the plate blanks are separated through steel plates; feeding the stacked plate blanks into a press machine, pressing the plate blanks and extruding excessive water; and drying, air-drying or air-drying the prepared plate blank to obtain a finished product. The anhydrous gypsum board is good in moisture resistance and water resistance, high in strength, good in toughness, excellent in fire resistance, good in size stability and low in deformation coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to an anhydrous gypsum board and a preparation method thereof. Background Art

[0002] Gypsum board is a kind of building board made of semi-hydrated gypsum as the main raw material. It is a building material with light weight, high strength, thin thickness, easy processing, good sound insulation, heat insulation and fire resistance. It is one of the new lightweight boards that are currently being developed. Gypsum board has been widely used in various buildings such as residential buildings, office buildings, shops, hotels and industrial plants, such as interior partitions, wall covering panels (instead of wall plastering), ceilings, sound-absorbing panels, ground base panels and various decorative panels. It is not suitable for indoor installation in bathrooms or kitchens. Semi-hydrated gypsum, also known as β-gypsum or building gypsum, is a product obtained by heating and dehydrating dihydrate gypsum. Its main component is hemihydrate of calcium sulfate (CaSO4·1 / 2H2O). Since semi-hydrated gypsum contains less water, its setting speed is relatively fast. When semi-hydrated gypsum is mixed with water, a hydration reaction will occur rapidly to generate dihydrate gypsum and release a lot of heat. This reaction process leads to the rapid setting and hardening of the gypsum slurry, so that it can obtain higher strength in a short time. Therefore, the gypsum board made of hydrated gypsum as the main raw material has the following disadvantages:

[0003] 1. Poor toughness and easy to break;

[0004] 2. Poor water resistance, easy to powder when exposed to moisture, and low softening coefficient.

[0005] To improve water resistance, silicone waterproofing agents must be applied to the surface of the board, which can only improve the waterproof effect of the board surface and increase costs.

[0006] Anhydrous gypsum, also known as hard gypsum, is a product obtained by high-temperature calcination of dihydrate gypsum, and its main component is anhydrous calcium sulfate (CaSO4). It is divided into two variants, α-type and β-type, which are respectively formed by heating and dehydrating α-type and β-type hemihydrate gypsum. Type II anhydrous gypsum is also called hard gypsum, or insoluble anhydrite (Insolustrongle-anhydrite), the final product of insoluble anhydrous gypsum. It is the final product of dihydrate gypsum, hemihydrate gypsum and type I anhydrous gypsum that is stable at room temperature after high-temperature dehydration. Natural anhydrite that exists stably in nature also belongs to this category. Foreign countries use a large number of type II anhydrous gypsum and β-hemihydrate gypsum to form a composite phase gypsum binder to improve the performance of hemihydrate gypsum. However, anhydrous gypsum and type II anhydrous gypsum coagulate and harden slowly and cannot be used directly. They must be activated or modified. Foreign countries often use the technical route of modifying active activated materials or combining modification and activation. There is no corresponding report in the prior art on the preparation of gypsum board using anhydrous gypsum as the main raw material. Summary of the invention

[0007] In view of this, the present invention provides an anhydrous gypsum board and a preparation method thereof. The present invention uses anhydrous gypsum as a main raw material, adds an activator, a retarder, and paper pulp to make a building decoration board to solve the problems of poor toughness, easy breakage and poor water resistance of existing gypsum boards.

[0008] In order to solve the above technical problems, the technical solution of the present invention is:

[0009] An anhydrous gypsum board is made by adding water to the following raw materials in parts by weight: 300-700 parts of anhydrous gypsum or type II anhydrous gypsum, 300-700 parts of an activator, 80-120 parts of pulp and 0.5-3 parts of a retarder. The activator is composed of calcium hydroxide and hemihydrate gypsum in a weight ratio of 1: (6-15). The purpose of adding the pulp is to accelerate the hydration rate of the anhydrous gypsum, thereby increasing the initial strength of the anhydrous gypsum. The purpose of adding the pulp is to improve the toughness and nail holding force of the board and reduce the weight of the board, and the adsorption of the pulp is required when the slab is formed.

[0010] Wherein, the retarder is citric acid, sodium citrate or sodium hexametaphosphate. The function of adding the retarder is to adjust the initial setting time of the slurry during the production process.

[0011] The present invention also provides a method for preparing anhydrous gypsum board, comprising the following steps:

[0012] Step 1, putting anhydrous gypsum, activator, pulp, retarder and water into a mixer and uniformly stirring them to form a slurry;

[0013] Step 2, extracting excess water from the slurry prepared in step 1 to reduce the water content of the slurry to 20-40%.

[0014] Step 3, evenly spread the slurry prepared in step 2, and evenly apply it on a rotating cylindrical drum. After the drum rotates for several circles, it is cut with a knife to obtain a slab;

[0015] Step 4, stacking the slabs produced in step 3, separating the slabs with steel plates; sending the stacked slabs into a press to press the slabs and squeeze out excess water;

[0016] Step 5, drying, air-drying or air-drying the stacked slabs obtained in step 4.

[0017] Wherein, in step 1, the amount of water added is 70-90% of the total amount of anhydrous gypsum, activator, pulp and retarder.

[0018] In step 3, the roller rotates one circle to apply a layer, and the thickness of the layer is 0.3-1.5mm; during coating, the roller rotates 8-20 circles. The pulp is evenly coated on the rotating cylindrical roller by using the adsorption type of the pulp. The circumference of the roller is ≥ the length of the plate. Generally, a slab with a thickness of >6mm is made. When the predetermined thickness is reached, it is cut with a knife to form a slab.

[0019] Among them, in step 4, each stack of slabs consists of 10-100 sheets, and the pressure applied during pressing is 8-12MPa. Different pressures can be applied according to different density models of plates.

[0020] Among them, in step 4, the drying temperature is less than 50° C.; the choice of drying, air-drying or air-drying can be selected according to the ambient temperature and humidity.

[0021] The present invention adopts anhydrous gypsum as the main raw material, which has good water resistance, high softening coefficient and slow hydration and solidification speed and is more suitable for the production process of the board.

[0022] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0023] The anhydrous gypsum board of the present invention is a building decoration board prepared by taking anhydrous gypsum as the main raw material, adding an activator, a retarder and paper pulp through pulping, blank making, pressing, drying and other main production links. The board has good moisture resistance and water resistance, high strength, good toughness, excellent fire resistance, good dimensional stability and low deformation coefficient. DETAILED DESCRIPTION

[0024] The following embodiments are provided for a better understanding of the present invention, but are not limited to the best mode of implementation, and do not limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0025] Example 1

[0026] This embodiment provides an anhydrous gypsum board, which is made by adding water to the following raw materials in parts by weight: 400 parts of type II anhydrous gypsum, 500 parts of an activator, 100 parts of pulp and 1 part of citric acid. The activator is composed of calcium hydroxide and hemihydrate gypsum in a weight ratio of 1:9.

[0027] This embodiment also provides a method for preparing the above-mentioned anhydrous gypsum board, comprising the following steps:

[0028] Step 1, putting type II anhydrous gypsum, activator, pulp, retarder and water into a mixer and uniformly stirring to form a slurry; the amount of water added is 80% of the total amount of anhydrous gypsum, activator, pulp and retarder;

[0029] Step 2, extracting excess water from the slurry prepared in step 1 to reduce the water content of the slurry to 30%;

[0030] Step 3, after evenly spreading the slurry prepared in step 2, evenly coating it on a rotating cylindrical roller, the roller rotates one circle to coat a layer, and the thickness of the layer is 0.1 mm; after the roller rotates 15 circles, cut it with a knife to obtain a slab;

[0031] Step 4, stacking the slabs prepared in step 3, each stack of slabs consisting of 50 slabs, and separating the slabs with steel plates; sending the stacked slabs into a press, applying a pressure of 10 MPa to press the slabs, and squeezing out excess water;

[0032] Step 5, drying the stacked slabs pressed in step 4 (drying temperature is 50° C.), to obtain.

[0033] Example 2

[0034] This embodiment provides an anhydrous gypsum board, which is made by adding water to the following raw materials in parts by weight: 300 parts of anhydrous gypsum, 300 parts of activator, 120 parts of pulp and 0.8 parts of sodium citrate. The activator is composed of calcium hydroxide and hemihydrate gypsum in a weight ratio of 1:6.

[0035] This embodiment also provides a method for preparing the above-mentioned anhydrous gypsum board, comprising the following steps:

[0036] Step 1, anhydrous gypsum, activator, pulp, retarder and water are put into a mixer and uniformly stirred to form a slurry; the amount of water added is 70% of the total amount of anhydrous gypsum, activator, pulp and retarder;

[0037] Step 2, extracting excess water from the slurry prepared in step 1 to reduce the water content of the slurry to 20%;

[0038] Step 3, after evenly spreading the slurry prepared in step 2, evenly coating it on a rotating cylindrical roller, the roller rotates one circle to coat a layer, and the thickness of the layer is 0.3 mm; after the roller rotates 20 circles, cut it with a knife to obtain a slab;

[0039] Step 4, stacking the slabs prepared in step 3, each stack of slabs consisting of 100 slabs, and separating the slabs with steel plates; sending the stacked slabs into a press, applying a pressure of 8 MPa to press the slabs, and squeezing out excess moisture;

[0040] Step 5, drying the stacked slabs pressed in step 4.

[0041] Example 3

[0042] This embodiment provides an anhydrous gypsum board, which is made by adding water to the following raw materials in parts by weight: 700 parts of anhydrous gypsum, 700 parts of activator, 80 parts of pulp and 1.2 parts of sodium hexametaphosphate. The activator is composed of calcium hydroxide and hemihydrate gypsum in a weight ratio of 1:15.

[0043] This embodiment also provides a method for preparing the above-mentioned anhydrous gypsum board, comprising the following steps:

[0044] Step 1, anhydrous gypsum, activator, pulp, retarder and water are put into a mixer and uniformly stirred to form a slurry; the amount of water added is 90% of the total amount of anhydrous gypsum, activator, pulp and retarder;

[0045] Step 2, extracting excess water from the slurry prepared in step 1 to reduce the water content of the slurry to 40%;

[0046] Step 3, after evenly spreading the slurry prepared in step 2, evenly coating it on a rotating cylindrical roller, the roller rotates one circle to coat a layer, and the thickness of the layer is 1.5 mm; after the roller rotates 8 circles, it is cut with a knife to obtain a slab;

[0047] Step 4, stacking the slabs prepared in step 3, wherein each stack of slabs consists of 10 slabs, and the slabs are separated by steel plates; sending the stacked slabs into a press, applying a pressure of 12 MPa to press the slabs, and squeezing out excess water;

[0048] Step 5, air-drying the stacked slabs pressed in step 4.

[0049] Example 4

[0050] This embodiment provides an anhydrous gypsum board, which is made by adding water to the following raw materials in parts by weight: 380 parts of type II anhydrous gypsum, 480 parts of an activator, 90 parts of pulp and 0.9 parts of sodium citrate. The activator is composed of calcium hydroxide and hemihydrate gypsum in a weight ratio of 1:9.

[0051] This embodiment also provides a method for preparing the above-mentioned anhydrous gypsum board, comprising the following steps:

[0052] Step 1, putting type II anhydrous gypsum, activator, pulp, retarder and water into a mixer and uniformly stirring to form a slurry; the amount of water added is 85% of the total amount of anhydrous gypsum, activator, pulp and retarder;

[0053] Step 2, extracting excess water from the slurry prepared in step 1 to reduce the water content of the slurry to 35%;

[0054] Step 3, after evenly spreading the slurry prepared in step 2, evenly coating it on a rotating cylindrical roller, the roller rotates one circle to coat a layer, and the thickness of the layer is 0.8 mm; after the roller rotates 12 circles, it is cut with a knife to obtain a slab;

[0055] Step 4, stacking the slabs prepared in step 3, each stack of slabs consisting of 40 slabs, and separating the slabs with steel plates; sending the stacked slabs into a press, applying a pressure of 11 MPa to press the slabs, and squeezing out excess water;

[0056] Step 5, drying the stacked slabs pressed in step 4.

[0057] Example 5

[0058] This embodiment provides an anhydrous gypsum board, which is made by adding water to the following raw materials in parts by weight: 420 parts of anhydrous gypsum, 520 parts of activator, 110 parts of pulp and 1.1 parts of citric acid. The activator is composed of calcium hydroxide and hemihydrate gypsum in a weight ratio of 1:9.

[0059] This embodiment also provides a method for preparing the above-mentioned anhydrous gypsum board, comprising the following steps:

[0060] Step 1, anhydrous gypsum, citric acid, pulp, retarder and water are put into a mixer and uniformly stirred to form a slurry; the amount of water added is 75% of the total amount of anhydrous gypsum, activator, pulp and retarder;

[0061] Step 2, extracting excess water from the slurry prepared in step 1 to reduce the water content of the slurry to 25%;

[0062] Step 3, after evenly spreading the slurry prepared in step 2, evenly coating it on a rotating cylindrical roller, the roller rotates one circle to coat a layer, and the thickness of the layer is 0.5 mm; after the roller rotates 15 circles, cut it with a knife to obtain a slab;

[0063] Step 4, stacking the slabs prepared in step 3, each stack of slabs consisting of 75 sheets, and separating the slabs with steel plates; sending the stacked slabs into a press, applying a pressure of 9 MPa to press the slabs, and squeezing out excess water;

[0064] Step 5, drying the stacked slabs pressed in step 4 (drying temperature is 40° C.), to obtain.

[0065] Experimental example:

[0066] The anhydrous gypsum boards prepared in Examples 1-5 were tested according to the requirements of JC / T 799-2016 "Decorative Gypsum Board" and JC / T2702-2022 "Fiber-reinforced Gypsum Board". The test results are shown in Table 1:

[0067] Table 1-1 Performance test results of anhydrous gypsum board

[0068]

[0069]

[0070] Table 1-2 Performance test results of anhydrous gypsum board

[0071]

[0072]

[0073] After testing, the screw holding force test results of Examples 1-5 were the actual measured values, and other items met the index requirements for ordinary boards (P) in JG / T799-2016 "Decorative Gypsum Board".

[0074] Among them, the screw holding force, appearance quality, flatness, right-angle deviation, moisture content, unit area mass and breaking load are tested according to JC / T 799-2016, and the combustion performance is tested according to JC / T2702-2022.

[0075] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention. The protection scope of the present invention is defined by the claims and their equivalent technical solutions.

Claims

1. A waterless gypsum board, It is characterized by The invention is prepared by adding water to the following raw materials in parts by weight: 300-700 parts of anhydrous gypsum or type II anhydrous gypsum, 300-700 parts of an activator, 80-120 parts of pulp and 0.5-3 parts of a retarder.

2. The anhydrous gypsum board according to claim 1, Features: The activator is composed of calcium hydroxide and hemihydrate gypsum in a weight ratio of 1:(6-15).

3. The anhydrous gypsum board according to claim 1, Features: The retarder is citric acid, sodium citrate or sodium hexametaphosphate.

4. A method for preparing the anhydrous gypsum board according to any one of claims 1 to 3, Features The steps include: Step 1, putting anhydrous gypsum or type II anhydrous gypsum, an activator, paper pulp, a retarder and water into a mixer and uniformly stirring them to form a slurry; Step 2, extracting excess water from the slurry prepared in step 1 to reduce the water content of the slurry to 20-40%; Step 3, evenly spread the slurry prepared in step 2, and evenly apply it on a rotating cylindrical drum. After the drum rotates for several circles, it is cut with a knife to obtain a slab; Step 4, stacking the slabs produced in step 3, separating the slabs with steel plates; sending the stacked slabs into a press to press the slabs and squeeze out excess water; Step 5, drying, air-drying or air-drying the stacked slabs obtained in step 4.

5. A method for preparing anhydrous gypsum board according to claim 4, Features: In step 1, the amount of water added is 70-90% of the total amount of anhydrous gypsum, activator, pulp and retarder.

6. The method for preparing anhydrous gypsum board according to claim 4, Features: In step 3, the roller rotates one circle to apply a layer, and the thickness of the layer is 0.3-1.5 mm; during coating, the roller rotates 8-20 circles.

7. The method for preparing anhydrous gypsum board according to claim 4, Features: In step 4, each stack of slabs consists of 10-100 sheets, and the pressure applied during pressing is 5-15 MPa.

8. The method for preparing anhydrous gypsum board according to claim 4, Features: In step 4, the drying temperature is less than 50°C.