Preparation method of surface isolation slurry for silicon nitride ceramic substrate

By preparing boron nitride isolation slurry on the surface of silicon nitride ceramic substrate, using a combination of a planetary mill and a specific solvent and dispersant, the problem of poor dispersion and stability of boron nitride powder slurry is solved, and the ceramic substrate is realized Uniform sintering and high thermal conductivity reduce the problems of chromatic aberration and bending instability.

CN118955179AInactive Publication Date: 2024-11-15江苏海古德半导体科技有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411086050.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing boron nitride powder slurry has poor dispersion and stability, which leads to uneven density of the isolation powder layer, affects the sintering process of ceramic substrates, and is prone to problems of color difference and bending unstable resistance.

Method used

A planetary mill mixes 94-106 parts of oily solvent and 2-5 parts of glue powder, adds 63-72 parts of isolation powder and 1-4 parts of dispersant, and after ball milling and defoaming, the viscosity reaches 65,000-67,000mpa*s. The slurry is uniformly scraped with a thickness of 8 to 10 um on the surface of the ceramic substrate, and terpineol is used as the solvent, acrylic resin is used as the glue powder, sorbitan trioleate is used as the dispersant, and boron nitride is used as the isolation powder.

Benefits of technology

The dispersion efficiency and stability of the slurry are improved, and a slurry with narrow particle size distribution and uniformity is formed, which enhances heat conduction and chemical stability, reduces the settlement speed, and ensures the uniformity and bending resistance of the ceramic substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955179A_ABST
    Figure CN118955179A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of surface isolation slurry for a silicon nitride ceramic substrate, which comprises the following steps: a, adding 94-106 parts of oily solvent and 2-5 parts of rubber powder into a ball mill, mixing, and ball-milling for 0.5 hour at the rotating speed of 300r / min; b, 63-72 parts of isolation powder and 1-4 parts of a dispersing agent are added into the slurry obtained in the step a, and ball milling continues to be conducted for 0.5 h at the rotating speed of 300 r / min; c, defoaming the prepared slurry by using a vacuum defoaming machine, so that the viscosity of the slurry reaches 65000-67000 mpa * s; and d, coating the de-foamed slurry on the surface of a ceramic substrate at the temperature of 15-20 DEG C in a scraping manner to form a thin film with the thickness of 8-10 microns. According to the preparation method of the isolation slurry for the surface of the silicon nitride ceramic substrate, the adopted oily slurry system has good dispersity and stability, and it is ensured that the thickness of the isolation slurry on the surface of the ceramic substrate is uniform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic substrate isolation layers, in particular to a method for preparing isolation slurry for the surface of a silicon nitride ceramic substrate. Background Art

[0002] Ceramic green body debinding is an important step in the manufacturing process of ceramic substrates. It mainly involves removing organic components in ceramic green bodies, such as adhesives and plasticizers, to ensure that the ceramic can achieve ideal densification and performance during the subsequent sintering process. When debinding ceramic green bodies, multiple layers of ceramic green bodies need to be stacked and pressurized and sent into a debinding furnace for heating and debinding. In order to prevent adhesion between ceramic green bodies, an isolation slurry is usually applied to the surface of each ceramic green body.

[0003] In the prior art, the boron nitride powder particles in the boron nitride powder slurry have poor dispersibility, which easily leads to agglomeration of powder particles and uneven density of the formed isolation powder layer. The thickness of the boron nitride powder slurry layer is uneven, which affects the heat conduction between layers during the sintering process of the substrate, and the substrate is prone to color difference and bending instability. In addition, the boron nitride aqueous slurry system has poor stability and easy sedimentation, and requires the addition of stabilizers or regular stirring to maintain uniformity. Summary of the invention

[0004] The technical problem to be solved by the present invention is: in order to overcome the shortcomings of the prior art that the boron nitride powder slurry has poor dispersibility and stability, which easily leads to uneven thickness of the slurry layer, the present invention provides a method for preparing a surface isolation slurry for a silicon nitride ceramic substrate.

[0005] The technical solution to be adopted by the present invention to solve the technical problem is: a method for preparing a surface isolation slurry for a silicon nitride ceramic substrate, comprising the following steps:

[0006] a. Add 94-106 parts of oily solvent and 2-5 parts of rubber powder into a planetary ball mill and mix them at a speed of 300 r / min for 0.5 h;

[0007] b. Add 63-72 parts of isolated powder and 1-4 parts of dispersant to the slurry of step a, and continue ball milling at a speed of 300 r / min for 0.5 h;

[0008] c. Defoam the prepared slurry with a vacuum defoamer to make the slurry viscosity reach

[0009] 65000~67000mpa*s;

[0010] d. Scrape and evenly coat the defoamed slurry on the surface of the ceramic substrate at a temperature of 15-20°C to form a film with a thickness of 8-10um.

[0011] Furthermore, the solvent is terpineol.

[0012] Furthermore, the isolation powder is boron nitride powder.

[0013] Furthermore, the rubber powder is acrylic resin.

[0014] Furthermore, the dispersant is sorbitan trioleate.

[0015] The present invention provides a method for preparing a surface isolation slurry for a silicon nitride ceramic substrate, which has the following beneficial effects:

[0016] 1. The planetary ball milling process is used. The grinding drum rotates while revolving. This allows the revolution speed to exceed the critical speed limit of ordinary ball mills, driving the grinding balls to make complex movements, more effectively impacting and grinding the materials, and improving the dispersion efficiency of the slurry. The slurry particle size after grinding is 1.3-1.5μm, the particle size distribution is narrow, and the slurry uniformity is high.

[0017] 2. Use pinene alcohol as a solvent carrier. It contains unsaturated double bonds. As a solvent carrier, it can enhance the stability and suspension of the colloid and better disperse the boron nitride particles. Acrylic resin provides a suspension stabilizer for the isolation powder. The lightly cross-linked acrylic resin can form a three-dimensional network structure, which increases its stability in the medium and helps maintain the stability of the suspension system. Acrylic resin has excellent rheological modification ability and can be used as a thickener. Its pseudoplastic (shear thinning) characteristics make the viscosity higher in a static state, which helps to suspend particles, and the viscosity decreases in a flowing state, which is easy to process and apply. It also has good thermal stability and can withstand certain temperature changes during processing and application without losing its suspension stability. Trioleyl sorbitan is used as a dispersant, and its molecules contain a hydrophilic sorbitan head and a hydrophobic oleic acid chain. When added to a liquid, it can reduce the surface tension of the liquid and make the dispersion process easier, thereby helping to isolate the dispersion of powder particles in the liquid. Its molecules are adsorbed on the surface of the particles with their hydrophilic heads facing the water phase, increasing the electrostatic repulsion between particles and preventing particle aggregation, thereby improving dispersion stability. The adsorption layer formed on the surface of the particles can serve as a protective film to prevent contact and aggregation between particles, while increasing the viscosity of the dispersion medium, thereby slowing down the sedimentation rate of the particles and maintaining the stability of the dispersion system.

[0018] 3. Boron nitride is used as the isolation powder. Boron nitride has high thermal conductivity and can effectively transfer heat from the silicon nitride substrate, thereby forming a good heat conduction channel between the substrate and the isolation powder. Boron nitride has good chemical stability at high temperatures and will not react chemically with silicon nitride, which helps to keep the interface between the substrate and the isolation powder clear and stable. Moreover, the thermal expansion coefficient of boron nitride is similar to that of silicon nitride. Boron nitride is used as the isolation powder, which helps to reduce the stress and cracks caused by thermal expansion mismatch during the thermal cycle of the silicon nitride ceramic substrate. Boron nitride has a layered structure, which helps to form a uniform isolation layer, and its performance can be optimized by regulating the interlayer spacing. The boron nitride layer on the surface of the sintered ceramic substrate can be easily removed by polishing and ultrasonic cleaning, which is convenient for post-processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0020] Figure 1 It is a process flow chart of the best embodiment of the present invention;

[0021] Figure 2 It is a schematic diagram of the isolation film application structure.

[0022] In the figure: 1. Ceramic substrate, 2. Thin film. DETAILED DESCRIPTION

[0023] The present invention will now be described in detail with reference to the accompanying drawings. This figure is a simplified schematic diagram, which only illustrates the basic structure of the present invention in a schematic manner, and therefore only shows the components related to the present invention.

[0024] like Figure 1-2 As shown, a method for preparing a surface isolation slurry for a silicon nitride ceramic substrate of the present invention comprises the following steps:

[0025] a. Add 1000g of pine alcohol and 20g of acrylic resin into a ball mill and mix them, and then ball mill them at a speed of 300r / min for 0.5h;

[0026] b. Add 700 g of boron nitride powder and 20 g of sorbitan trioleate to the slurry of step a, and continue ball milling at a speed of 300 r / min for 0.5 h;

[0027] c. Defoam the prepared slurry with a vacuum defoamer to make the slurry viscosity reach 65994mpa*s;

[0028] d. Scrape the defoamed slurry onto the surface of the ceramic substrate 1 at a temperature of 16° C. to form a thin film 2 with a thickness of 8 to 10 μm.

[0029] Working process:

[0030] The defoamed slurry is coated on the surface of the ceramic substrate 1 at a temperature of 16°C by a tape casting machine. After the isolation slurry is coated on the surface of multiple ceramic substrates 1, they are stacked and pressurized and sent into the debinding furnace. The isolation slurry can prevent the ceramic substrates 1 from sticking to each other during the sintering process. The organic matter in the isolation slurry is completely decomposed and volatilized during the debinding process of the ceramic substrate 1, and a uniform 8-10um thick isolation powder layer can be formed on the surface of the ceramic substrate 1. Since boron nitride as an isolation powder has the characteristics of not reacting with silicon nitride and is resistant to high temperature and high pressure, the structure remains unchanged after sintering. When the ceramic substrate 1 after debinding is taken out, the boron nitride powder on the surface of the silicon nitride ceramic substrate 1 can be easily removed by washing with water.

[0031] Directions and references (e.g., up, down, left, right, etc.) in the present invention may only be used to assist in the description of features in the accompanying drawings. Therefore, the following detailed description is not to be taken in a limiting sense, and the scope of the subject matter claimed is limited only by the attached claims and their equivalents.

[0032] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the scope of the present invention through the above description. The technical scope of this invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a surface isolation slurry for a silicon nitride ceramic substrate, characterized in that: The following steps are involved: a. Add 94-106 parts of oily solvent and 2-5 parts of rubber powder into a planetary ball mill and mix them at a speed of 300 r / min for 0.5 h; b. Add 63-72 parts of isolated powder and 1-4 parts of dispersant to the slurry of step a, and continue ball milling at a speed of 300 r / min for 0.5 h; c. Defoam the prepared slurry with a vacuum defoamer to make the slurry viscosity reach 65000~67000mpa*s; d. Evenly scrape the defoamed slurry on the surface of the ceramic substrate (1) at a temperature of 15 to 20° C. to form a thin film (2) with a thickness of 8 to 10 μm.

2. The method for preparing a surface isolation slurry for a silicon nitride ceramic substrate according to claim 1, characterized in that: The solvent is terpineol.

3. The method for preparing a surface isolation slurry for a silicon nitride ceramic substrate according to claim 1, characterized in that: The isolation powder is boron nitride powder.

4. The method for preparing a surface isolation slurry for a silicon nitride ceramic substrate according to claim 1, characterized in that: The rubber powder is acrylic resin.

5. The method for preparing a surface isolation slurry for a silicon nitride ceramic substrate according to claim 1, characterized in that: The dispersant is sorbitan trioleate.

Citation Information

Patent Citations

  • Method for preparing ceramic substrate isolating layer by using boron nitride ultrathin cast film tape

    CN115196972A

  • Preparation method of boron nitride printing paste

    CN116063084A

  • Laminated sintering process method of high-performance silicon nitride ceramic substrate

    CN116161970A

  • Oxide-containing ceramic sintered body production method and release sheet

    WO2021106533A1