Polyvinylidene fluoride copolymer as well as preparation method and application thereof
By developing a binder containing vinylidene fluoride and fluorine atomic copolymer, the problem of poor adhesion caused by expansion of silicon negative electrode of lithium-ion batteries is solved, and the electrochemical performance and stability of the battery are significantly improved.
Patent Information
- Application Number
- CN202411322371.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-15
AI Technical Summary
There is a serious volume expansion problem in the charging and discharging process of lithium-ion batteries, which leads to poor adhesion between the negative electrode materials and between the negative electrode and the current collector, affecting the electrochemical performance of the battery. The existing technology This issue was not effectively resolved.
A C2-C6 olefin copolymer containing vinylidene fluoride, fluorine atoms and non-fluorine halogen atoms were developed to prepare a copolymer with thermal stability, oxidation resistance and chemical inertness through copolymerization for use as lithium-ion batteries. The adhesive enhances bond strength and stability.
It effectively alleviates the interface instability caused by negative electrode expansion, significantly improves the electrode sheet performance, and improves the electrochemical performance of lithium-ion batteries and the overall stability of the battery.
Smart Images

Figure CN118955777A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymers and batteries, and in particular to a polyvinylidene fluoride copolymer, a method for synthesizing the copolymer, and application of the copolymer in adhesives and electrodes of lithium ion batteries. Background Art
[0002] In recent years, lithium-ion batteries have been widely used in portable consumer electronics, electric vehicles, and energy storage. Due to the limitation of the theoretical specific capacity of positive and negative electrode materials, the energy density of battery systems based on embedded electrodes (such as LiCoO2|graphite) has approached its theoretical upper limit, which has severely restricted its widespread application in pure electric vehicles and aerospace fields. In order to further improve the specific capacity of batteries and meet the increasing requirements of related fields, people are actively researching and developing electrodes using alternative materials. For example, the silicon negative electrode has a theoretical specific capacity ten times that of graphite (3579mAh·g -1 ) is considered one of the best candidates for the development of the next generation of high energy density lithium-ion batteries. However, with the development of these new electrode materials, people have discovered new problems that need to be solved urgently.
[0003] For example, the silicon negative electrode has a serious volume expansion problem during the charge and discharge process. In the state of complete lithium deintercalation, the volume change of the silicon negative electrode can reach 300%. In this case, the conventional electrode binder in the prior art has poor adhesion between the negative electrode materials (silicon materials) and / or between the negative electrode silicon materials and the current collector. With the charge / discharge cycle of the battery, the bonding inside the electrode and at the electrode interface will be quickly destroyed, seriously affecting the electrochemical performance of the battery.
[0004] In order to solve the above problems, major lithium-ion battery manufacturers and scientific research institutions in the field have invested a lot of scientific research costs, time and energy in recent years to develop and improve binders in order to overcome the above problems, but have not been able to achieve satisfactory results so far.
[0005] In view of the above problems, the inventors of the present application have developed a novel vinylidene fluoride copolymer that can be used as a binder for silicon negative electrodes of lithium-ion batteries through extensive and in-depth research, which unexpectedly solves the above problems. Summary of the invention
[0006] The first aspect of the present invention provides a copolymer, the copolymer comprising:
[0007] (1) a first copolymerized unit derived from vinylidene fluoride;
[0008] (2) a second comonomer derived from a second comonomer which is a C2-C6 olefin containing at least one fluorine atom and at least one non-fluorine halogen atom;
[0009] (3) a third copolymerized unit derived from a third copolymerized monomer represented by the following formula I:
[0010] R1-O-R2 formula I
[0011] Wherein R1 is selected from: C2-C8 alkyl, C2-C8 haloalkyl, C3-C8 cycloalkyl, C3-C8 halocycloalkyl, C6-C12 aryl;
[0012] R2 is selected from: C2-C6 alkenyl, halogenated C2-C6 alkenyl.
[0013] According to one embodiment of the first aspect of the present application, in the copolymer, the molar ratio of the first copolymerization unit to the second copolymerization unit is 99:1 to 75:25.
[0014] According to another embodiment of the first aspect of the present application, in the copolymer, the weight ratio of the sum of the weights of the first copolymerization unit and the second copolymerization unit to the third copolymerization unit is: (first copolymerization unit+second copolymerization unit):third copolymerization unit=100:0.5 to 100:20.
[0015] According to another embodiment of the first aspect of the present application, the weight average molecular weight of the copolymer is 20,000 to 2.2 million.
[0016] According to another embodiment of the first aspect of the present application, the second comonomer is chlorotrifluoroethylene, and the third comonomer is isobutyl vinyl ether.
[0017] The second aspect of the present application provides a method for preparing the copolymer of the present invention, which comprises carrying out a copolymerization reaction in a reactor containing vinylidene fluoride, a second comonomer, a third comonomer, an emulsifier, a chain transfer agent, an initiator, a pH adjuster and water to form the copolymer.
[0018] According to one embodiment of the second aspect of the present application, the chain transfer agent is selected from one or more of the following: dimethyl carbonate, diethyl carbonate, ethylene carbonate, ethyl methyl carbonate, ethyl acetate, methyl propionate, and ethyl propionate.
[0019] According to another embodiment of the second aspect of the present application, the initiator is selected from one or more of the following: alkali metal persulfates, sodium peroxyphosphates, potassium peroxyphosphates, ammonium persulfate, peroxysuccinic acid, dibenzoyl peroxide, tert-butyl perbenzoate, and dibenzoyl peroxide.
[0020] According to another embodiment of the second aspect of the present application, the pH regulator is selected from one or more of the following: NaHSO3, Na2CO3, NaHCO3, Na2S2O3, Na2HPO3, KHCO3, K2HPO3, K2CO3, NH4HCO3, CH3COONH 4、 Triethylolamine.
[0021] According to another embodiment of the second aspect of the present application, the emulsifier is selected from one or more of the following: fluorine-containing carboxylates and fluorine-containing sulfonates.
[0022] According to another embodiment of the second aspect of the present application, the ratio of the total weight of vinylidene fluoride and the second comonomer added to the reactor to the weight of water is 1:100 to 20:100. According to another embodiment of the second aspect of the present application, the weight ratio of the emulsifier to water is 0.02:100 to 1.75:100. According to another embodiment of the second aspect of the present application, the weight ratio of the chain transfer to water is 0.002:100 to 6:100. According to another embodiment of the second aspect of the present application, the weight ratio of the initiator to water is 0.06:100 to 6:100. According to another embodiment of the second aspect of the present application, the pH adjuster is used to maintain the pH value at 8-10 during the copolymerization reaction.
[0023] According to another embodiment of the second aspect of the present application, the copolymerization reaction is carried out at a reaction temperature of 60-90°C and under anaerobic conditions, wherein at least a portion of the first comonomer, the second comonomer and the third comonomer are intermittently or continuously input into the reactor during the copolymerization reaction.
[0024] The third aspect of the present application provides a binder comprising the copolymer of the present invention.
[0025] A fourth aspect of the present application provides a lithium ion battery comprising the binder of the present invention applied on or within an electrode.
[0026] In the following detailed description, the copolymer of the present application and its preparation and use are described in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The charge-discharge curves of the first two cycles of the silicon negative electrode manufactured using the copolymer prepared according to one embodiment of the present invention as a binder;
[0028] Figure 2 The charge-discharge curves of the first two cycles of the silicon negative electrode made of PVDF binder prepared in the comparative example. DETAILED DESCRIPTION
[0029] "Range" disclosed herein is in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundary of a particular range. All ranges that can be defined in this way are inclusive of end values and combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.
[0030] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in this document, and "0-5" is just an abbreviation of these numerical combinations.
[0031] In the present invention, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.
[0032] In the present invention, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0033] In the present invention, if there is no special explanation, the "including" mentioned herein means open or closed. For example, the "including" may mean that other components not listed may also be included, or only the listed components may be included.
[0034] In the present invention, when describing the spatial relationship of a specific component or object relative to other components or objects, the terms "inside", "outside", "above", "below", etc. are used to indicate that the former is located inside, outside, above or below the latter, and the two may be in direct contact, or be separated by a certain distance or separated by a third component or object.
[0035] The copolymer of the present invention comprises a first copolymerization unit, a second copolymerization unit and a third copolymerization unit, and the above copolymerization units are derived from the corresponding first comonomer, the second comonomer and the third comonomer. In the present invention, "derived from" means that the comonomers undergo polymerization reaction (specifically, the carbon-carbon double bonds in the monomers undergo addition polymerization reaction) to form corresponding copolymerization units covalently linked together.
[0036] According to one embodiment of the present application, the first comonomer is vinylidene fluoride, which forms a first copolymerization unit shown in the following formula after copolymerization and is incorporated into the copolymer of the present invention, more specifically, connected to the main chain or side chain of the copolymer of the present invention, where "*" indicates the position connected to the adjacent copolymerization unit through a covalent bond:
[0037]
[0038] According to another embodiment of the present application, the second comonomer is a C2-C6 olefin containing at least one fluorine atom and at least one non-fluorine halogen atom, preferably a C2-C4 olefin containing at least one fluorine atom and at least one non-fluorine halogen atom, and more preferably a C2-C3 olefin containing at least one fluorine atom and at least one non-fluorine halogen atom. According to a specific embodiment of the present application, the second comonomer contains one, two or three carbon-carbon double bonds, preferably one or two carbon-carbon double bonds. According to a specific embodiment of the present application, the second comonomer contains one or more fluorine atoms, for example, 1-11 fluorine atoms, preferably 3-7 fluorine atoms. According to another specific embodiment of the present application, the non-fluorine halogen atoms in the second comonomer include one or more of the following: chlorine, bromine, iodine, preferably chlorine. According to another specific embodiment of the present application, the non-fluorine halogen atoms are 1-6, preferably 1-4, and more preferably 1-2.
[0039] According to a preferred embodiment of the present application, the second comonomer is selected from one or more of the following: chlorotrifluoroethylene, chlorodifluoroethylene, chlorotrifluoropropylene, chlorotetrafluoropropylene, chloropentafluoropropylene, chlorotetrafluorobutylene, chloropentafluorobutylene, chlorohexafluorobutylene, chlorohexafluorobutylene, chloroheptafluorobutylene, chlorotetrafluorobutylene; more preferably, the second comonomer is chlorotrifluoroethylene.
[0040] According to one embodiment of the present application, the molar ratio of the first comonomer to the second comonomer is 99:1 to 75:25, or 90:10 to 80:20, or 95:5 to 85:15, or 82:18 to 78:22.
[0041] According to one embodiment of the present application, the third comonomer has a structure shown in Formula I:
[0042] R1-O-R2 formula I
[0043] According to another embodiment of the present application, R1 in Formula I is selected from: C2-C8 alkyl, C2-C8 haloalkyl, C3-C8 cycloalkyl, C3-C8 halocycloalkyl, C6-C12 aryl; preferably, R1 is selected from: C3-C6 alkyl, C3-C6 haloalkyl, C4-C6 cycloalkyl, C4-C6 halocycloalkyl, C6-C10 aryl; more preferably, R1 is selected from: C3-C4 alkyl, C3-C4 haloalkyl, C5-C6 cycloalkyl, C5-C6 halocycloalkyl, C6-C8 aryl. According to another embodiment of the present application, R2 in Formula I is selected from: C2-C6 alkenyl, halogenated C2-C6 alkenyl; preferably, R2 is selected from: C2-C4 alkenyl, halogenated C2-C4 alkenyl; more preferably, R2 is selected from: C2-C3 alkenyl, halogenated C2-C3 alkenyl. In the above-mentioned haloalkyl, halocycloalkyl and haloalkenyl groups, "halogenated" means that the group is substituted by 1-8, preferably 1-6, more preferably 1-4 halogen atoms, and the halogen atoms include at least one of the following: fluorine, chlorine, bromine, iodine.
[0044] According to a preferred embodiment of the present application, in Formula I, R1 is isopropyl, isobutyl, n-butyl, sec-butyl, isopentyl, neopentyl; R2 is vinyl, allyl.
[0045] According to one embodiment of the present application, the weight ratio of the three comonomers satisfies the following relationship: the ratio of the sum of the weights of the first comonomer and the second comonomer to the weight of the third comonomer (first comonomer + second comonomer): (third comonomer) = 100:0.5 to 100:20, or 100:2.5 to 100:19, or 100:5 to 100:18, or 100:3 to 100:6, or 100:8 to 100:12, or 100:13 to 100:15, or 100:16 to 100:19.
[0046] According to one embodiment of the present application, the ratio of the three comonomers provided to the copolymerization reaction is specially adjusted and controlled to be within the above-mentioned range, so that the various copolymer units in the copolymer obtained by the copolymerization reaction also meet the above-mentioned ratio.
[0047] According to one embodiment of the present application, the weight average molecular weight (Mw) of the copolymer is 20,000 to 2.2 million, preferably 100,000 to 2 million, more preferably 500,000 to 1.5 million, and further preferably 1 million to 1.1 million.
[0048] The copolymer of the present invention can be prepared by a method comprising the following steps: copolymerizing in a reactor containing vinylidene fluoride, a second comonomer, a third comonomer, an emulsifier, a chain transfer agent, an initiator, a pH adjuster and water to form the copolymer.
[0049] In the method of the present invention, the types and ratios of the first comonomer (vinylidene fluoride), the second comonomer and the third comonomer are as described above.
[0050] According to one embodiment of the present application, the ratio of the total weight of the first comonomer (vinylidene fluoride) and the second comonomer added to the reactor to the weight of water is 1:100 to 20:100; preferably 3:100 to 15:100; more preferably 5:100 to 10:100; further preferably 6:100 to 8:100.
[0051] According to one embodiment of the present application, the emulsifier is selected from one or more of the following: fluorine-containing carboxylates, fluorine-containing sulfonates; preferably, the emulsifier is hexafluoroepoxy tetracarboxylic acid ammonium. According to one embodiment of the present application, in the reactor, the weight ratio of the emulsifier to water is 0.02:100 to 1.75:100.
[0052] According to one embodiment of the present application, the chain transfer agent is selected from one or more of the following: dimethyl carbonate, diethyl carbonate, ethylene carbonate, ethyl methyl carbonate, ethyl acetate, methyl propionate, ethyl propionate; preferably dimethyl carbonate. According to one embodiment of the present application, in the reactor, the weight ratio of the chain transfer to water is 0.002:100 to 6:100.
[0053] According to one embodiment of the present application, the initiator is selected from one or more of the following: persulfates of alkali metals (such as lithium, sodium, potassium), sodium peroxyphosphates, potassium peroxyphosphates, ammonium persulfate, peroxysuccinic acid, dibenzoyl peroxide, tert-butyl perbenzoate, dibenzoyl peroxide; preferably ammonium persulfate. According to one embodiment of the present application, in the reactor, the weight ratio of the initiator to water is 0.06:100 to 6:100.
[0054] According to one embodiment of the present application, the pH regulator is selected from one or more of the following: NaHSO3, Na2CO3, NaHCO3, Na2S2O3, Na2HPO3, KHCO3, K2HPO3, K2CO3, NH4HCO3, CH3COONH 4、 triethyl alcoholamine; preferably ammonium bicarbonate. According to one embodiment of the present application, in the reactor, the amount of the pH regulator added should be able to maintain the pH value of the polymerization reaction system (the aqueous solution or aqueous dispersion of the emulsifier, chain transfer agent, and initiator at the beginning of the polymerization reaction, and the emulsion of polyvinylidene fluoride is formed as the polymerization reaction proceeds) at 8-10 during the copolymerization reaction.
[0055] According to one embodiment of the present application, the copolymerization reaction is carried out at a reaction temperature of 60-90° C. under anaerobic conditions. In the present application, “anaerobic conditions” means that the oxygen content in the reactor is less than 100 ppm, preferably less than 50 ppm during the reaction.
[0056] According to one embodiment of the present application, in the copolymerization method of the present invention, at least a portion (e.g., 5-100%, or 10%, or 30%, or 50%, or 70%, or 80%, or 90%) of the first comonomer, the second comonomer, and the third monomer is input into the reactor in an intermittent or continuous manner during the copolymerization reaction.
[0057] According to a specific exemplary embodiment of the present application, the polymerization reaction of the present invention is carried out in the following manner:
[0058] 1) Add water, an emulsifier and a portion of the third comonomer into a reactor, and then perform a vacuum / nitrogen replacement cycle on the reactor until the reactor becomes an oxygen-free environment, for example, the oxygen content in the reactor is less than 50 ppm.
[0059] 2) The temperature of the reactor is raised to the reaction temperature, for example, 60-90° C., preferably 80-85° C., and then the mixture of the first monomer and the second monomer is introduced into the reactor until the pressure in the reactor is raised to the target pressure, for example, 2.5-5 MPa, preferably 3-4 MPa, and a chain transfer agent, an initiator and a pH adjuster are added into the reactor to start the copolymerization reaction.
[0060] 3) During the copolymerization reaction, the reaction temperature is maintained, and the mixture of the first monomer and the second monomer is continuously added to the reactor so that the pressure in the reactor is maintained at the above level. The initiator and the third comonomer are added to the reactor in a continuous or intermittent manner. And as needed, one or more of a chain transfer agent, a pH adjuster, and an emulsifier can be optionally added to the reactor.
[0061] 4) After the predetermined amount of comonomer has been added, the reaction is stopped, the temperature is reduced, the pressure is released, and the remaining gas is recovered. The material discharged from the reactor is washed until the conductivity of the washing water reaches a specific level, for example, a level below 5 μs / cm, and the copolymer of the present invention is obtained.
[0062] According to a preferred embodiment of the present application, the copolymer of the present invention is (vinylidene fluoride-chlorotrifluoroethylene-isobutyl vinyl ether) copolymer, also written as P(VDF-CTFE-IBVE) or VDF-CTFE-IBVE.
[0063] According to one embodiment of the present application, the copolymer of the present invention can be used to prepare a binder, in particular a binder specifically used for electrodes (in particular silicon negative electrodes) of lithium ion batteries.
[0064] For example, the copolymer of the present application can be used as a binder, a silicon-based electrode material (such as silicon-based powder) can be mixed with the binder, and then sintered at high temperature to obtain a silicon-based negative electrode. The obtained silicon-based negative electrode can be assembled into a lithium-ion battery to achieve excellent silicon-based electrode stability performance.
[0065] The advantages of the present invention are:
[0066] (i) The copolymer of the present invention has thermal stability, oxidation resistance and chemical inertness through the combination of three specially selected comonomers, which greatly enhances the bonding strength and stability of the adhesive. Meanwhile, the good film-forming property and flexibility further balance the mechanical stiffness.
[0067] (ii) The copolymer of the present invention as a binder for lithium-ion batteries can effectively alleviate the interface instability caused by the expansion of the negative electrode (especially the silicon-based negative electrode), greatly improve the performance of the electrode sheet, and thus improve the electrochemical performance of the lithium-ion battery.
[0068] The method of the present application is specifically described in the following examples, the purpose of which is to provide a better understanding of the content of the present application. It should be understood that these examples are merely illustrative and not restrictive.
[0069] Example
[0070] The water used in the following examples is deionized water, and the other reagents used are purchased from suppliers and used directly without further purification and treatment.
[0071] Example 1
[0072] In this example, P(VDF-CTFE-IBVE) was synthesized and its properties were characterized.
[0073] The copolymerization reaction is carried out in a 20-liter high-pressure polymerization reactor. First, 10kg of deionized water, 9.5g of ammonium hexafluoroepoxy tetracarboxylate and 28g of monomer IBVE are added to the reactor, the reactor is closed, stirring is started, the reactor is evacuated and then the atmosphere in the reactor is replaced with nitrogen, and the atmosphere in the reactor is detected with an oxygen meter, and the evacuation-nitrogen replacement operation is repeated until the oxygen content in the reactor is less than 50ppm. At this time, the reactor is heated to 85°C, and then a diaphragm pump is used to charge the pre-mixed VDF / CTFE (the molar ratio of the two is 80:20) mixed gas into the reactor until the pressure in the reactor reaches 4.0MPa. 3.5g of dimethyl carbonate, 10g of ammonium persulfate and 3g of 0.15mol / L ammonium bicarbonate aqueous solution are respectively input into the reactor by a metering pump to start the polymerization reaction. During the polymerization process, an automatic control system is used to monitor the pressure in the reactor, and a diaphragm pump is continuously used to input VDF / CTFE (the molar ratio of the two is 80:20) mixed gas into the reactor, so that the pressure in the reactor is always maintained at 4.0MPa. Every time the reaction is carried out for 50 minutes, 3.5 grams of ammonium persulfate are added to the reactor, and a total of three additions are made; and every time the reaction is carried out for 50 minutes, 5 grams of IBVE are added to the reactor, and a total of two additions are made. When the total amount of VDF / CTFE mixed gas added reaches the preset value of 750 grams, the diaphragm pump is turned off, the feeding is stopped, the reaction time is recorded, and the temperature is cooled to room temperature. The reactor is opened to recover the small amount of gas monomer remaining in the reactor.
[0074] The emulsion material in the reaction kettle was collected and washed with deionized water for multiple times, and the conductivity of the washing water was tested after each washing until the conductivity of the washing water was lower than 5 μs / cm. A white material was obtained after drying.
[0075] The weight average molecular weight of the product of this example was measured using a gel permeation chromatograph produced by Agilent Technologies.
[0076] The melting point of the product of this example was measured using a differential scanning calorimeter produced by TA Corporation.
[0077] The viscosity of the product of this example was measured using a viscometer produced by Brookfield.
[0078] The peeling force of the product of this embodiment was tested using a tensile testing machine produced by Zwick / Roell according to the method of GB / T2790-1995 "Test method for 180° peel strength of adhesives - flexible material to rigid material".
[0079] Through the following steps, the copolymer prepared in this embodiment is used to manufacture a silicon negative electrode plate, the original thickness of the negative electrode plate is tested, and then the silicon-based negative electrode plate is assembled into a lithium-ion battery, and the silicon-based electrode is used to perform a charge-discharge cycle. After 1000 charge-discharge cycles, the plate is taken out, the plate thickness is tested again, and the plate thickness expansion rate is calculated.
[0080] The copolymer of the present invention is dissolved in N-methylpyrrolidone solvent to prepare a 5% concentration of glue as a binder. Silicon powder with a particle size of about 1 micron, graphite powder and the above binder are mixed evenly according to a weight ratio of 95:3:2 (herein, the weight of the copolymer in the binder) to form a slurry with a solid content of about 56%. The slurry is coated on a copper foil using a coating machine, dried at 60°C, and rolled at a pressure of 0.3Mpa to prepare a silicon negative electrode sheet.
[0081] The above-mentioned electrode sheet was sliced and weighed, and the thickness was measured with a thickness gauge. It was assembled together with the metal lithium sheet and the PP separator in a glove box, and 80 μl of 1 mol / L lithium battery electrolyte (LiPF6+ethylene carbonate (EC)+diethyl carbonate ethyl carbonate (DEC)) was injected into it, and then the performance of the lithium-ion battery was tested.
[0082] The test results are summarized in Table 1.
[0083] Example 2
[0084] In this example, P(VDF-CTFE-IBVE) was synthesized and its properties were characterized.
[0085] The copolymerization reaction is carried out in a 20-liter high-pressure polymerization reactor. First, 10kg of deionized water, 9.5g of ammonium hexafluoroepoxy tetracarboxylate and 65g of monomer IBVE are added to the reactor, the reactor is closed, stirring is started, the reactor is evacuated and then the atmosphere in the reactor is replaced with nitrogen, and the atmosphere in the reactor is detected with an oxygen meter, and the evacuation-nitrogen replacement operation is repeated until the oxygen content in the reactor is less than 50ppm. At this time, the reactor is heated to 85°C, and then a diaphragm pump is used to charge the pre-mixed VDF / CTFE (the molar ratio of the two is 80:20) mixed gas into the reactor until the pressure in the reactor reaches 4.0MPa. 3.5g of dimethyl carbonate, 10g of ammonium persulfate and 3g of 0.15mol / L ammonium bicarbonate aqueous solution are respectively input into the reactor by a metering pump to start the polymerization reaction. During the polymerization process, an automatic control system is used to monitor the pressure in the reactor, and a diaphragm pump is continuously used to input VDF / CTFE (the molar ratio of the two is 80:20) mixed gas into the reactor, so that the pressure in the reactor is always maintained at 4.0MPa. Every time the reaction is carried out for 50 minutes, 3.5 grams of ammonium persulfate are added to the reactor, and a total of three additions are made; and every time the reaction is carried out for 50 minutes, 5 grams of IBVE are added to the reactor, and a total of two additions are made. When the total amount of VDF / CTFE mixed gas added reaches the preset value of 750 grams, the diaphragm pump is turned off, the feeding is stopped, the reaction time is recorded, and the temperature is cooled to room temperature. The reactor is opened to recover the small amount of gas monomer remaining in the reactor.
[0086] The emulsion material in the reaction kettle was collected and washed with deionized water for multiple times, and the conductivity of the washing water was tested after each washing until the conductivity of the washing water was lower than 5 μs / cm. A white material was obtained after drying.
[0087] The weight average molecular weight, melting point, viscosity, peel force and thickness expansion ratio after 1000 charge-discharge cycles of the product of this example were tested in the same manner as in Example 1. The test results are summarized in Table 1.
[0088] in addition, Figure 1 The first two charge-discharge curves of a lithium-ion battery manufactured using the copolymer of this example are shown.
[0089] Example 3
[0090] In this example, P(VDF-CTFE-IBVE) was synthesized and its properties were characterized.
[0091] The copolymerization reaction is carried out in a 20-liter high-pressure polymerization reactor. First, 10kg of deionized water, 9.5g of ammonium hexafluoroepoxy tetracarboxylate and 100g of monomer IBVE are added to the reactor, the reactor is closed, stirring is started, the reactor is evacuated and then the atmosphere in the reactor is replaced with nitrogen, and the atmosphere in the reactor is detected with an oxygen meter, and the evacuation-nitrogen replacement operation is repeated until the oxygen content in the reactor is less than 50ppm. At this time, the reactor is heated to 85°C, and then a diaphragm pump is used to charge the pre-mixed VDF / CTFE (the molar ratio of the two is 90:10) mixed gas into the reactor until the pressure in the reactor reaches 4.0MPa. 3.5g of dimethyl carbonate, 10g of ammonium persulfate and 3g of 0.15mol / L ammonium bicarbonate aqueous solution are respectively input into the reactor by a metering pump to start the polymerization reaction. During the polymerization process, an automatic control system is used to monitor the pressure in the reactor, and a diaphragm pump is used to continuously input VDF / CTFE (the molar ratio of the two is 90:10) mixed gas into the reactor, so that the pressure in the reactor is always maintained at 4.0MPa. Every time the reaction is carried out for 50 minutes, 3.5 grams of ammonium persulfate are added to the reactor, and a total of three additions are made; and every time the reaction is carried out for 50 minutes, 5 grams of IBVE are added to the reactor, and a total of two additions are made. When the total amount of VDF / CTFE mixed gas added reaches the preset value of 750 grams, the diaphragm pump is turned off, the feeding is stopped, the reaction time is recorded, and the temperature is cooled to room temperature. The reactor is opened to recover the small amount of gas monomer remaining in the reactor.
[0092] The emulsion material in the reaction kettle was collected and washed with deionized water for multiple times, and the conductivity of the washing water was tested after each washing until the conductivity of the washing water was lower than 5 μs / cm. A white material was obtained after drying.
[0093] The weight average molecular weight, melting point, viscosity, peel force and thickness expansion ratio after 1000 charge-discharge cycles of the product of this example were tested in the same manner as in Example 1. The test results are summarized in Table 1.
[0094] Example 4
[0095] In this example, P(VDF-CTFE-IBVE) was synthesized and its properties were characterized.
[0096] The copolymerization reaction is carried out in a 20-liter high-pressure polymerization reactor. First, 10kg of deionized water, 9.5g of ammonium hexafluoroepoxy tetracarboxylate and 120g of monomer IBVE are added to the reactor, the reactor is closed, stirring is started, the reactor is evacuated and then the atmosphere in the reactor is replaced with nitrogen, and the atmosphere in the reactor is detected with an oxygen meter, and the evacuation-nitrogen replacement operation is repeated until the oxygen content in the reactor is less than 50ppm. At this time, the reactor is heated to 85°C, and then a diaphragm pump is used to charge the pre-mixed VDF / CTFE (the molar ratio of the two is 90:10) mixed gas into the reactor until the pressure in the reactor reaches 4.0MPa. 3.5g of dimethyl carbonate, 10g of ammonium persulfate and 3g of an aqueous solution of ammonium bicarbonate with a concentration of 0.15mol / L are respectively input into the reactor by a metering pump to start the polymerization reaction. During the polymerization process, an automatic control system is used to monitor the pressure in the reactor, and a diaphragm pump is used to continuously input VDF / CTFE (the molar ratio of the two is 90:10) mixed gas into the reactor, so that the pressure in the reactor is always maintained at 4.0MPa. Every time the reaction is carried out for 50 minutes, 3.5 grams of ammonium persulfate are added to the reactor, and a total of three additions are made; and every time the reaction is carried out for 50 minutes, 5 grams of IBVE are added to the reactor, and a total of two additions are made. When the total amount of VDF / CTFE mixed gas added reaches the preset value of 750 grams, the diaphragm pump is turned off, the feeding is stopped, the reaction time is recorded, and the temperature is cooled to room temperature. The reactor is opened to recover the small amount of gas monomer remaining in the reactor.
[0097] The emulsion material in the reaction kettle was collected and washed with deionized water for multiple times, and the conductivity of the washing water was tested after each washing until the conductivity of the washing water was lower than 5 μs / cm. A white material was obtained after drying.
[0098] The weight average molecular weight, melting point, viscosity, peel force and thickness expansion ratio after 1000 charge-discharge cycles of the product of this example were tested in the same manner as in Example 1. The test results are summarized in Table 1.
[0099] Comparative Example 1
[0100] In this comparative example, PVDF was synthesized and its properties were characterized and compared with those of the copolymer of the present invention.
[0101] The copolymerization reaction is carried out in a 20-liter high-pressure polymerization reactor. First, 10kg of deionized water and 9.5g of ammonium hexafluoroepoxy tetracarboxylate are added to the reactor, the reactor is closed, stirring is started, the reactor is evacuated and then the atmosphere in the reactor is replaced with nitrogen, and the atmosphere in the reactor is detected with an oxygen meter, and the evacuation-nitrogen replacement operation is repeated until the oxygen content in the reactor is less than 50ppm. At this time, the reactor is heated to 85°C, and then VDF gas is filled into the reactor using a diaphragm pump until the pressure in the reactor reaches 4.0MPa. 3.5g of dimethyl carbonate, 10g of ammonium persulfate and 3g of an aqueous solution of ammonium bicarbonate with a concentration of 0.15mol / L are respectively input into the reactor by a metering pump to start the polymerization reaction. During the polymerization reaction, the pressure in the reactor is monitored using an automatic control system, and the VDF gas is continuously input into the reactor using a diaphragm pump so that the pressure in the reactor is always maintained at 4.0MPa. Every time the reaction lasts for 50 minutes, 3.5 grams of ammonium persulfate is added to the reactor for a total of three times. When the total amount of VDF gas added reaches the preset value of 750 grams, the diaphragm pump is turned off, the feed is stopped, the reaction time is recorded, the temperature is lowered to room temperature, the reactor is opened, and the small amount of gas monomer remaining in the reactor is recovered.
[0102] The emulsion material in the reaction kettle was collected and washed with deionized water for multiple times, and the conductivity of the washing water was tested after each washing until the conductivity of the washing water was lower than 5 μs / cm. A white material was obtained after drying.
[0103] The weight average molecular weight, melting point, viscosity, peel force and thickness expansion ratio after 1000 charge-discharge cycles of the comparative example product were measured in the same manner as in Example 1. The measurement results are summarized in Table 1.
[0104] in addition, Figure 2 The first two charge-discharge curves of lithium-ion batteries made using the PVDF of this comparative example are shown.
[0105] Table 1 Performance test of products of Examples 1-4 and Comparative Example 1
[0106]
[0107] From the above experimental results, it can be seen that compared with Comparative Example 1, the copolymer of the embodiment of the present invention can not only enhance its adhesion, but also improve its stability, mechanical strength and flexibility. After using it as a silicon negative electrode binder, the peeling force of the pole piece is improved, the thickness expansion rate of the pole piece is reduced after multiple charge-discharge cycles, and the coulomb efficiency of the first charge-discharge cycle of the battery is greatly improved.
Claims
1. A copolymer, comprising: (1) a first copolymerized unit derived from vinylidene fluoride; (2) a second comonomer derived from a second comonomer which is a C2-C6 olefin containing at least one fluorine atom and at least one non-fluorine halogen atom; (3) a third copolymerized unit derived from a third copolymerized monomer represented by the following formula I: R1-O-R2 formula I Wherein R1 is selected from: C2-C8 alkyl, C2-C8 haloalkyl, C3-C8 cycloalkyl, C3-C8 halocycloalkyl, C6-C12 aryl; R2 is selected from: C2-C6 alkenyl, halogenated C2-C6 alkenyl.
2. The copolymer according to claim 1, characterized in that In the copolymer, the molar ratio of the first copolymerization unit to the second copolymerization unit is 99:1 to 75:25; In the copolymer, the weight ratio of the sum of the weights of the first copolymerization unit and the second copolymerization unit to the third copolymerization unit is: (first copolymerization unit+second copolymerization unit):third copolymerization unit=100:0.5 to 100:
20.
3. The copolymer according to claim 1, characterized in that The weight average molecular weight of the copolymer is 20,000 to 2.2 million.
4. The copolymer according to any one of claims 1 to 3, characterized in that The second comonomer is chlorotrifluoroethylene, and the third comonomer is isobutyl vinyl ether.
5. A method for preparing the copolymer according to any one of claims 1 to 4, the method comprising carrying out a copolymerization reaction in a reactor containing vinylidene fluoride, a second comonomer, a third comonomer, an emulsifier, a chain transfer agent, an initiator, a pH adjuster and water to form the copolymer.
6. The method according to claim 5, characterized in that The chain transfer agent is selected from one or more of the following: dimethyl carbonate, diethyl carbonate, ethylene carbonate, ethyl methyl carbonate, ethyl acetate, methyl propionate, ethyl propionate; The initiator is selected from one or more of the following: alkali metal persulfate, sodium peroxyphosphate, potassium peroxyphosphate, ammonium persulfate, peroxysuccinic acid, dibenzoyl peroxide, tert-butyl perbenzoate, dibenzoyl peroxide; The pH regulator is selected from one or more of the following: NaHSO3, Na2CO3, NaHCO3, Na2S2O3, Na2HPO3, KHCO3, K2HPO3, K2CO3, NH4HCO3, CH3COONH 4、 Triethylolamine; The emulsifier is selected from one or more of the following: fluorine-containing carboxylates and fluorine-containing sulfonates.
7. The method according to claim 5, characterized in that The ratio of the total weight of vinylidene fluoride and the second comonomer added to the reactor to the weight of water is 1:100 to 20:100; The weight ratio of the emulsifier to water is 0.02:100 to 1.75:100; The weight ratio of chain transfer to water is 0.002:100 to 6:100; The weight ratio of the initiator to water is 0.06:100 to 6:100; The pH adjuster is used to maintain the pH value at 8-10 during the copolymerization reaction.
8. The method according to claim 5, characterized in that The copolymerization reaction is carried out at a reaction temperature of 60-90° C. under anaerobic conditions, wherein at least a portion of the first comonomer, the second comonomer and the third comonomer are intermittently or continuously fed into the reactor during the copolymerization reaction.
9. A binder comprising the copolymer according to any one of claims 1 to 4.
10. A lithium ion battery comprising the binder of claim 9 applied on or in an electrode.