Polypropylene flame-retardant composite material reinforced by waste wind power blade material and preparation method thereof

By modifying the waste wind power blade powder and combining it with the flame retardant, polypropylene composite material with excellent mechanical and flame retardant properties is prepared, which solves the poor mechanical properties and reuse of waste wind power blades and the poor mechanical properties in the treatment and reuse of waste wind power blades. Environmental pollution problems have achieved efficient resource regeneration.

CN118955963APending Publication Date: 2024-11-15SICHUAN UNIV
View PDF 0 Cites 7 Cited by

Patent Information

Application Number
CN202411107779.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively deal with and reuse waste wind power blades, and traditional methods have problems such as environmental pollution, waste of resources and poor mechanical properties.

Method used

The waste wind power blade powder modified with coupling agent is combined with the flame retardant PAPI and MPP to prepare a polypropylene flame retardant composite material with mechanical strength and excellent flame retardant properties.

Benefits of technology

It significantly improves the mechanical properties and flame retardant properties of polypropylene composite materials, expands the high-value application scenarios of waste wind power blade materials, and realizes efficient reuse of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955963A_ABST
    Figure CN118955963A_ABST
Patent Text Reader

Abstract

The invention provides a polypropylene flame-retardant composite material reinforced by using a waste wind power blade material and a preparation method thereof, the waste wind power blade material is preliminarily crushed, the crushed material is added into a millstone-type solid-phase mechanochemical reactor for grinding and crushing, wind power blade powder is collected, the wind power blade powder is added into a coupling agent solution for dipping treatment, and the composite material is obtained. And mixing the coupling agent modified wind power blade powder with polypropylene, polypropylene grafted maleic anhydride, piperazine phytate and melamine polyphosphate, and carrying out extrusion granulation to obtain the polypropylene flame-retardant composite material. According to the invention, the coupling agent modified waste wind power blade powder is compounded with the flame retardants PAPI and MPP which are prepared by ionic reaction, so that the polypropylene flame-retardant composite material with mechanical strength and excellent flame retardance is successfully prepared, and a high-value application scene is expanded for reutilization of waste wind power blade materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of recycling waste / retired wind turbine blade materials, and specifically relates to a flame-retardant polypropylene composite material reinforced with waste wind turbine blade materials and a preparation method thereof, and particularly relates to processing the above-mentioned waste wind turbine blade materials using a mechanochemical reactor disclosed in China's authorized invention patent ZL95111258.9. Background Art

[0002] As a clean, renewable and abundant energy source, wind power can reduce dependence on traditional fossil fuels and slow down global warming. It has become a key driving force for global energy transformation. However, the booming development of wind power generation has also brought about the problem of handling old wind power equipment, especially the inability to effectively handle wind turbine blades. The structural material of wind turbine blades is mainly fiber-reinforced epoxy resin composite materials, while epoxy resin is a thermosetting resin that cannot be melted and processed after solidification. It is estimated that for every 1kW installed wind turbine, about 10kg of structural materials are required. At present, the installed capacity of wind power is usually megawatt-level, and a wind turbine requires several tons of structural materials. With the trend of large-scale wind turbine blades and the further increase in total installed capacity, it will bring more severe problems in the treatment of retired wind turbine blades. Traditional landfill and incineration treatment seriously pollute the environment and waste resources greatly. Therefore, how to deal with retired wind turbine blades (WTB) in a green and effective way is a very challenging problem. It is urgent to develop new methods and technologies for recycling and utilizing abandoned retired wind turbine blades to realize their resource utilization.

[0003] Wind turbine blades are mainly made of fiber-reinforced epoxy resin materials. Currently, most of the wind power industry uses glass fiber-reinforced epoxy resin. This composite material is difficult to dispose of due to the irreversible three-dimensional cross-linked network of the matrix epoxy resin. Currently, various methods for disposing retired wind turbine blades in industry and academic research are roughly divided into direct utilization, energy recovery, pyrolysis recovery, solvent decomposition recovery and mechanical recovery.

[0004] The direct utilization method has the lowest cost and does not cause pollution to the environment, but the utilization scenarios of the blades after cutting are limited, and it cannot cope with the retirement of a large number of wind turbine blades in recent years, and the reused wind turbine blades will face the problem of re-disposal. Energy recovery uses the heat released by the combustion of epoxy resin and other organic matter in the blades to generate electricity, heating, etc. This method can directly use existing equipment and has a low cost, but the combustion of organic matter may produce CO and NO due to incomplete combustion, and the residue after combustion contains a large amount of reinforcing fibers (more than 70%), which causes waste of resources and environmental pollution, and does not conform to the current concept of sustainable development. The pyrolysis method uses high temperature to degrade the matrix resin of the wind turbine blade into small molecular substances to utilize the fibers therein. This method has strong adaptability, but it consumes a lot of energy and has a high cost. It is currently mostly used for the recovery of carbon fibers; and high temperature will seriously damage the mechanical properties of recycled fibers, especially glass fibers, shorten their service life, and high temperature pyrolysis will also produce toxic and harmful gases, which makes this method have high requirements for equipment, especially large-scale industrial equipment. The solvent decomposition recycling method is effective in recycling retired wind turbine blades and can obtain regenerated fibers with high retained strength. Currently, there are a lot of studies using different catalytic solvent systems to decompose fiber-reinforced thermosetting resins; however, this method uses acid-base catalysts and a large amount of solvents, and the waste liquid needs to be treated, otherwise it will cause environmental pollution. In addition, its process is complicated. For materials with different compositions, different systems are required to achieve a good decomposition effect. The matrix resin after decomposition is complex and difficult to separate and reuse. This method is currently only used in the laboratory stage, and the technical maturity is not high.

[0005] In order to provide a new approach for the recycling of discarded wind turbine blades, the present invention applies for a prior patent application "Glass fiber reinforced plastic recycled products using discarded wind turbine blades as raw materials and preparation method thereof" (CN118063854A) provides a method for preparing highly compatible and reactive fillers using discarded wind turbine blades, comprising adding the discarded wind turbine blade products into a grinding disc-type solid phase force chemical reactor after pretreatment for grinding and pulverizing to obtain ultrafine wind turbine blade powder, then mixing the ultrafine wind turbine blade powder with an activator and co-grinding to obtain a highly compatible and reactive filler; and then using the highly compatible and reactive filler as part of the raw material to prepare the glass fiber reinforced plastic recycled products.

[0006] However, in the above patent application, only a new basic approach for the recycling of discarded wind turbine blades is provided. The highly compatible and reactive fillers prepared by the invention can be added to resin base materials as part of the raw materials, which means that they have basic enhanced functionality and successfully point out a new recycling approach for discarded wind turbine blades. However, in the technical solution of the patent application, there is still a blank in terms of high-value empowerment for the reuse of discarded wind turbine blades. Summary of the invention

[0007] In order to solve the problems in the above-mentioned prior art, the present invention provides a polypropylene flame-retardant composite material reinforced with waste wind turbine blade materials and a preparation method thereof. The composite material is compounded with waste wind turbine blade powder modified by a coupling agent and flame retardants PAPI and MPP prepared by ion reaction to successfully prepare a polypropylene flame-retardant composite material with both mechanical strength and excellent flame retardant properties, thereby expanding high-value application scenarios for the reuse of waste wind turbine blade materials.

[0008] To achieve the above objectives, the present invention is implemented by adopting a technical solution consisting of the following technical measures.

[0009] In one aspect, the present invention provides a method for preparing a flame-retardant polypropylene composite material reinforced with waste wind turbine blade materials, which mainly comprises the following steps:

[0010] (1) After pretreatment including cleaning, the waste wind turbine blade materials are crushed into wind turbine blade fragments with an average particle size of no more than 3 cm;

[0011] (2) adding the wind turbine blade fragments obtained in step (1) into a disc-type solid phase force chemical reactor for grinding and pulverization, and collecting the wind turbine blade powder after the grinding is completed; wherein the process parameters of the disc-type solid phase force chemical reactor are: grinding pressure of 4 to 6 MPa, the temperature of the disc surface is controlled at -8 to -4°C by passing a circulating cooling liquid, the grinding is repeated 1 to 3 times, and the disc speed is 80 to 100 rpm;

[0012] (3) diluting an amino-containing silane coupling agent to a coupling agent solution with a mass concentration of 1 to 3 wt%, adding the wind turbine blade powder obtained in step (2) to the coupling agent solution for immersion treatment for at least 30 min, and obtaining a wind turbine blade powder modified with the coupling agent after drying;

[0013] (4) The coupling agent-modified wind turbine blade powder obtained in step (3) is mixed evenly with the following raw materials according to weight percentage to form a mixed material:

[0014]

[0015] (5) Extruding and granulating the mixture obtained in step (4) to obtain a polypropylene flame retardant composite material.

[0016] On the other hand, the present invention is based on the preparation of a polypropylene flame-retardant composite material, and can prepare a polypropylene flame-retardant recycled product using waste wind turbine blade materials through conventional thermoplastic processing methods.

[0017] In this article, step (1) includes a pretreatment of cleaning, which is mainly to remove impurities on the surface of the waste wind turbine blade material. If necessary, part of the non-wind turbine blade material needs to be removed. Technical personnel in this field can perform specific treatment according to the actual conditions of the waste wind turbine blade products that need to be recycled and based on the existing technology.

[0018] In this article, the wind turbine blade fragments processed and crushed to an average particle size of no more than 3 cm in step (1) can be processed and crushed in a conventional manner to facilitate the placement of the fragments into a disc-type solid phase force chemical reactor for grinding, for example, by using existing conventional crushing equipment such as a jaw crusher, a planetary ball mill, and a cryogenic ball mill.

[0019] Herein, the grinding disc type solid phase mechanochemical reactor in step (2) is the mechanochemical reactor disclosed in the prior authorized patent ZL 95111258.9 of the applicant of the present invention.

[0020] In this article, the actual operation of the cyclic milling process described in step (2) is to grind the milled material in a disc-shaped solid phase force chemical reactor, collect the product at the discharge end, and then place it in a disc-shaped solid phase force chemical reactor for grinding again. The above process is regarded as one cycle of milling.

[0021] In one of the technical solutions, the temperature of the grinding disc surface in step (2) is controlled to be -8 to -4°C by introducing circulating cooling liquid, and the cooling liquid is ethylene glycol or water.

[0022] Herein, the amino-containing silane coupling agent in step (3) is a commercially available silane coupling agent containing amino functional groups commonly used in the prior art, for example, any one or more of KH550, KH560, and KH570.

[0023] It should be noted that one of the inventive points of the present invention is that, through comparative experiments, it was found that when the wind turbine blade powder modified with an amino-containing silane coupling agent was used as a reinforcing filler, it showed a significant improvement in mechanical properties when compared with the wind turbine blade powder not modified with an amino-containing silane coupling agent as a comparative experimental group, which solved the problem of poor mechanical strength of discarded wind turbine blades during mechanical recycling and reuse, and provided a theoretical and experimental basis for the high-value empowerment of the reuse of discarded wind turbine blades, and is expected to be applied to the recycling of large-scale discarded / retired wind turbine blades.

[0024] In one of the technical solutions, comparative experiments found that when the amino-containing silane coupling agent in step (3) is selected as KH550, the prepared wind turbine blade powder modified by the coupling agent has the best enhanced mechanical properties for the polymer matrix. In the verification example, the tensile strength and modulus of the polypropylene-based composite material prepared by the wind turbine blade powder modified by KH550 reached 43.27MPa and 1148.64MPa, respectively, which were increased by 37.1% and 147.3%, respectively, compared with pure PP.

[0025] In this article, the step (3) dilutes the amino-containing silane coupling agent to a coupling agent solution with a mass concentration of 1 to 3 wt%, wherein the dilution and the solvent used for dilution are selected by conventional known methods when the silane coupling agent is used. Those skilled in the art can directly select an appropriate method according to the common knowledge in the art or according to the instructions for use of the amino-containing silane coupling agent.

[0026] In order to better illustrate the present invention and provide a technical solution for reference, the amino-containing silane coupling agent is diluted to a coupling agent solution with a mass concentration of 1 to 3 wt %, wherein the solvent used for the dilution is a mixture of ethanol and water, and the mass ratio of the two is 4:1.

[0027] In this article, step (3) is described as adding the wind turbine blade powder obtained in step (2) to a coupling agent solution and immersing it for at least 30 minutes, wherein the immersion treatment is a conventional treatment method in the art, for example, adding the wind turbine blade powder obtained in step (2) to a coupling agent solution and immersing it for at least 30 minutes, and the mass of the wind turbine blade powder is not more than 40% of the mass of the coupling agent solution.

[0028] Furthermore, the reason why the present invention utilizes amino-containing silane coupling agents is that one end of their molecular chains has organic functional groups of different structures, thus having different polarities, and their compatibility with the polypropylene matrix will also be different. Another inventive point of the present invention is that it was surprisingly found during the experiment that there was a synergistic effect between the amino-containing silane coupling agent and polypropylene grafted maleic anhydride, and through comparative experiments it was found that the combination of KH550 and polypropylene grafted maleic anhydride produced the best results, and a polypropylene-based composite material with the best mechanical properties was obtained. The synergistic mechanism between KH550 and polypropylene grafted maleic anhydride is as follows: Figure 3As shown. First, the silanol groups formed by the hydrolysis of KH550 can react with the hydroxyl groups on the surface of the glass fiber in the wind turbine blade powder, so that the -NH2 in KH550 can be grafted onto the fiber surface. The introduction of the -NH2 functional group enhances the compatibility between the glass fiber and the polypropylene matrix. Subsequently, the anhydride groups in the polypropylene grafted maleic anhydride can react with -NH2 at high temperatures to form amide bonds. At the same time, the non-polar PP molecular chains in the polypropylene grafted maleic anhydride will be chain entangled with the PP matrix. This complex process ultimately leads to a significant increase in the interfacial strength between the glass fiber and PP.

[0029] In one of the more preferred technical solutions, in order to further improve the mechanical properties of the prepared polypropylene flame retardant composite material, the amino-containing silane coupling agent in step (3) is selected as KH550, and KH550 is diluted to a coupling agent solution with a mass concentration of 2wt%, and the amount of polypropylene grafted maleic anhydride added in step (4) is 5wt% of the mixture.

[0030] Herein, the phytic acid piperazine in step (4) is a flame retardant containing nitrogen and phosphorus elements prepared by a solution synthesis method using phytic acid and piperazine, and those skilled in the art can directly prepare it according to the technical contents disclosed in the prior art literature.

[0031] Another inventive point of the present invention is that a polypropylene flame retardant composite material having both mechanical properties and excellent flame retardancy is prepared by compounding piperazine phytate with melamine polyphosphate.

[0032] In order to further enhance the synergistic flame retardant effect of the compound of phytic acid piperazine and melamine polyphosphate, in one preferred technical scheme, the preparation method of phytic acid piperazine in step (4) is as follows:

[0033] Piperazine (7.75 g, 0.09 mol) is completely dissolved in 300 mL of ethanol under mechanical stirring to prepare a piperazine solution; subsequently, a phytic acid solution (PA, 39.6 g, 50 wt% aqueous solution, 0.03 mol) is dissolved in 150 mL of ethanol, and then added dropwise to the piperazine solution to react at room temperature for 12 hours; after the reaction time is reached, a white product is collected by suction filtration and washed with ethanol for 3 to 5 times to remove unreacted piperazine and phytic acid; finally, the obtained white product is dried at 80° C. for 12 hours to obtain phytic acid piperazine with a phosphorus content of 28 wt%. In the preparation method, the yield of phytic acid piperazine is about 90%.

[0034] When using the phytic acid piperazine (phosphorus content of 28wt%) prepared in the above preferred technical scheme, it was surprisingly found that its compound combination with melamine polyphosphate helps to slow down the reduction of the mechanical properties of the material at the proportion specified in the present invention. In one of the most preferred technical schemes, when the mass ratio of phytic acid piperazine to melamine polyphosphate is 2:1, and the addition amount of both is 20wt% of the mixture, the mechanical properties of the prepared polypropylene flame retardant composite material are close to those of the control group without adding flame retardant, which breaks through the conventional perception in the prior art that the addition of flame retardants will cause the deterioration of the mechanical properties of the composite material.

[0035] Herein, the polypropylene in step (4) is selected from conventional polypropylene industrial raw materials, such as at least one of conventional isotactic polypropylene, syndiotactic polypropylene, and atactic polypropylene, or a blend thereof; those skilled in the art can select a suitable polypropylene raw material according to actual product needs or process requirements.

[0036] Herein, the polypropylene grafted maleic anhydride in step (4) is a conventional industrial additive, which can be directly obtained from the market by a person skilled in the art, or prepared by the person skilled in the art according to the prior art literature in the art.

[0037] Herein, the uniform mixing in step (4) is a conventional process in the art, for example, uniform dispersion by mechanical stirring such as a high-speed rotary mixer.

[0038] Herein, the extrusion granulation described in step (4) is a conventional process for preparing polypropylene-based composite materials. Those skilled in the art may directly refer to the general process parameters of polypropylene materials or the methods described in the prior art literature in the field.

[0039] In order to better illustrate the present invention and provide a technical solution for reference, the specific process parameters of the extrusion granulation in step (4) are as follows: the temperatures of the extruder from the feed port to the die are set to 130°C, 175°C, 180°C, 180°C, 175°C and 170°C, respectively, and the screw speed is set to 80r / min.

[0040] The present invention has the following beneficial effects:

[0041] (1) The present invention provides a polypropylene flame-retardant composite material reinforced with waste wind turbine blade materials and a preparation method thereof. By compounding waste wind turbine blade powder modified with a coupling agent with flame retardants PAPI and MPP prepared by ion reaction, a polypropylene flame-retardant composite material with both mechanical strength and excellent flame retardant properties is successfully prepared, thereby expanding high-value application scenarios for the reuse of waste wind turbine blade materials.

[0042] (2) The present invention uses an amino-containing silane coupling agent to modify the wind turbine blade powder, significantly improving the mechanical properties of the polypropylene composite material. In one of the technical solutions, when KH550 is used, an amidation reaction occurs between the -NH2 in KH550 and the polypropylene grafted maleic anhydride, so that the final prepared polypropylene flame-retardant composite material has stronger mechanical properties.

[0043] (3) The synergistic use of piperazine phytate and melamine polyphosphate in the present invention helps to slow down the reduction of the mechanical properties of the material, and makes the modulus of the polypropylene flame-retardant composite material finally prepared better than that of the control example without adding flame retardant; in addition, the unreacted phosphate groups in piperazine phytate improve its compatibility with the polypropylene matrix, and melamine polyphosphate reduces the relative movement resistance between polypropylene molecular chains by virtue of its rigid nitrogen heterocycle, thereby improving the dispersibility.

[0044] (4) The present invention uses phytic acid piperazine and melamine polyphosphate in combination, and the maximum thermal decomposition temperature is increased by up to 20°C compared with the control example without adding flame retardant. This is mainly because the decomposition products of the flame retardant contribute to the carbonization of the polypropylene matrix, thereby slowing down the decomposition rate of the matrix and improving its thermal stability.

[0045] (5) The present invention effectively improves the flame retardant properties of the composite material by using phytic acid piperazine in conjunction with melamine polyphosphate, and their ratio has a significant effect on the flame retardant effect. When the mass ratio of phytic acid piperazine to melamine polyphosphate is 2:1, the prepared polypropylene flame retardant composite material reaches the UL-94V-0 flame retardant grade and has a limiting oxygen index of up to 37.8%. On the one hand, the phosphoric acid substances in the decomposition products of phytic acid piperazine can promote the formation of a dense and stable carbon layer in the polypropylene matrix. On the other hand, the inert gases such as ammonia generated by the decomposition of melamine polyphosphate can expand and foam the carbon layer, enhance its barrier effect, and dilute the concentration of combustible gases, so that the material can achieve a better flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 The FTIR spectrum and XPS spectrum of the coupling agent-modified wind turbine blade powder prepared in Examples 1 to 3 of the present invention are verified. Among them, Figure (a) is the full XPS spectrum; Figure (b) is the high-resolution spectrum of the 2p orbital of the Si element in the WTB powder; Figure (c) is the high-resolution spectrum of the 2p orbital of the Si element in the coupling agent-modified wind turbine blade powder prepared in Example 1; Figure (d) is the FTIR spectrum; Figure (e) is the high-resolution spectrum of the 2p orbital of the Si element in the coupling agent-modified wind turbine blade powder prepared in Example 2; Figure (f) is the high-resolution spectrum of the 2p orbital of the Si element in the coupling agent-modified wind turbine blade powder prepared in Example 3.

[0047] Figure 2 The mechanical properties test results of the polypropylene composite strips prepared in Examples 4 to 8 are verified. Figure (a) is a tensile strength and tensile modulus comparison point diagram; Figure (b) is a flexural strength and flexural modulus comparison point diagram; Figure (c) is a notched impact strength comparison line diagram; Figure (d) is a comprehensive comparison radar diagram.

[0048] Figure 3 Schematic diagram of the structures of different coupling agents in the present invention and the synergistic enhancement mechanism of the interface strength between PP and glass fiber by KH550 and PP-g-MAH.

[0049] Figure 4 The tensile and bending performance test results of the polypropylene flame retardant composite strips prepared in Examples 1 to 3 and Comparative Examples 2 to 3 of the present invention are shown in Figure (a) as a line graph comparing tensile strength and tensile modulus; Figure (b) as a line graph comparing bending strength and bending modulus.

[0050] Figure 5 The TG and DTG comparison curves of the polypropylene flame retardant composite strips prepared in Examples 1 to 3 and Comparative Examples 2 to 3 of the present invention are shown in Figure (a) for the TG curve comparison and Figure (b) for the DTG curve comparison.

[0051] Figure 6 The following are the combustion state diagrams of the flame-retardant composite strips of polypropylene prepared in Examples 1 to 3 and Comparative Examples 2 to 3 during the vertical combustion test. Among them, Figure (a) corresponds to the flame-retardant composite strips of polypropylene prepared in Comparative Example 2; Figure (b) corresponds to the flame-retardant composite strips of polypropylene prepared in Comparative Example 3; Figure (c) corresponds to the flame-retardant composite strips of polypropylene prepared in Example 1; Figure (d) corresponds to the flame-retardant composite strips of polypropylene prepared in Example 2; Figure (e) corresponds to the flame-retardant composite strips of polypropylene prepared in Example 3; Figure (f) corresponds to the combustion state images of the flame-retardant composite strips of polypropylene prepared in Example 3 during the second ignition; Figures (a) to (f) all correspond to the combustion state at the 2nd second of ignition.

[0052] Figure 7 The HRR and THR comparison curves of the polypropylene flame retardant composite samples prepared in Example 3 and Comparative Examples 1 to 3 are shown in FIG. 1A and FIG. 1B are HRR comparison curves and FIG. 1C and FIG. 1D are THR comparison curves.

[0053] Figure 8 The residual carbon morphology of the polypropylene flame retardant composite sample prepared in Example 3 and Comparative Examples 1 to 3 after cone calorimetry test. Among them, Figure (a) corresponds to the polypropylene flame retardant composite sample prepared in Comparative Example 1; Figure (b) corresponds to the polypropylene flame retardant composite sample prepared in Comparative Example 2; Figure (c) corresponds to the polypropylene flame retardant composite sample prepared in Comparative Example 3; Figure (d) corresponds to the polypropylene flame retardant composite sample prepared in Example 3. DETAILED DESCRIPTION

[0054] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously change or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention. Although it is believed that those of ordinary skill in the art fully understand the following terms, the following definitions are still stated to help illustrate the subject matter disclosed by the present invention.

[0055] In one aspect, the present invention provides a method for preparing a flame-retardant polypropylene composite material reinforced with waste wind turbine blade materials, which mainly comprises the following steps:

[0056] (1) After pretreatment including cleaning, the waste wind turbine blade materials are crushed into wind turbine blade fragments with an average particle size of no more than 3 cm;

[0057] (2) adding the wind turbine blade fragments obtained in step (1) into a disc-type solid phase force chemical reactor for grinding and pulverization, and collecting the wind turbine blade powder after the grinding is completed; wherein the process parameters of the disc-type solid phase force chemical reactor are: grinding pressure of 4 to 6 MPa, the temperature of the disc surface is controlled at -8 to -4°C by passing a circulating cooling liquid, the grinding is repeated 1 to 3 times, and the disc speed is 80 to 100 rpm;

[0058] (3) diluting an amino-containing silane coupling agent to a coupling agent solution with a mass concentration of 1 to 3 wt%, adding the wind turbine blade powder obtained in step (2) to the coupling agent solution for immersion treatment for at least 30 min, and obtaining a wind turbine blade powder modified with the coupling agent after drying;

[0059] (4) The coupling agent-modified wind turbine blade powder obtained in step (3) is mixed evenly with the following raw materials according to weight percentage to form a mixed material:

[0060]

[0061] (5) Extruding and granulating the mixture obtained in step (4) to obtain a polypropylene flame retardant composite material.

[0062] On the other hand, the present invention is based on the preparation of a polypropylene flame-retardant composite material, and can prepare a polypropylene flame-retardant recycled product using waste wind turbine blade materials through conventional thermoplastic processing methods.

[0063] In this article, step (1) includes a pretreatment of cleaning, which is mainly to remove impurities on the surface of the waste wind turbine blade material. If necessary, part of the non-wind turbine blade material needs to be removed. Technical personnel in this field can perform specific treatment according to the actual conditions of the waste wind turbine blade products that need to be recycled and based on the existing technology.

[0064] In this article, the wind turbine blade fragments processed and crushed to an average particle size of no more than 3 cm in step (1) can be processed and crushed in a conventional manner to facilitate the placement of the fragments into a disc-type solid phase force chemical reactor for grinding. In one embodiment, the fragments are processed by conventional crushing equipment such as a jaw crusher, a planetary ball mill, or a cryogenic ball mill.

[0065] Herein, the grinding disc type solid phase mechanochemical reactor in step (2) is the mechanochemical reactor disclosed in the prior authorized patent ZL 95111258.9 of the applicant of the present invention.

[0066] In this article, the actual operation of the cyclic milling process described in step (2) is to grind the milled material in a disc-shaped solid phase force chemical reactor, collect the product at the discharge end, and then place it in a disc-shaped solid phase force chemical reactor for grinding again. The above process is regarded as one cycle of milling.

[0067] In one embodiment, the temperature of the grinding disc surface in step (2) is controlled to be -8 to -4°C by introducing circulating cooling liquid, and the cooling liquid is ethylene glycol or water.

[0068] In one embodiment, the process parameters of the grinding disc type solid phase force chemical reactor in step (2) are: grinding pressure of 4 to 6 MPa, for example, 4 MPa, 4.5 MPa, 5 MPa, 5.5 MPa, 6 MPa or any range or point value therebetween; the grinding disc surface temperature is controlled by introducing circulating cooling liquid to a temperature of -8 to -4°C, for example, -8°C, -7°C, -6°C, -5°C, -4°C or any range or point value therebetween; cyclic grinding is performed 1 to 3 times, for example, 1 time, 2 times or 3 times; the grinding disc speed is 80 to 100 rpm, for example, 80 rpm, 85 rpm, 90 rpm, 95 rpm, 100 rpm or any range or point value therebetween.

[0069] Herein, the amino-containing silane coupling agent in step (3) is a commercially available silane coupling agent containing amino functional groups commonly used in the prior art. In one embodiment, for example, any one or more of KH550, KH560, and KH570 are selected.

[0070] It should be noted that one of the inventive points of the present invention is that, through comparative experiments, it was found that when the wind turbine blade powder modified with an amino-containing silane coupling agent was used as a reinforcing filler, it showed a significant improvement in mechanical properties when compared with the wind turbine blade powder not modified with an amino-containing silane coupling agent as a comparative experimental group, which solved the problem of poor mechanical strength of discarded wind turbine blades during mechanical recycling and reuse, and provided a theoretical and experimental basis for the high-value empowerment of the reuse of discarded wind turbine blades, and is expected to be applied to the recycling of large-scale discarded / retired wind turbine blades.

[0071] In one embodiment, it is found through comparative experiments that when the amino-containing silane coupling agent in step (3) is selected as KH550, the wind turbine blade powder modified by the coupling agent has the best enhanced mechanical properties for the polymer matrix. In the verification example, the tensile strength and modulus of the polypropylene-based composite material prepared by the wind turbine blade powder modified by KH550 reach 43.27MPa and 1148.64MPa, respectively, which are 37.1% and 147.3% higher than those of pure PP, respectively.

[0072] In this article, the step (3) dilutes the amino-containing silane coupling agent to a coupling agent solution with a mass concentration of 1 to 3 wt%, wherein the dilution and the solvent used for dilution are selected by conventional known methods when the silane coupling agent is used. Those skilled in the art can directly select an appropriate method according to the common knowledge in the art or according to the instructions for use of the amino-containing silane coupling agent.

[0073] In order to better illustrate the present invention and provide an implementation method for reference, the amino-containing silane coupling agent is diluted to a coupling agent solution with a mass concentration of 1 to 3 wt %, wherein the solvent used for the dilution is a mixture of ethanol and water, and the mass ratio of the two is 4:1.

[0074] In this article, step (3) is described in which the wind turbine blade powder obtained in step (2) is added to a coupling agent solution and immersed for at least 30 minutes, wherein the immersion treatment is a conventional treatment method in the art. In one embodiment, for example, the wind turbine blade powder obtained in step (2) is added to a coupling agent solution and immersed for at least 30 minutes, and the mass of the wind turbine blade powder is 40% of the mass of the coupling agent solution.

[0075] Furthermore, the reason why the present invention utilizes amino-containing silane coupling agents is that one end of their molecular chains has organic functional groups of different structures, thus having different polarities, and their compatibility with the polypropylene matrix will also be different. Another inventive point of the present invention is that it was surprisingly found during the experiment that there was a synergistic effect between the amino-containing silane coupling agent and polypropylene grafted maleic anhydride, and through comparative experiments it was found that the combination of KH550 and polypropylene grafted maleic anhydride produced the best results, and a polypropylene-based composite material with the best mechanical properties was obtained. The synergistic mechanism between KH550 and polypropylene grafted maleic anhydride is as follows: Figure 3 As shown. First, the silanol groups formed by the hydrolysis of KH550 can react with the hydroxyl groups on the surface of the glass fiber in the wind turbine blade powder, so that the -NH2 in KH550 can be grafted onto the fiber surface. The introduction of the -NH2 functional group enhances the compatibility between the glass fiber and the polypropylene matrix. Subsequently, the anhydride groups in the polypropylene grafted maleic anhydride can react with -NH2 at high temperatures to form amide bonds. At the same time, the non-polar PP molecular chains in the polypropylene grafted maleic anhydride will be chain entangled with the PP matrix. This complex process ultimately leads to a significant increase in the interfacial strength between the glass fiber and PP.

[0076] In one of the more preferred embodiments, in order to further improve the mechanical properties of the prepared polypropylene flame retardant composite material, the amino-containing silane coupling agent in step (3) is selected as KH550, and KH550 is diluted to a coupling agent solution with a mass concentration of 2wt%, and the amount of polypropylene grafted maleic anhydride added in step (4) is 5wt% of the mixture.

[0077] Herein, the phytic acid piperazine in step (4) is a flame retardant containing nitrogen and phosphorus elements prepared by a solution synthesis method using phytic acid and piperazine, and those skilled in the art can directly prepare it according to the technical contents disclosed in the prior art literature.

[0078] Another inventive point of the present invention is that a polypropylene flame retardant composite material having both mechanical properties and excellent flame retardancy is prepared by compounding piperazine phytate with melamine polyphosphate.

[0079] In order to further enhance the synergistic flame retardant effect of the compound of phytic acid piperazine and melamine polyphosphate, in one preferred embodiment, the preparation method of phytic acid piperazine in step (4) is as follows:

[0080] Piperazine (7.75 g, 0.09 mol) is completely dissolved in 300 mL of ethanol under mechanical stirring to prepare a piperazine solution; subsequently, a phytic acid solution (PA, 39.6 g, 50 wt% aqueous solution, 0.03 mol) is dissolved in 150 mL of ethanol, and then added dropwise to the piperazine solution to react at room temperature for 12 hours; after the reaction time is reached, a white product is collected by suction filtration and washed with ethanol for 3 to 5 times to remove unreacted piperazine and phytic acid; finally, the obtained white product is dried at 80° C. for 12 hours to obtain phytic acid piperazine with a phosphorus content of 28 wt%. In the preparation method, the yield of phytic acid piperazine is about 90%.

[0081] When using the phytic acid piperazine (phosphorus content of 28wt%) prepared in the above preferred technical scheme, it was surprisingly found that its compound combination with melamine polyphosphate helps to slow down the reduction of the mechanical properties of the material at the proportion specified in the present invention. In one of the most preferred technical schemes, when the mass ratio of phytic acid piperazine to melamine polyphosphate is 2:1, and the addition amount of both is 20wt% of the mixture, the mechanical properties of the prepared polypropylene flame retardant composite material are close to those of the control group without adding flame retardant, which breaks through the conventional perception in the prior art that the addition of flame retardants will cause the deterioration of the mechanical properties of the composite material.

[0082] Herein, the polypropylene in step (4) is selected from conventional polypropylene industrial raw materials, such as at least one of conventional isotactic polypropylene, syndiotactic polypropylene, and atactic polypropylene, or a blend thereof; those skilled in the art can select a suitable polypropylene raw material according to actual product needs or process requirements.

[0083] Herein, the polypropylene grafted maleic anhydride in step (4) is a conventional industrial additive, which can be directly obtained from the market by a person skilled in the art, or prepared by the person skilled in the art according to the prior art literature in the art.

[0084] In one embodiment, the polypropylene in step (4) is 45 to 60 parts, such as 45 parts, 46 parts, 47 parts, 48 ​​parts, 49 parts, 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts or any range or point value therebetween; the polypropylene grafted maleic anhydride is 2 to 5 parts, such as 2 parts, 3 parts, 4 parts, 5 parts or any range or point value therebetween. any range or point value; the phytic acid piperazine is 5-15 parts, for example 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 parts or any range or point value therebetween; the melamine polyphosphate is 5-15 parts, for example 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 parts or any range or point value therebetween.

[0085] Herein, the uniform mixing in step (4) is a conventional process in the art, for example, uniform dispersion by mechanical stirring such as a high-speed rotary mixer.

[0086] Herein, the extrusion granulation described in step (4) is a conventional process for preparing polypropylene-based composite materials. Those skilled in the art may directly refer to the general process parameters of polypropylene materials or the methods described in the prior art literature in the field.

[0087] In order to better illustrate the present invention and provide an implementation method for reference, the specific process parameters of the extrusion granulation in step (4) are as follows: the temperatures of the extruder from the feed port to the die are set to 130°C, 175°C, 180°C, 180°C, 175°C and 170°C, respectively, and the screw speed is set to 80r / min.

[0088] The present invention will be further explained in detail with reference to the following examples. However, it should be understood by those skilled in the art that these examples are provided for illustrative purposes only and are not intended to limit the present invention.

[0089] Example

[0090] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. The specific conditions not specified in the examples are carried out according to the conditions recommended by normal conditions or manufacturers. The reagents used or the instruments not specified by the manufacturer are all conventional products that can be obtained commercially. The application should not be construed as being limited to the specific examples described.

[0091] 1. Raw materials

[0092] Abandoned wind turbine blades, provided by Dongfang Boiler Group;

[0093] Silane coupling agent (KH550, KH560, KH570, purity 98%), deionized water, anhydrous ethanol, Chengdu Kelong Chemical Co., Ltd.;

[0094] T30S isotactic polypropylene (2.6 g / 10 min), Xinjiang Dushanzi Petrochemical Co., Ltd., China;

[0095] Polypropylene grafted with maleic anhydride (grafting rate 1.2%), Dow Chemical Company;

[0096] 70% phytic acid solution (PA), Aladdin Reagents;

[0097] Anhydrous piperazine (99%, PI), MacLean Reagent Company;

[0098] Melamine polyphosphate (MPP, 99%), Chengdu Ounruisi Chemical Reagent Co., Ltd.

[0099] 2. Preparation method

[0100] (1) After pretreatment including cleaning, the waste wind turbine blade materials are crushed into wind turbine blade fragments with an average particle size of no more than 3 cm;

[0101] (2) Adding the wind turbine blade fragments obtained in step (1) into a disc-type solid phase force chemical reactor for grinding and pulverization, after the grinding is completed, collecting the wind turbine blade powder, which is recorded as WTB or WTB powder; wherein the process parameters of the disc-type solid phase force chemical reactor are: grinding pressure of 6 MPa, the temperature of the disc surface is controlled at -5°C by passing a circulating cooling liquid, cyclic grinding is performed once, and the disc speed is 100 rpm;

[0102] (3) diluting an amino-containing silane coupling agent to a coupling agent solution with a mass concentration of 2 wt%, adding the wind turbine blade powder obtained in step (2) to the coupling agent solution for immersion treatment for 30 min, and obtaining a wind turbine blade powder modified with a coupling agent after drying;

[0103] (4) The coupling agent-modified wind turbine blade powder obtained in step (3) is mixed evenly with the following raw materials according to weight percentage to form a mixed material:

[0104]

[0105] (5) preparing a polypropylene flame retardant composite material by extruding and granulating the mixture obtained in step (4);

[0106] The specific process parameters of the extrusion granulation are as follows: the temperatures of the extruder from the feed port to the die are set to 130°C, 175°C, 180°C, 180°C, 175°C and 170°C respectively, and the screw speed is set to 80r / min;

[0107] (6) For the convenience of testing, a polypropylene flame retardant composite material was prepared based on step (5), and a polypropylene flame retardant composite strip was prepared by injection molding using an injection molding machine. The temperature of the injection molding machine from the barrel to the nozzle was set to 130°C, 180°C, 180°C, 180°C and 185°C, respectively, the injection pressure was set to 60 MPa, and the injection speed was set to 40 mm / s.

[0108] The preparation method of the piperazine phytate is as follows:

[0109] Piperazine (7.75 g, 0.09 mol) is completely dissolved in 300 mL of ethanol under mechanical stirring to prepare a piperazine solution; subsequently, a phytic acid solution (PA, 39.6 g, 50 wt% aqueous solution, 0.03 mol) is dissolved in 150 mL of ethanol, and then added dropwise to the piperazine solution to react at room temperature for 12 hours; after the reaction time is reached, a white product is collected by suction filtration and washed with ethanol for 3 to 5 times to remove unreacted piperazine and phytic acid; finally, the obtained white product is dried at 80° C. for 12 hours to obtain phytic acid piperazine with a phosphorus content of 28 wt%. In the preparation method, the yield of phytic acid piperazine is about 90%.

[0110] 3. Test methods

[0111] Fourier Transform Infrared Spectroscopy (FTIR) Test

[0112] The samples were analyzed by transmission mode spectroscopy using a Nicolet 6700 Fourier transform infrared spectrometer from Thermo Fisher Scientific, USA. The scanning range of the spectrometer was 4000-400 cm -1 , resolution 4cm -1 , scan number 32 times. KBr pellet was used in transmission mode.

[0113] X-ray Photoelectron Spectroscopy (XPS) Test

[0114] The AXIS Ultra DLD X-ray photoelectron spectrometer from Kratos Analytical Instruments of the United Kingdom was used to analyze the types and composition of elements in the samples, and to record the energy spectrum data and spectra of elements such as C, N, O, P, and Si.

[0115] Raman spectroscopy analysis

[0116] The residue after cone calorimetric combustion was analyzed using a RA802 Raman spectrometer from Renishaw, UK, with a helium-neon laser wavelength of 532 nm.

[0117] Scanning electron microscopy (SEM) analysis

[0118] The surface morphology of WTB powder and the cross-sectional morphology of composite products after liquid nitrogen brittle fracture or tensile test were observed using an Inspect F scanning electron microscope from FEI, USA. Test conditions: acceleration voltage 20 kV, samples were gold-sprayed before testing. The elemental spectrum was obtained by an energy dispersive X-ray spectroscopy (EDS) elemental composition analyzer installed on the scanning electron microscope.

[0119] Polarized light microscopy (PLM)

[0120] WTB powder was observed using a DM2500P polarizing microscope from Leica, Germany, in combination with a THMS600 hot stage from Linkam, UK, and a PL-A662 camera from Pixelink, Canada.

[0121] Transmission electron microscopy (TEM) analysis

[0122] The morphology and element distribution of WTB powder were observed using a Talos FEI 200 transmission electron microscope (USA Thermo Scientific).

[0123] Thermogravimetric analysis (TGA)

[0124] The Q50 thermogravimetric analyzer from TA Instruments, USA, was used to test the mass change of the sample with temperature in a N2 atmosphere. Heating rate: 10°C / min; temperature range: room temperature-600°C.

[0125] Thermogravimetric-infrared spectroscopy test

[0126] The gas phase decomposition products of the material were tested by thermogravimetric-infrared spectroscopy. The infrared spectrometer was connected to the thermogravimetric analyzer through a gas delivery tube. 10.0 mg of the sample was weighed and placed in the thermogravimetric analyzer. In a nitrogen atmosphere, the temperature was raised at a rate of 50 °C / min to 800 °C. The resolution of the infrared analyzer was 4 cm -1 , wave number range is 4000-400cm -1 .

[0127] Differential Scanning Calorimetry (DSC) Test

[0128] The melting and crystallization behaviors of the samples were analyzed using a Q 20 differential scanning calorimeter from TA Instruments, Inc., USA. Temperature range: 40-180°C; heating and cooling rates: 10°C / min; N2 atmosphere.

[0129] The crystallinity of the sample (X c ) can be calculated using the following formula:

[0130]

[0131] Where ΔH m Indicates the melting heat of PP, ΔH* m The heat of fusion of fully crystallized PP is 209 J / g.

[0132] Dynamic Mechanical Testing (DMA)

[0133] The dynamic mechanical properties of the samples were analyzed using a Q800 dynamic rheometer from TA Instruments, USA. Test conditions: three-point bending mode, frequency 1 Hz, heating rate 3 °C / min, temperature range -40 to 160 °C.

[0134] Tensile properties test

[0135] The tensile strength and modulus of the samples were tested using a DWD-10KN microcomputer-controlled electronic universal testing machine produced by Sichuan Dexiang Kechuang Instrument Co., Ltd. The injection molded specimens were tested according to the GB / T 1449-2005 standard. The width and thickness of the solid phase tensile specimens were the average of 5 measurements. At least five different experimental results were taken for each group to calculate the average value.

[0136] Impact performance test

[0137] The room temperature impact strength of the samples was tested using the cantilever beam impact tester (GC-XJL-5D) of Guangdong Guangce Instrument Technology Co., Ltd. according to the GB / T1451-2005 standard. Before the test, the impact specimens were processed with a V-notch on the GC-QK-A fully automatic notch sample making machine of Guangdong Guangce Instrument Technology Co., Ltd., with a notch depth of 2 mm. At least 8 specimens were tested in each group, and the average value was calculated.

[0138] Bending performance test

[0139] The bending properties of the samples were tested according to the GB / T 1447-2005 standard using a DWD-10KN microcomputer-controlled electronic universal testing machine from Sichuan Dexiang Kechuang Instrument Co., Ltd. The crossbeam speed was 2 mm / min. At least 5 samples were tested in each group and the average value was calculated.

[0140] Limiting oxygen index test

[0141] The Limiting Oxygen Index (LOI) refers to the minimum oxygen concentration at which a polymer material can burn with a flame in a mixture of nitrogen and oxygen under specified conditions. This test is conducted in accordance with the ASTM D2863 standard, and the sample size is 120mm×10mm×4mm. First, all test samples are marked with a scale line 50mm away from the ignition point, and the sample is held vertically on the fixture. After the airflow in the glass cover is stable, the igniter is used to perform a combustion test from above the sample. Each group of 10 samples is continuously increased and decreased to obtain the LOI value corresponding to the flame burning to the scale line within 3 minutes.

[0142] Vertical burning test

[0143] The vertical burning test is carried out according to the GB / T5169.16-2017 standard test process. Before the test, place the absorbent cotton directly under the fixture and adjust the flame height (20±1mm). During the test, 5 samples are grouped together, and the sample size is 125.0mm×13mm×3.2mm.

[0144] Cone calorimetry testing

[0145] The combustion behavior of the samples was evaluated according to the ISO 5660-1 test standard. The cone calorimeter test sample size was 100mm×100mm×3mm and the heat flux radiation power was 25kV / m 2 .

[0146] Comparative Example 1

[0147] Comparative Example 1 was prepared according to the above-mentioned "2. Preparation method", except that the amino-containing silane coupling agent in step (3) was KH550, and no piperazine phytate and melamine polyphosphate were added in step (4), and the amount of polypropylene was 65 parts, and finally a polypropylene composite strip / sample plate was prepared, which was recorded as PP / WTB / FR-0.

[0148] Comparative Example 2

[0149] Comparative Example 2 was prepared according to the above "2. Preparation method", except that the amino-containing silane coupling agent in step (3) was KH550, no piperazine phytate was added in step (4), and the amount of melamine polyphosphate was 20 parts, and finally a polypropylene flame retardant composite strip / plate was prepared, which was recorded as PP / WTB / FR-1.

[0150] Comparative Example 3

[0151] Comparative Example 3 was prepared according to the above "2. Preparation method", except that the amino-containing silane coupling agent in step (3) was KH550, no melamine polyphosphate was added in step (4), and the amount of piperazine phytate was 20 parts, and finally a polypropylene flame retardant composite strip / plate was prepared, which was recorded as PP / WTB / FR-2.

[0152] Example 1

[0153] Example 1 is prepared according to the above "2. Preparation method", in which the amino-containing silane coupling agent in step (3) is KH550, in step (4) the amount of piperazine phytate is 6.7 parts, and the amount of melamine polyphosphate is 13.3 parts, and finally a polypropylene flame retardant composite strip / plate is prepared, which is recorded as PP / WTB / FR-3.

[0154] Example 2

[0155] Example 2 is prepared according to the above "2. Preparation method", in which the amino-containing silane coupling agent in step (3) is KH550, in step (4) the amount of piperazine phytate is 10 parts, and the amount of melamine polyphosphate is 10 parts, and finally a polypropylene flame retardant composite strip / plate is prepared, which is recorded as PP / WTB / FR-4.

[0156] Example 3

[0157] Example 3 is prepared according to the above "2. Preparation method", in which the amino-containing silane coupling agent in step (3) is KH550, in step (4) the amount of piperazine phytate is 13.3 parts, and the amount of melamine polyphosphate is 6.7 parts, and finally a polypropylene flame retardant composite strip / plate is prepared, which is recorded as PP / WTB / FR-5.

[0158] Verification Example 1

[0159] In order to verify the modification of wind turbine blade powders by silane coupling agents containing different amino groups, the preparation was carried out in Verification Example 1 with reference to steps (1) to (3) of "2. Preparation method" above, and in step (3), the amino-containing silane coupling agent was KH550, and finally, a wind turbine blade powder modified by a coupling agent was prepared, which was recorded as WTB@550.

[0160] Verification Example 2

[0161] In order to verify the modification of wind turbine blade powders by silane coupling agents containing different amino groups, the preparation was carried out in Verification Example 2 with reference to steps (1) to (3) of "2. Preparation method" above, and in step (3), the amino-containing silane coupling agent was KH560, and finally, a wind turbine blade powder modified by a coupling agent was prepared, which was recorded as WTB@560.

[0162] Verification Example 3

[0163] In order to verify the modification of wind turbine blade powders by silane coupling agents containing different amino groups, the preparation was carried out with reference to steps (1) to (3) of "2. Preparation method" mentioned above in Verification Example 3, and the amino-containing silane coupling agent in step (3) was KH570, and finally a wind turbine blade powder modified by a coupling agent was prepared, which was recorded as WTB@570.

[0164] Verification Example 4

[0165] In order to verify the synergistic effect of the amino-containing silane coupling agent and polypropylene grafted maleic anhydride, the above-mentioned "2. Preparation method" was used for preparation in Verification Example 4, but the amino-containing silane coupling agent was not used to modify the wind turbine blade powder. In step (4), the wind turbine blade powder obtained in step (2) was uniformly mixed with the following raw materials according to parts by weight to form a mixture:

[0166] 50 parts of wind turbine blade powder,

[0167] Polypropylene 45 parts,

[0168] Polypropylene grafted with maleic anhydride 5 parts;

[0169] Finally, polypropylene composite strips were prepared and recorded as PP / WTB-50 / MAH.

[0170] Verification Example 5

[0171] In order to verify the synergistic effect of the amino-containing silane coupling agent and polypropylene grafted maleic anhydride, the preparation was carried out in Verification Example 5 with reference to the above "2. Preparation method", and in step (3), the amino-containing silane coupling agent was KH550. In step (4), the wind turbine blade powder modified with the coupling agent obtained in step (3) was uniformly mixed with the following raw materials in parts by weight to form a mixture:

[0172] 50 parts of wind turbine blade powder modified with coupling agent,

[0173] Polypropylene 45 parts,

[0174] Polypropylene grafted with maleic anhydride 5 parts;

[0175] Finally, a polypropylene composite strip was prepared and recorded as PP / WTB@550-50.

[0176] Verification Example 6

[0177] In order to verify the synergistic effect of the amino-containing silane coupling agent and polypropylene grafted maleic anhydride, the preparation was carried out in Verification Example 6 with reference to the above "2. Preparation method", and in step (3), the amino-containing silane coupling agent was KH560. In step (4), the wind turbine blade powder modified with the coupling agent obtained in step (3) was uniformly mixed with the following raw materials according to parts by weight to form a mixture:

[0178] 50 parts of wind turbine blade powder modified with coupling agent,

[0179] Polypropylene 45 parts,

[0180] Polypropylene grafted with maleic anhydride 5 parts;

[0181] Finally, polypropylene composite strips were prepared and recorded as PP / WTB@560-50.

[0182] Verification Example 7

[0183] In order to verify the synergistic effect of the amino-containing silane coupling agent and polypropylene grafted maleic anhydride, the preparation was carried out in Verification Example 7 with reference to the above "2. Preparation method", and in step (3), the amino-containing silane coupling agent was KH570. In step (4), the wind turbine blade powder modified with the coupling agent obtained in step (3) was uniformly mixed with the following raw materials according to parts by weight to form a mixture:

[0184] 50 parts of wind turbine blade powder modified with coupling agent,

[0185] Polypropylene 45 parts,

[0186] Polypropylene grafted with maleic anhydride 5 parts;

[0187] Finally, polypropylene composite strips were prepared and recorded as PP / WTB@570-50.

[0188] Verification Example 8

[0189] In order to verify the synergistic effect of the amino-containing silane coupling agent and polypropylene grafted maleic anhydride, the above-mentioned "2. Preparation method" was used for preparation in Verification Example 8, but the amino-containing silane coupling agent was not used to modify the wind turbine blade powder. In step (4), the wind turbine blade powder obtained in step (2) was uniformly mixed with the following raw materials in parts by weight to form a mixture:

[0190] 50 parts of wind turbine blade powder,

[0191] Polypropylene 50 parts;

[0192] Finally, a polypropylene composite strip was prepared and recorded as PP / WTB-50.

[0193] 4. Test results

[0194] In order to clarify the effect of amino-containing silane coupling agent modification on the surface chemical structure of WTB powder, the FTIR spectra and XPS spectra of different powders were tested, such as Figure 1 shown. Figure 1 (a) reveals the elemental composition of WTB powder, which mainly includes C, N, O and Si elements, indicating that the coupling agent modification did not cause changes in the elements of WTB powder. Figure 1 In the high-resolution spectrum of Si 2p orbitals in (b), the peak at 104.1 eV corresponds to silicon dioxide (SiO2) in the glass fiber, while the peak at 102.9 eV indicates that the glass fiber surface contains Si-OH groups. Figure 1As shown in (c), (e) and (f), after the coupling agent is modified, new peaks appear at 101.5eV, 102.1eV and 102.1eV. These new peaks belong to Si-O-Si bonds, indicating that the silanol groups after hydrolysis of the coupling agent react chemically with the hydroxyl groups on the surface of the glass fiber, proving that the glass fiber in the WBT powder is successfully grafted with the coupling agent molecules. FTIR infrared spectra of different WTB powders are shown in Figure 1. Figure 1 As shown in (d), the main infrared absorption peak position of WTB powder remains unchanged before and after modification, which may be due to the low content of coupling agent molecules, which has no significant effect on the infrared spectrum. -1 The absorption peak at 2962cm -1 and 2868cm -1 The absorption peaks at 2923 cm-1 and 2963 cm-2 correspond to the asymmetric and symmetric stretching vibrations of the -CH3 group. -1 and 1458cm -1 ; 1609cm -1 and 1509cm -1 The absorption peak at 830 cm-1 is attributed to the stretching vibration of the benzene ring skeleton. -1 The absorption peak at is caused by the out-of-plane bending vibration of the benzene ring.

[0195] The mechanical properties of polypropylene composite strips modified with different WTB powder contents and different coupling agents were studied. It was found that with the increase of WTB powder content, the tensile strength and modulus, flexural strength and modulus of the polypropylene composite strips increased accordingly. This is because the increase in WTB powder content also increases the glass fiber content, thereby enhancing the mechanical properties of the material.

[0196] Further research was conducted on the polypropylene composite strips with the best mechanical properties containing 50wt% WTB powder to reveal the relationship between different formulations and different coupling agent modifications and the mechanical properties of the composite materials. Figure 2 As shown. Figure 2As can be seen in (a), the tensile strength and tensile modulus of polypropylene (PP) are 31.55MPa and 464.54MPa, respectively. However, when unmodified WTB powder is added, the tensile strength drops to 22.09MPa, but due to the high modulus glass fiber in WTB powder, the tensile modulus increases to 670.93MPa. This shows that the unmodified WTB powder has poor compatibility with PP, resulting in low material interface strength and therefore no reinforcement effect. After adding polypropylene grafted maleic anhydride (PP-g-MAH), the tensile strength and modulus of the polypropylene composite spline increased to 37.07MPa and 960.15MPa, respectively, an increase of 17.5% and 106.7%, respectively. In addition, the use of different coupling agents to modify WTB powder can further improve the tensile strength and modulus. In particular, after KH550 modification, the tensile strength and modulus of the material reached 43.27MPa and 1148.64MPa, respectively, which were increased by 37.1% and 147.3% compared with pure PP.

[0197] Figure 2 (b) shows the change trend of bending strength close to the change of tensile strength. Without modification, the bending strength of the spline is only 43.09MPa, which is only 5.3% higher than PP (40.91MPa). When PP-g-MAH is used alone, the bending strength reaches 56.16MPa, an increase of 37.3%. After further modification with KH550, the bending strength reaches 67.02MPa, an increase of 63.8%, which is the largest increase compared with the values ​​after KH560 modification (62.17MPa) and KH570 modification (59.57MPa). In terms of bending modulus, due to the presence of a large amount of glass fiber, all different samples with 50wt% WTB powder content have been significantly improved. After modification with KH550, KH560 and KH570, the bending modulus of the splines are 3234.33MPa, 3258.67MPa and 3424.67MPa, respectively. This is a slight deviation from the trend observed for the flexural strength and may be due to slight differences in the crystalline structure of the PP matrix.

[0198] The test results of notched impact strength are as follows Figure 2 (c) As shown. From a macroscopic point of view, the notched impact strength of the spline decreases with the addition of WTB powder. Compared with the commercially available short glass fibers of several centimeters in length, the glass fiber size in WTB powder is relatively small, which limits its ability to enhance toughness. However, it can be found that the use of coupling agents to enhance the interfacial strength of polypropylene composite splines is effective. The notched impact strength of the spline modified with KH550 is 2.960 kJ / m 2 , compared with PP's 3.625 kJ / m 2 Compared with the previous test, the KH560 (2.540 kJ / m2 ) and KH570 (2.270 kJ / m 2 ) after the notched impact strength is also higher than that without any modification (2.130 kJ / m 2 ) or only PP-g-MAH (2.190 kJ / m 2 ) samples have been improved. Figure 2 (d) The mechanical properties of different samples were comprehensively compared, and it can be concluded that the composite modified with KH550 and added with PP-g-MAH has the best mechanical properties.

[0199] like Figure 3 As shown in the figure, the reason for selecting KH550, KH560 and KH570 is that they have organic functional groups with different structures at one end of their molecular chains, thus having different polarities, and their compatibility with the PP matrix will also be different. The final results show that the combination of KH550 and PP-g-MAH produced the best results, and the polypropylene composite strips with the best mechanical properties were obtained. The synergistic mechanism between KH550 and PP-g-MAH is shown in the figure. Figure 3 As shown. First, the silanol groups formed by the hydrolysis of KH550 can react with the hydroxyl groups on the surface of the glass fiber in the WTB powder, so that the -NH2 in KH550 can be grafted onto the fiber surface. The introduction of the -NH2 functional group enhances the compatibility between the glass fiber and the PP matrix. Subsequently, the anhydride groups in PP-g-MAH can react with -NH2 at high temperatures to form amide bonds. At the same time, the non-polar PP molecular chains in PP-g-MAH will be entangled with the PP matrix. This complex process ultimately leads to a significant increase in the interfacial strength between the glass fiber and PP.

[0200] Piperazine phytate (PAPI) contains less nitrogen, so it is compounded with melamine polyphosphate (MPP) with a high nitrogen content to prepare polypropylene flame retardant composite strips. First, the effect of adding flame retardants on the mechanical properties of the material was studied. The tensile and bending properties test results of different polypropylene flame retardant composite strips are shown in Figure 2. Figure 4 As shown. Figure 4As can be seen in (a), when MPP and PAPI are used alone, the tensile strength of the splines is low, which is more than 30% lower than that of PP / WTB / FR-0 without flame retardant (tensile strength and tensile modulus are 38.3MPa and 707.6MPa, respectively), but the tensile modulus has increased by about 35%. This may be because the addition of MPP and PAPI makes it easier to form defects inside the material, resulting in a decrease in tensile strength, but its addition can also play a certain role in limiting the molecular chain segments, so the modulus has increased. It can be further seen that in the PAPI and MPP compound system, as the mass ratio of PAPI to MPP increases, the tensile strength and modulus of the splines also increase, and the strength of the splines compounded with all flame retardants is higher than that of the single use, indicating that the compounding of PAPI and MPP is conducive to slowing down the decline in material strength, and the higher the PAPI content, the smaller the decline in strength. Figure 4 (b) shows the bending properties of polypropylene flame retardant composite strips. Similar to the changes in tensile properties, PP / WTB / FR-5, which has the highest proportion of PAPI in the compound system, has the best bending strength, which is equivalent to PP / WTB / FR-0 (52.7MPa), and the bending modulus is increased by about 56%.

[0201] The thermal stability of polypropylene flame retardant composite strips was further studied. Figure 5 As shown. It can be seen that their thermal degradation processes are similar and are mainly divided into two stages. The first stage is between 300-430℃, corresponding to the breakage of the epoxy resin molecular chain in the WTB powder, the dehydration of PAPI, and the decomposition of MPP into melamine and ammonia. The second decomposition stage is between 430-500℃, mainly for the decomposition of polyphosphoric acid, metaphosphoric acid and melamine produced in the previous stage, as well as the decomposition of the PP matrix. Due to the addition of flame retardants, the thermal stability of the composite material is better than that without addition (T 5% =355.9℃), which is mainly due to the relatively low thermal decomposition temperature of PAPI and MPP. However, for flame retardant materials, the flame retardant decomposes before the matrix resin, which can first play a role in protecting the matrix resin and improve its thermal stability. As shown in Table 1, compared with PP / WTB / FR-0 (T P =450.5℃), after adding flame retardant, the maximum thermal decomposition temperature of the material is significantly increased. In addition, when the mass ratio of PAPI to MPP is 2, the amount of residual carbon after thermal decomposition of the material is the largest, which may be because at this ratio, the ratio of N and P elements in PAPI and MPP is more conducive to the generation of (PNO) X Carbon-like layer.

[0202] Table 1 Thermal parameters of different samples in TG curves

[0203]

[0204] The vertical combustion and limiting oxygen index (LOI) tests are effective ways to evaluate the flame retardant properties of materials, and can intuitively judge the quality of their flame retardant properties. The vertical combustion test results are widely evaluated using the UL-94 standard. In order to study the effects of the compounding of PAPI and MPP and the different mass ratios of the two on the flame retardant properties of the material, the vertical combustion and limiting oxygen index test results of polypropylene flame retardant composite strips are shown in Table 2.

[0205] First of all, it can be seen that the LOI of PP / WTB / FR-0 without adding flame retardant is only 19.2%, which does not reach any flame retardant level of UL-94, cannot self-extinguish, and the flame will burn to the top of the sample when burning, with molten droplets. When the flame retardant is added, the LOI value of the material is significantly improved, and the flame retardant level also changes accordingly. Comparing PP / WTB / FR-1 and PP / WTB / FR-2, it is found that under the same addition amount, PAPI alone has a better flame retardant effect than MPP alone. The material using 20wt% PAPI alone can reach the UL-94V-2 flame retardant level, while the material using MPP alone has no flame retardant level, but both still have molten droplets when burning. In the case of PAPI and MPP compounding, with the increase of PAPI ratio, the flame retardant performance of polypropylene flame retardant composite strips is also improved. When PAPI:MPP=2:1, the flame retardant level of the material reaches V-0 level, there is no molten drop phenomenon, and the LOI reaches 37.6%. This shows that PAPI and MPP, when used in a certain ratio, can achieve better flame retardant effect than when used alone.

[0206] Table 2 Vertical combustion (UL-94) and LOI test results of polypropylene flame retardant composite strips

[0207]

[0208] Figure 6 The figure shows the burning state of the polypropylene flame retardant composite sample at the same time after 10s of ignition during the vertical combustion test. Figure 6(a), (b), (c), (d) and (e) show that when MPP is used alone, the sample has burned to the top after 30 seconds of burning, and there is no tendency to extinguish; when PAPI is used alone, the sample has self-extinguished; when PAPI:MPP=1:2, the sample has burned more than half, and there is no tendency to self-extinguish; increasing the PAPI content to make PAPI:MPP=1:1, the sample has only a small flame at 30 seconds, and the degree of combustion is low. When PAPI:MPP=2:1, the sample is extinguished, and the flame is extinguished 2 seconds after the second ignition. The above results show that PAPI has a better flame retardant effect than MPP because it has a higher content of phosphorus, which promotes the formation of the carbon layer; the mass ratio of PAPI to MPP has an important influence on the flame retardant effect. When the mass ratio is 2, the flame retardant effect is the best and the flame retardant efficiency is the highest.

[0209] The combustion process of polypropylene flame retardant composite samples was systematically studied using cone calorimetry. First, the differences in the combustion process when PAPI and MPP were compounded and used alone were studied. Figure 7 (a) and (b) show the changes in heat release rate (HRR) and total heat release (THR) of different polypropylene flame retardant composite samples. It can be seen that the HRR peak (PHRR) of PP / WTB / FR-0 is as high as 767.98kW / m 2 The flame went out about 300 seconds after ignition, and the THR was 90.96 MJ / m 2 The amount of residual carbon after combustion is 18.34%, which is similar to the glass fiber content in 30wt% WTB powder, indicating that there is almost no carbon layer. In contrast, adding 20wt% MPP to PP / WTB / FR-1 can reduce the PHRR by about 467kW / m 2 , the carbon residue increased to 25.2%, and THR decreased to 79.44MJ / m 2 This is because the inert gas released when MPP decomposes dilutes the combustible gas and oxygen. PP / WTB / FR-2 with 20wt% PAPI added also achieved a similar effect, with PHRR reduced by 52.1%, THR reduced by 15.3%, and residual carbon increased by 61.1%. Phosphoric acid, metaphosphoric acid and other substances generated by the decomposition of PAPI have dehydration ability, which promotes the carbonization of the PP matrix to form a carbon layer, isolating the oxygen and heat required for combustion. The PHRR of PP / WTB / FR-5 with V-0 flame retardant grade is further reduced to only 241.62kW / m 2 , the reduction was up to 67.9%, and the residual carbon content reached 39.31%, which was due to the condensed phase and gas phase flame retardant effect when PAPI and MPP were used together.

[0210] The changes of HRR during the combustion process were further analyzed to reveal the combustion characteristics of the materials. Since PP / WTB / FR-0 does not contain flame retardants, the combustibles in it burn rapidly after ignition, causing the HRR to reach a peak within tens of seconds. Subsequently, due to the reduction of combustibles, the HRR began to decline and gradually tended to remain unchanged, at which time the combustion ended. However, after the start of combustion, the HRR of PP / WTB / FR-2 and PP / WTB / FR-1, to which PAPI and MPP were added, increased rapidly to a peak value. Subsequently, due to the inhibitory effect of the flame retardant on the combustion process, the HRR kept declining slowly until the end of combustion. The entire combustion time was relatively longer than that of PP / WTB / FR-0. In addition, the HRR of PP / WTB / FR-2 had an HRR peak at about 100s, and the subsequent HRR was lower than that of PP / WTB / FR-1, which may be caused by the protective carbon layer generated by the decomposition of PAPI. The phosphorus-containing decomposition products in PAPI can promote the formation of a carbon layer in the composite material. In addition, the mechanism of phosphorus free radicals capturing gas-phase free radicals and terminating the chain reaction also has a gas-phase flame retardant effect. PP / WTB / FR-5 shows a similar combustion process to PP / WTB / FR-2, and the HRR of the entire combustion process is lower and the combustion time is longer, about 523s. The compounding of PAPI and MPP greatly increases the proportion of phosphorus-containing and nitrogen-containing compounds in the combustion system, and at the same time improves the condensed phase flame retardant and gas phase flame retardant capabilities of the material, so it has higher flame retardant efficiency at the same addition amount.

[0211] The CO yield is not only important for fire hazard assessment, but also provides objective evidence of flame retardant properties to a certain extent. CO is mainly produced by the decomposition of hydrocarbon structure materials. It disappears due to oxidation to CO2 during the combustion process. The significant increase in its yield reflects the inhibitory effect of the flame retardant on the combustion process, and a relative decrease means that the inhibitory effect is weak. From Table 3, it can be seen that PP / WTB / FR-0 without adding flame retardant has the lowest Av-COY value, while the Av-COY values ​​of the three materials with added flame retardants are relatively high, indicating that they all have a strong ability to inhibit combustion. Further comparison shows that the Av-COY value of PP / WTB / FR-5 is higher than that of PP / WTB / FR-1, which shows that the addition of PAPI and MPP can significantly improve the flame retardant properties of the material. However, the Av-COY value of PP / WTB / FR-5 is slightly smaller than that of PP / WTB / FR-2. This slight antagonistic effect may be caused by changes in ventilation conditions during combustion.

[0212] FGI is an important parameter for evaluating the fire resistance of materials under actual fire conditions. It is the ratio of PHRR to the burning time (t PHRR). The larger the FGI, the shorter the time required for the material to reach the maximum heat release rate, that is, the faster the fire spreads and the greater the harm. Conversely, the slower the spread, the smaller the potential harm. It can be seen that compared with PP / WTB / FR-0, the FGI of PP / WTB / FR-1, PP / WTB / FR-2 and PP / WTB / FR-5 have all decreased significantly, among which PP / WTB / FR-5 has the smallest FGI value (2.01), indicating that it has the best fire resistance.

[0213] Table 3 Cone calorimeter data of polypropylene flame retardant composite samples

[0214]

[0215] In order to further reveal the flame retardant mechanism of polypropylene flame retardant composite samples, the morphology and structure of the residual carbon after combustion were studied.

[0216] The continuous and dense carbon layer plays an important role in improving the flame retardant properties of the material. The carbon layer formed in the short time when the flame contacts the material effectively cuts off the contact between the flame and the combustibles inside the material, slowing down the burning speed and preventing the further expansion of the fire. At the same time, the carbon layer has excellent thermal insulation, which can reduce the heat conducted from the fire source to the inside of the material, further delaying the combustion process. In addition, the carbon layer also has the function of absorbing harmful gases and smoke produced by combustion, reducing the harm of combustion to the environment and human body. Therefore, the quality of residual carbon has become an important indicator to measure the quality of the flame retardant properties of materials. Figure 8 The figure shows the carbon residue morphology of four polypropylene flame retardant composite samples after cone calorimetry testing. Figure 8 As shown in (a), the residue of PP / WTB / FR-0 after cone calorimetry test is mostly white, which is presumed to be mainly undecomposed glass fiber and a small amount of residual material that is not fully burned. The residue is loose in structure, similar to a flat powder, and is in an amorphous state. This shows that when no flame retardant is added, most of the combustibles in the material are completely burned and no carbon layer can be formed. After adding MPP, Figure 8 As shown in (b), the surface of PP / WTB / FR-1 after combustion is generally black, with many expanded bubble structures of different sizes, and the structure is relatively compact and stable. MPP contains a certain amount of phosphorus, which helps to form a carbon layer during combustion, and a large amount of nitrogen generates inert gases during the combustion process, which causes the carbon layer to expand. Therefore, the surface of PP / WTB / FR-1 shows many raised bubbles. The expanded carbon layer has a larger specific surface area, which helps to isolate more heat and oxygen and improve the condensed phase flame retardancy. In contrast, when PAPI is added alone, Figure 8As shown in (c), PP / WTB / FR-2 presents a darker black color after combustion, with a relatively smooth surface and only a small amount of expanded carbon layer, which indicates that PAPI has an excellent carbon-forming effect. The large amount of phosphorus it contains promotes the carbonization of the matrix during combustion and hinders the combustion process. However, due to the low nitrogen content, the expansion of the carbon layer is not obvious. Figure 8 (d) When PAPI:MPP=2:1, the residual carbon morphology of the material can be clearly observed. Compared with PP / WTB / FR-1 and PP / WTB / FR-2, PP / WTB / FR-5 has a larger expanded carbon layer, and the carbon layer is dense and complete, indicating that the combination of PAPI and MPP can significantly promote the formation of high-quality carbon layer, so that the material can achieve more excellent flame retardant properties.

[0217] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a flame-retardant polypropylene composite material reinforced with waste wind turbine blade materials, characterized in that The main steps include: (1) After pretreatment including cleaning, the waste wind turbine blade materials are crushed into wind turbine blade fragments with an average particle size of no more than 3 cm; (2) adding the wind turbine blade fragments obtained in step (1) into a disc-type solid phase force chemical reactor for grinding and pulverization, and collecting the wind turbine blade powder after the grinding is completed; wherein the process parameters of the disc-type solid phase force chemical reactor are: grinding pressure of 4 to 6 MPa, the temperature of the disc surface is controlled at -8 to -4°C by passing a circulating cooling liquid, the grinding is repeated 1 to 3 times, and the disc speed is 80 to 100 rpm; (3) diluting an amino-containing silane coupling agent to a coupling agent solution with a mass concentration of 1 to 3 wt%, adding the wind turbine blade powder obtained in step (2) to the coupling agent solution for immersion treatment for at least 30 min, and obtaining a wind turbine blade powder modified with the coupling agent after drying; (4) The coupling agent-modified wind turbine blade powder obtained in step (3) is mixed evenly with the following raw materials according to weight percentage to form a mixed material: (5) Extruding and granulating the mixture obtained in step (4) to obtain a polypropylene flame retardant composite material.

2. The preparation method according to claim 1, characterized in that: The amino-containing silane coupling agent in step (3) includes any one or more of KH550, KH560, and KH570.

3. The preparation method according to claim 1, characterized in that: In step (3), the amino-containing silane coupling agent is diluted to a coupling agent solution with a mass concentration of 1 to 3 wt %, wherein the solvent used for the dilution is a mixture of ethanol and water, and the mass ratio of the two is 4:

1.

4. The preparation method according to claim 1, characterized in that: In step (3), the wind turbine blade powder obtained in step (2) is added to the coupling agent solution and immersed for at least 30 minutes, and the mass of the wind turbine blade powder is not more than 40% of the mass of the coupling agent solution.

5. The preparation method according to claim 1, characterized in that: In step (3), the amino-containing silane coupling agent is KH550, and KH550 is diluted to a coupling agent solution with a mass concentration of 2 wt%. In step (4), the amount of polypropylene grafted maleic anhydride added is 5 wt% of the mixture.

6. The preparation method according to claim 1, characterized in that: The mass ratio of phytic acid piperazine to melamine polyphosphate in step (4) is 2:1, and the addition amount of both is 20wt% of the mixture.

7. The preparation method according to claim 1, characterized in that: The preparation method of phytic acid piperazine described in step (4) is specifically as follows: 7.75g of piperazine is completely dissolved in 300mL of ethanol under mechanical stirring to prepare a piperazine solution; subsequently, 39.6g of a 50wt% phytic acid solution is dissolved in 150mL of ethanol, and then added dropwise to the piperazine solution, and reacted at room temperature for 12 hours; after the reaction time is reached, a white product is collected by suction filtration, and washed with ethanol for 3 to 5 times to remove unreacted piperazine and phytic acid; finally, the obtained white product is dried at 80°C for 12 hours to obtain phytic acid piperazine with a phosphorus content of 28wt%.

8. The polypropylene flame retardant composite material prepared by the method for preparing the polypropylene flame retardant composite material reinforced with waste wind turbine blade materials as claimed in claim 1.

9. A polypropylene flame retardant recycled product made of waste wind turbine blade materials, prepared by conventional thermoplastic processing based on the polypropylene flame retardant composite material according to claim 8.

10. A method for preparing a polypropylene composite material reinforced with waste wind turbine blade materials, characterized in that The main steps include: (1) After pretreatment including cleaning, the waste wind turbine blade materials are crushed into wind turbine blade fragments with an average particle size of no more than 3 cm; (2) adding the wind turbine blade fragments obtained in step (1) into a disc-type solid phase force chemical reactor for grinding and pulverization, and collecting the wind turbine blade powder after the grinding is completed; wherein the process parameters of the disc-type solid phase force chemical reactor are: grinding pressure of 4 to 6 MPa, the temperature of the disc surface is controlled at -8 to -4°C by passing a circulating cooling liquid, the grinding is repeated 1 to 3 times, and the disc speed is 80 to 100 rpm; (3) diluting an amino-containing silane coupling agent to a coupling agent solution with a mass concentration of 1 to 3 wt%, adding the wind turbine blade powder obtained in step (2) to the coupling agent solution for immersion treatment for at least 30 min, and obtaining a wind turbine blade powder modified with the coupling agent after drying; (4) The coupling agent-modified wind turbine blade powder obtained in step (3) is mixed evenly with the following raw materials according to weight percentage to form a mixed material: 50 parts of wind turbine blade powder modified with coupling agent, Polypropylene 45 parts, Polypropylene grafted with maleic anhydride 5 parts; (5) The mixed material obtained in step (4) is subjected to extrusion granulation to prepare a polypropylene composite material.

Citation Information

Cited By

  • Halogen-free flame-retardant packing belt and preparation method thereof

    CN119859347A

  • Regenerated board highly filled with modified waste wind power blade powder and preparation method of regenerated board

    CN120271783A

  • A recycled board made of highly filled modified waste wind turbine blade powder and its preparation method

    CN120271783B

  • PP (polypropylene) hollow plate capable of comprehensively utilizing solid wastes and preparation method of PP hollow plate

    CN120310130A

  • High-strength flame-retardant PP composite material and preparation method thereof

    CN120590801A