High-heat-fading-resistance metal-free resin-based brake material prepared from andalusite powder
By using metal-free resin-based braking materials prepared by using rosystone powder and other materials, the problem of poor thermal decay resistance of copper-free materials is solved, high friction coefficient and thermal decay resistance are achieved, environmental pollution is reduced, and It has economic benefits.
Patent Information
- Application Number
- CN202411118566.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Existing copper-free brake materials have poor thermal decay resistance during high-temperature friction and contain heavy metal components that are harmful to the environment, making it difficult to achieve true metallization and high thermal decay resistance.
Using rosylic powder as functional filler, combined with cashew shell oil-modified phenolic resin, bamboo fiber, alumina, barite and graphite, high heat-resistance-resistant metal-decaying resin is prepared through drying, uniform mixing, hot pressing molding and heat treatment steps. Base brake material, replaces copper powder to improve friction wear and resistance to heat fading.
It realizes the high friction coefficient and heat fading resistance of copper-free brake materials, reduces environmental pollution, has excellent friction coefficient stability, wear resistance and low cost characteristics, and solves the problem of poor high-temperature performance of copper-free materials.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the field of brake materials, and in particular relates to a metal-free, environment-friendly resin-based brake material with high heat-fading resistance prepared by using andalusite powder. Background Art
[0002] With the development of the automobile industry and the increasingly accelerated pace of human life, the speed of vehicles is constantly increasing. The braking system, as an important part of driving safety and comfort, has also attracted much attention. Braking composite materials are composed of binders, reinforcing fibers, friction performance regulators and fillers, and are brake actuators in the braking system. In recent years, people have found that the wear debris generated by friction materials during braking contains heavy metal components, such as zinc powder, copper powder, etc. The wear debris will be suspended in the atmosphere for a long time in the form of aerosol particles. This inhalable particulate matter will be deposited in people's lungs through the respiratory system and cause great harm to the body; in addition, the heavy metal components contained in the wear debris will cause varying degrees of pollution to the atmosphere and rivers. However, copper has excellent thermal conductivity and ductility, which is conducive to improving the heat decay resistance and friction and wear performance of friction materials. In the process of high-temperature friction, copper can also play a role of solid lubrication. Therefore, the high heat decay resistance and less or no metallization of brake friction materials have become the focus of research on new brake friction materials in recent years.
[0003] The patent "A method for preparing a semi-metallic brake pad" (ZL 201610672710.8) uses natural zeolite as raw material, which is soaked and frozen in a quaternary ammonium salt solution, ground and calcined, and then immediately immersed in a calcium bicarbonate solution to deposit a layer of calcium carbonate to prepare a copper-free semi-metallic brake material with a stable friction coefficient (0.31-0.33); the patent "Copper-free friction material and its preparation method" (ZL 201410317332.2) uses a combination of carbon fiber and zinc powder to replace the copper in the formula to obtain a copper-free brake material with stable braking performance; the patent "A new fiber copper-free composition for automobile brake pads, its application and its preparation method" (ZL 201710610855.X) uses a single layer of heat-modified synthetic aluminum fiber to replace copper powder, quickly conduct the friction heat during braking, and reduce the occurrence of thermal decay. However, the high-temperature friction coefficient and anti-fading performance of the copper-free materials obtained by the above patents are not as good as those of copper-containing brake materials. Other metal elements are also added, and the metal-free nature of the brake materials is not truly achieved. At the same time, its anti-thermal fading performance still needs to be further improved.
[0004] Andalusite is an anhydrous aluminum silicate mineral, which is between kaolin refractory containing ω (Al2O3) = 37% and bauxite refractory containing ω (Al2O3) = 80-90%, and belongs to the range of medium aluminum-containing aluminum silicate refractory. Andalusite has the properties of high-temperature volume stability, melting resistance and easy transformation into mullite, and the raw material itself does not need to be calcined. Therefore, andalusite materials have good application effects in fields with high requirements for thermal shock resistance and high-temperature strength. At the same time, compared with copper powder, andalusite powder is cheap (one ton of andalusite powder costs about 5,000 yuan, while one ton of copper powder costs about 95,000 yuan), and the use of andalusite powder instead of copper powder has significant economic benefits. At the same time, andalusite powder itself has good thermal decay resistance. Using it in brake composite materials can not only reduce the pollution of wear debris to the environment, but also improve the thermal decay resistance of brake composite materials, which is of great significance to the green and sustainable development of my country's brake material industry. Summary of the invention
[0005] The object of the present invention is to provide a metal-free resin-based brake material with high thermal decay resistance, which is prepared by using andalusite powder as a functional filler to replace copper powder.
[0006] To achieve the above object, the present invention adopts the following technical solution: A metal-free resin-based brake material with high heat-fading resistance prepared by using andalusite powder is made of the following raw materials in parts by weight: 5-25 parts of andalusite powder, 15-20 parts of cashew nut shell oil-modified phenolic resin, 5-10 parts of bamboo fiber, 20-25 parts of alumina, 12-47 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
[0007] Furthermore, the mesh size of the andalusite powder is 60-320 meshes.
[0008] The preparation of the resin-based brake material comprises the following steps: 1) Processing of bamboo fibers: Shearing the bamboo fibers to obtain bamboo fibers with a length of less than 20 mm; 2) Drying of raw materials: Dry the cashew nut shell oil-modified phenolic resin and the sheared bamboo fiber at 60-70°C for 40 minutes, dry the nitrile powder at 70-80°C for 30 minutes, and dry the andalusite powder, alumina, barite and graphite at 110-120°C for 60 minutes; 3) Even mixing: Weigh the dried raw materials according to the proportion and put them into the mixer for short-term high-frequency stirring to make the materials evenly mixed; 4) Hot pressing: placing the mixed material obtained in step 3) into a hydraulic press for hot pressing; 5) Heat treatment: The sample obtained by hot pressing is placed in an electric constant temperature forced air drying oven, heat treated at 160° C. for 12 hours, and cooled in the furnace to obtain the metal-free resin-based brake material with high heat decay resistance.
[0009] Furthermore, the total stirring time of the short-term high-frequency stirring in step 3) is 5 to 8 minutes, and the stirring time each time does not exceed 10 seconds.
[0010] Furthermore, the temperature of the hot pressing molding in step 4) is 165-170° C., the pressure is 10 MPa, the holding time is 6 min, and the exhaust is performed 2-3 times during the holding time.
[0011] The obtained resin-based brake material does not contain copper and other heavy metal components harmful to human body, and its friction coefficient at 300-350℃ is above 0.38 and is not lower than the friction coefficient at 100℃.
[0012] The beneficial effects of the present invention are: (1) Andalusite powder is an irregular hard powder whose main components are SiO2 and Al2O3. Its structure is mostly irregular, and its surface is relatively rough. It has a high hardness. Adding it to brake materials can improve the friction and wear properties of the materials. At the same time, the characteristics of andalusite powder can enhance its bonding strength with resin, which is beneficial to the preparation of materials and the improvement of thermal decay resistance.
[0013] (2) The resin-based brake material provided by the present invention does not contain copper and other heavy metal components that are harmful to the human body, and has excellent friction and wear properties, especially outstanding resistance to thermal decay, which solves the problem of poor high-temperature tribological properties of copper-free brake materials.
[0014] (3) The price of andalusite powder is relatively low. Its application in the field of brake materials has important engineering application value and significant economic benefits.
[0015] (4) The present invention uses inorganic non-metallic materials and natural plant fibers to prepare composite materials, and uses andalusite powder to replace copper, so that the obtained brake material has the characteristics of excellent friction coefficient stability, good wear resistance, high strength and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 Three-dimensional response surface model diagram of the effect of changing the content of andalusite powder and cashew nut shell liquid modified phenolic resin on the friction coefficient in the deterministic screening design experiment at different temperature stages. DETAILED DESCRIPTION
[0017] As introduced in the background technology section, copper has excellent thermal conductivity and plays an important role in the high-temperature friction performance of resin-based brake materials. Andalusite powder is mainly composed of silicon oxide and aluminum oxide, and has good thermal decay resistance. Applying it to brake composite materials can not only improve the thermal decay resistance of brake composite materials but also reduce the pollution of wear debris to the environment. Therefore, the present invention uses andalusite powder to replace copper in brake materials in order to obtain a metal-free resin-based brake material with high thermal decay resistance.
[0018] In order to study the content of andalusite powder and its interaction with resin, reinforcing fiber and alumina, the response surface methodology was used to study their effects on the friction coefficient. Thirteen experiments were designed using the deterministic screening design experiment, and the factors and their corresponding levels are shown in Table 1.
[0019] Table 1 Factors and levels of the definitive screening design
[0020] According to the 13 experimental formulas designed in the deterministic screening design test table, the corresponding brake material samples were prepared (the remaining raw materials were 12-37 wt% barite, 5 wt% nitrile powder, and 3 wt% graphite, with a total of 100 wt%), and the friction coefficient of each sample at different temperatures was tested using an X-DM variable-speed friction tester. The experimental design and results are shown in Tables 2 and 3.
[0021] Table 2 Definitive screening design test table
[0022] Table 3 Deterministic screening design experimental friction coefficient results
[0023] The quadratic polynomial regression model in the response surface methodology was used to establish the nonlinear mapping relationship between the content of andalusite powder, cashew nut shell oil-modified phenolic resin, bamboo fiber and alumina and the friction coefficient of the material, and a friction coefficient regression model was established. The quantitative model was established between each evaluation index and the method parameters using formula (1). Where b0 is a constant; b i , b ii and b ij are the regression coefficients of the linear term, quadratic term and interaction term respectively. i and X j are parameters, Y are evaluation indicators, and the stepwise regression method is used to simplify the equation.
[0024] (1) In order to study the interaction between various factors, Figure 1 Provide explanation. Figure 1The three-dimensional response surface model diagram of the effect of the content change of andalusite powder (A) and cashew nut shell oil modified phenolic resin (B) on the friction coefficient at different temperature stages. It can be seen from the three-dimensional response surface model diagrams in (a) and (b) that the model trend is steeper along the direction of andalusite powder content, while the resin direction is relatively gentle. When the andalusite powder content is close to the middle value, the friction coefficient in the low temperature stage is most suitable. It can be seen from the three-dimensional response surface model diagram in (c) that the model trend is steeper along the direction of andalusite powder content, while the resin direction is almost a horizontal transition. The interaction effect on the friction coefficient in this area is mainly reflected in the effect of andalusite powder content on the friction coefficient. It can be seen from the three-dimensional response surface model diagram in (d) that the trends along the direction of andalusite powder content and the direction of resin are similar, indicating that the friction coefficient in this area no longer changes significantly due to the change of variables. The area with a relatively gentle overall trend is concentrated in the interval close to the middle value of andalusite powder content and resin content, which is most favorable for the friction coefficient of the sample at 250℃. It can also be seen from the three-dimensional response surface model diagram in Figure (e) that the model trend is steeper along the direction of andalusite powder content, and the resin direction is relatively gentle. When the andalusite powder content is close to the middle value, the friction coefficient of the brake material at 300°C is the most suitable. It can also be seen from the three-dimensional response surface model in Figure (f) that the model trend is steeper along the direction of andalusite powder content, while the resin direction is almost a horizontal transition, indicating that the interaction of the friction coefficient in this area is mainly reflected in the andalusite powder. It can be seen that the model trend is the steepest in the two stages of too high and low andalusite content, and the model trend in the middle stage is relatively gentle. This shows that the friction coefficient at 350°C reaches its peak when the andalusite powder content is close to the middle value, and the content value at this time is the most suitable.
[0025] Overall analysis shows that the preferred contents of andalusite powder, cashew nut shell liquid-modified phenolic resin, bamboo fiber and alumina are 20%, 20%, 8% and 20%, respectively.
[0026] The regression coefficient values of the friction coefficient retrospective model established are shown in Table 4 Table 4 Regression coefficient values of friction coefficient regression model
[0027] It can be seen from Table 4 that the optimized formula has a high level of friction coefficient and has certain advantages in the stability of the friction coefficient.
[0028] The technical solution of the present invention is further described below in conjunction with specific implementations. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0029] The mesh size of the andalusite powder used is 320 mesh unless otherwise specified.
[0030] Example 1 1) Composition of raw materials (by weight) 20 parts of andalusite powder, 20 parts of cashew nut shell oil modified phenolic resin, 8 parts of bamboo fiber, 20 parts of alumina, 24 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
[0031] 2) Preparation method: The bamboo fiber was chopped to obtain bamboo fiber with a length of 10 mm; the cashew nut shell oil-modified phenolic resin and the chopped bamboo fiber were dried at 60°C for 40 min, the nitrile powder was dried at 70°C for 30 min, and the andalusite powder, alumina, barite and graphite were dried at 120°C for 60 min; the dried raw materials were mixed according to the designed formula and put into a mixer and stirred for 8 min (each stirring time did not exceed 10 s) to ensure that the materials were mixed evenly and a uniform powdery mixture was obtained; the evenly mixed mixture was put into a hydraulic press and hot-pressed at 165-170°C and a pressure of 10 MPa for 6 min, during which the exhaust was performed twice; the hot-pressed sample was put into an electric constant temperature blast drying oven, heat-treated at 160°C for 12 h, and cooled with the furnace to obtain a metal-free resin-based brake material with high heat-fading resistance.
[0032] Example 2 1) Composition of raw materials (by weight) 5 parts of andalusite powder, 20 parts of cashew nut shell oil modified phenolic resin, 8 parts of bamboo fiber, 20 parts of alumina, 39 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
[0033] 2) Preparation method: The bamboo fiber was chopped to obtain bamboo fiber with a length of 10 mm; the cashew nut shell oil-modified phenolic resin and the chopped bamboo fiber were dried at 60°C for 40 min, the nitrile powder was dried at 70°C for 30 min, and the andalusite powder, alumina, barite and graphite were dried at 120°C for 60 min; the dried raw materials were mixed according to the designed formula and put into a mixer and stirred for 8 min (each stirring time did not exceed 10 s) to ensure that the materials were mixed evenly and a uniform powdery mixture was obtained; the evenly mixed mixture was put into a hydraulic press and hot-pressed at 165-170°C and a pressure of 10 MPa for 6 min, during which the exhaust was performed twice; the hot-pressed sample was put into an electric constant temperature blast drying oven, heat-treated at 160°C for 12 h, and cooled with the furnace to obtain a metal-free resin-based brake material with high heat-fading resistance.
[0034] Example 3 1) Composition of raw materials (by weight) 10 parts of andalusite powder, 20 parts of cashew nut shell oil-modified phenolic resin, 8 parts of bamboo fiber, 20 parts of alumina, 34 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
[0035] 2) Preparation method: The bamboo fiber was chopped to obtain bamboo fiber with a length of 10 mm; the cashew nut shell oil-modified phenolic resin and the chopped bamboo fiber were dried at 60°C for 40 min, the nitrile powder was dried at 70°C for 30 min, and the andalusite powder, alumina, barite and graphite were dried at 120°C for 60 min; the dried raw materials were mixed according to the designed formula and put into a mixer and stirred for 8 min (each stirring time did not exceed 10 s) to ensure that the materials were mixed evenly and a uniform powdery mixture was obtained; the evenly mixed mixture was put into a hydraulic press and hot-pressed at 165-170°C and a pressure of 10 MPa for 6 min, during which the exhaust was performed twice; the hot-pressed sample was put into an electric constant temperature blast drying oven, heat-treated at 160°C for 12 h, and cooled with the furnace to obtain a metal-free resin-based brake material with high heat-fading resistance.
[0036] Example 4 1) Composition of raw materials (by weight) 15 parts of andalusite powder, 20 parts of cashew nut shell oil-modified phenolic resin, 8 parts of bamboo fiber, 20 parts of alumina, 29 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
[0037] 2) Preparation method: The bamboo fiber was chopped to obtain bamboo fiber with a length of 10 mm; the cashew nut shell oil-modified phenolic resin and the chopped bamboo fiber were dried at 60°C for 40 min, the nitrile powder was dried at 70°C for 30 min, and the andalusite powder, alumina, barite and graphite were dried at 120°C for 60 min; the dried raw materials were mixed according to the designed formula and put into a mixer and stirred for 8 min (each stirring time did not exceed 10 s) to ensure that the materials were mixed evenly and a uniform powdery mixture was obtained; the evenly mixed mixture was put into a hydraulic press and hot-pressed at 165-170°C and a pressure of 10 MPa for 6 min, during which the exhaust was performed twice; the hot-pressed sample was put into an electric constant temperature blast drying oven, heat-treated at 160°C for 12 h, and cooled with the furnace to obtain a metal-free resin-based brake material with high heat-fading resistance.
[0038] Example 5 1) Composition of raw materials (by weight) 25 parts of andalusite powder, 20 parts of cashew nut shell oil modified phenolic resin, 8 parts of bamboo fiber, 20 parts of alumina, 19 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
[0039] 2) Preparation method: The bamboo fiber was chopped to obtain bamboo fiber with a length of 10 mm; the cashew nut shell oil-modified phenolic resin and the chopped bamboo fiber were dried at 60°C for 40 min, the nitrile powder was dried at 70°C for 30 min, and the andalusite powder, alumina, barite and graphite were dried at 120°C for 60 min; the dried raw materials were mixed according to the designed formula and put into a mixer and stirred for 8 min (each stirring time did not exceed 10 s) to ensure that the materials were mixed evenly and a uniform powdery mixture was obtained; the evenly mixed mixture was put into a hydraulic press and hot-pressed at 165-170°C and a pressure of 10 MPa for 6 min, during which the exhaust was performed twice; the hot-pressed sample was put into an electric constant temperature blast drying oven, heat-treated at 160°C for 12 h, and cooled with the furnace to obtain a metal-free resin-based brake material with high heat-fading resistance.
[0040] Example 6 1) Composition of raw materials (by weight) 20 parts of andalusite powder (60 mesh), 20 parts of cashew nut shell oil modified phenolic resin, 8 parts of bamboo fiber, 20 parts of alumina, 24 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
[0041] 2) Preparation method: The bamboo fiber was chopped to obtain bamboo fiber with a length of 10 mm; the cashew nut shell oil-modified phenolic resin and the chopped bamboo fiber were dried at 60°C for 40 min, the nitrile powder was dried at 70°C for 30 min, and the andalusite powder, alumina, barite and graphite were dried at 120°C for 60 min; the dried raw materials were mixed according to the designed formula and put into a mixer and stirred for 8 min (each stirring time did not exceed 10 s) to ensure that the materials were mixed evenly and a uniform powdery mixture was obtained; the evenly mixed mixture was put into a hydraulic press and hot-pressed at 165-170°C and a pressure of 10 MPa for 6 min, during which the exhaust was performed twice; the hot-pressed sample was put into an electric constant temperature blast drying oven, heat-treated at 160°C for 12 h, and cooled with the furnace to obtain a metal-free resin-based brake material with high heat-fading resistance.
[0042] Example 7 1) Composition of raw materials (by weight) 20 parts of andalusite powder (200 mesh), 20 parts of cashew nut shell oil modified phenolic resin, 8 parts of bamboo fiber, 20 parts of alumina, 24 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
[0043] 2) Preparation method: The bamboo fiber was chopped to obtain bamboo fiber with a length of 10 mm; the cashew nut shell oil-modified phenolic resin and the chopped bamboo fiber were dried at 60°C for 40 min, the nitrile powder was dried at 70°C for 30 min, and the andalusite powder, alumina, barite and graphite were dried at 120°C for 60 min; the dried raw materials were mixed according to the designed formula and put into a mixer and stirred for 8 min (each stirring time did not exceed 10 s) to ensure that the materials were mixed evenly and a uniform powdery mixture was obtained; the evenly mixed mixture was put into a hydraulic press and hot-pressed at 165-170°C and a pressure of 10 MPa for 6 min, during which the exhaust was performed twice; the hot-pressed sample was put into an electric constant temperature blast drying oven, heat-treated at 160°C for 12 h, and cooled with the furnace to obtain a metal-free resin-based brake material with high heat-fading resistance.
[0044] Comparative Example 1) Composition of raw materials (by weight) 25 parts of copper powder, 20 parts of cashew nut shell oil modified phenolic resin, 8 parts of bamboo fiber, 20 parts of aluminum oxide, 19 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
[0045] 2) Preparation method: The bamboo fiber was chopped to obtain bamboo fiber with a length of 10 mm; the cashew nut shell oil-modified phenolic resin and the chopped bamboo fiber were dried at 60°C for 40 min, the nitrile powder was dried at 70°C for 30 min, and the andalusite powder, alumina, barite and graphite were dried at 120°C for 60 min; the dried raw materials were mixed according to the designed formula and put into a mixer and stirred for 8 min (each stirring time did not exceed 10 s) to ensure that the materials were mixed evenly and a uniform powdery mixture was obtained; the evenly mixed mixture was put into a hydraulic press and hot-pressed at 165-170°C and a pressure of 10 MPa for 6 min, during which the exhaust was performed twice; the hot-pressed sample was put into an electric constant temperature blast drying oven, heat-treated at 160°C for 12 h, and cooled with the furnace to obtain a copper-containing resin-based brake material.
[0046] The brake material samples prepared in Examples 1-7 and the comparative example were tested for friction and wear performance on an X-DM type pressure-regulated variable speed friction testing machine. According to the requirements for the fourth type of disc brake linings in the national standard for disc brake linings (GB5763-2008), the friction coefficient and wear rate of the discs at 5000 revolutions at disc temperatures of 100°C, 150°C, 200°C, 250°C, 300°C and 350°C were measured during the heating process. The results are shown in Tables 5 and 6 respectively.
[0047] Table 5 Friction coefficient test results of different samples
[0048] Table 6 Wear rate test results of different samples
[0049] According to the test results of friction coefficient and wear rate in Tables 5 and 6, it can be found that the friction coefficient and wear rate of the brake materials prepared in the examples are within the allowable value range of the national standard, among which the effect of Example 1 is the best. At the same time, compared with the copper-containing resin-based brake material prepared in the comparative example, the brake material prepared in the example using andalusite powder instead of copper has a significantly high thermal decay resistance, which proves that the method of the present invention can solve the problem of copper-free and high thermal decay resistance of brake materials, and is of great significance to the green and sustainable development of my country's brake material industry.
[0050] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A metal-free resin-based brake material with high thermal decay resistance prepared by using andalusite powder, characterized in that: The resin-based brake material is made of the following raw materials in parts by weight: 5-25 parts of andalusite powder, 15-20 parts of cashew nut shell oil-modified phenolic resin, 5-10 parts of bamboo fiber, 20-25 parts of alumina, 12-47 parts of barite, 5 parts of nitrile powder, and 3 parts of graphite.
2. The metal-free resin-based brake material with high thermal decay resistance prepared by using andalusite powder according to claim 1, characterized in that: The mesh number of the andalusite powder is 60-320 meshes.
3. The metal-free resin-based brake material with high thermal decay resistance prepared by using andalusite powder according to claim 1, characterized in that: The preparation of the resin-based brake material comprises the following steps: 1) Processing of bamboo fibers: Shearing the bamboo fibers to obtain bamboo fibers with a length of less than 20 mm; 2) Drying of raw materials: Dry the cashew nut shell oil-modified phenolic resin and the sheared bamboo fiber at 60-70°C for 40 minutes, dry the nitrile powder at 70-80°C for 30 minutes, and dry the andalusite powder, alumina, barite and graphite at 110-120°C for 60 minutes; 3) Even mixing: Weigh the dried raw materials in proportion and stir them for a short time at a high frequency to make the materials evenly mixed; 4) Hot pressing: hot pressing the mixed material obtained in step 3); 5) Heat treatment: The sample obtained by hot pressing is heat treated at 160° C. for 12 hours and cooled in the furnace to obtain the metal-free resin-based brake material with high heat-fading resistance.
4. The metal-free resin-based brake material with high thermal decay resistance prepared by using andalusite powder according to claim 3, characterized in that: The total stirring time of the short-term high-frequency stirring in step 3) is 5 to 8 minutes, and the stirring time each time does not exceed 10 seconds.
5. The metal-free resin-based brake material with high thermal decay resistance prepared by using andalusite powder according to claim 3, characterized in that: The temperature of the hot pressing molding in step 4) is 165-170°C, the pressure is 10 MPa, the holding time is 6 minutes, and the exhaust is performed 2-3 times during the holding time.
6. The metal-free resin-based brake material with high thermal decay resistance prepared by using andalusite powder according to claim 1, characterized in that: The friction coefficient of the resin-based brake material at 300-350°C is above 0.38 and is not lower than the friction coefficient at 100°C.
Citation Information
Patent Citations
Friction material for brakes
CN103906942A
Copper-free friction material and preparation method thereof
CN114135609A
Copper-free resin-based brake material and preparation method thereof
CN118165463A
Sintered metallic friction material for brake