Antistatic bulk molding compound composite material and preparation method thereof
By subjecting glass fiber to low-temperature plasma treatment and chemical modification, combined with carbon black filler, the problems of brittleness and insufficient antistatic properties of bulk molding compounds were solved, and the overall performance of the material was improved.
Patent Information
- Application Number
- CN202411196393.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-29
AI Technical Summary
Existing bulk molding compounds with epoxy resin as the matrix suffer from high brittleness and poor mechanical properties, and fail to effectively improve antistatic properties.
Modified glass fibers were prepared by introducing amino groups through low-temperature plasma treatment and reacting them with benzophenone 4,4-dicarboxylic acid and 1,3-bis(aminopropane)tetramethyldisiloxane. These modified glass fibers were then combined with carbon black filler to enhance their antistatic and mechanical properties.
It improves the antistatic properties, mechanical properties, and impact resistance of bulk molding compounds, reduces UV aging, and enhances the bonding strength and UV resistance of the material.
Smart Images

Figure BDA0005016526880000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bulk molding compounds, in particular to an antistatic bulk molding compound composite material and a preparation method thereof. Background Art
[0002] Bulk molding compound is a composite material obtained by uniformly mixing resin material and reinforcing fiber material. It has the advantages of fast molding speed and high production efficiency. The current mainstream bulk molding compound generally uses polyester resin material as the resin matrix, but the mechanical properties of polyester resin are poor, while epoxy resin has excellent mechanical properties. Therefore, a bulk molding compound system with epoxy resin as the resin matrix has also appeared. However, epoxy resin is relatively brittle and still faces great restrictions during use. Summary of the invention
[0003] The object of the present invention is to provide an antistatic bulk molding compound composite material and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing an antistatic bulk molding compound composite material, comprising the following steps:
[0005] S1. Preparation of modified glass fiber;
[0006] Place the glass fiber in deionized water, heat it to 75-85°C, stir and wash for 10-15 minutes, filter it, dry it with hot air at 80°C, and after constant weight, perform low-temperature plasma treatment on the glass fiber;
[0007] S12. The glass fiber treated with low-temperature plasma is dispersed in an ethanol aqueous solution with an ethanol concentration of 90-95wt%, and after stirring and dispersing for 10-15min, 5-10% KH-550 by volume of the ethanol aqueous solution is added, the temperature is raised to 75-78°C, and the reaction is refluxed and stirred for 8-12h, and the glass fiber is separated by centrifugation, and the glass fiber is washed with deionized water for 2-3 times, and then dried to constant weight to obtain a pretreated glass fiber;
[0008] S13. Disperse 4,4-dicarboxylic acid benzophenone in DMF, stir and mix for 15-25 minutes, add 1-ethyl-(3-dimethylaminopropyl)carbodiimide, continue mixing for 3-5 minutes, and then uniformly dropwise add it to 1,3-bis(aminopropyl)tetramethyldisiloxane for 1.5-2.5 hours. After the dropwise addition is completed, heat to 78-92°C, stir and react for 2-8 hours, cool to room temperature, and dropwise add the reaction mixture again. Add to 1,6-hexanediol diglycidyl ether, the dripping time is 3-5h, and the process is continuously stirred. After the dripping is completed, the temperature is raised to 75-85°C, and the reaction is stirred for 2-8h. The temperature is raised to 135°C, and the reaction is continued with stirring for 0.5-1h. The pretreated glass fiber is added, and the ultrasonic oscillation reaction is performed for 1.5-3h. The pretreated glass fiber is separated by centrifugation, and its surface is washed with clean DMF for 2-3 times, and then dried to constant weight to obtain modified glass fiber;
[0009] S2. Preparation of antistatic bulk molding compound composites;
[0010] Epoxy resin, latent curing agent, accelerator, inorganic filler, conductive filler and release agent are weighed and mixed according to weight fractions, stirred evenly, and then modified glass fiber is added. After kneading at room temperature for 20-30 minutes, the fiber is fully impregnated and kneaded evenly to obtain an antistatic bulk molding compound material.
[0011] Furthermore, the antistatic bulk molding compound composite material is formed by uniformly mixing 20-55 parts of epoxy resin, 1.5-5 parts of latent curing agent, 0.5-1.5 parts of accelerator, 15-45 parts of inorganic filler, 3-10 parts of conductive filler, 1.5-3 parts of release agent, and 20-40 parts of chopped glass fiber, by weight.
[0012] Furthermore, the epoxy resin is any one or more of bisphenol A type E-51 epoxy resin and bisphenol A type E-55 epoxy resin.
[0013] Furthermore, the latent curing agent is dicyandiamide; and the accelerator is benzyltriethylammonium chloride.
[0014] Furthermore, the inorganic filler is any one of white carbon black and calcium carbonate; the conductive filler is carbon black; and the release agent is calcium stearate.
[0015] Furthermore, in step S11, the discharge mode during the low-temperature plasma treatment is glow discharge, the reaction gas is carbon dioxide, the gas pressure is 2000-5000 Pa, the treatment power is 300-1000 W, and the treatment time is 1-15 min.
[0016] Further, in step S13, the mass ratio of the 4,4-dicarboxylic acid benzophenone, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, and 1,3-bis(aminopropyl)tetramethyldisiloxane is 1:(0.01-0.03) by weight:
[0017] (1.5-1.8).
[0018] Furthermore, in step S13, the mass ratio of the 4,4-dicarboxylic acid benzophenone, 1,6-hexanediol diglycidyl ether, and the pretreated glass fiber is 1:(1.4-1.7):(5-30) in parts by weight.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] In order to enhance the antistatic property, mechanical property and impact resistance of the bulk molding compound, the present invention first defines the inorganic reinforcing component thereof, and adds a modified glass fiber material to the bulk molding compound; the present invention first performs a low-temperature plasma treatment on the surface of the glass fiber material, and uses plasma to roughen the surface morphology of the glass fiber, and after the plasma treatment, the surface free energy of the glass fiber can be effectively improved, thereby promoting the hydrolysis and grafting of the silane coupling agent on the surface of the glass fiber in step S12, thereby introducing more amino groups on the surface of the glass fiber;
[0021] On this basis, the present invention also uses 4,4-dicarboxylic acid benzophenone as a raw material, reacts it with 1,3-bis(aminopropyl)tetramethyldisiloxane and 1,6-hexanediol diglycidyl ether, thereby preparing a product having an epoxy group as the terminal group and containing benzophenone and a silicon-oxygen bond structure, and then mixing it with a glass fiber with an amino group for reaction, thereby introducing a benzophenone group, a silicon-oxygen bond and an epoxy end-capping group on the surface of the glass fiber; wherein the introduction of the benzophenone group can bring excellent anti-ultraviolet performance to the mixed material, and benzophenone can effectively absorb ultraviolet light and It is converted into heat energy for release, which reduces the aging of epoxy resin by ultraviolet rays; at the same time, the introduction of silicon-oxygen bonds can further improve the impact resistance of the resin material at the interface between epoxy resin and glass fiber, thereby better achieving stress dispersion and reducing the defect of brittle fracture of epoxy resin. The epoxy groups introduced on the surface of glass fiber can effectively change the surface polarity of glass fiber and improve the dispersion of glass fiber in epoxy resin. Moreover, these epoxy groups can participate in the curing and cross-linking of epoxy resin under the action of latent initiators, making the bonding strength between glass fiber and epoxy resin higher.
[0022] At the same time, the addition of carbon black filler can not only enhance the conductivity of the bulk molding compound and improve its antistatic performance, but also shield and absorb ultraviolet light, thereby further enhancing the ultraviolet resistance of the bulk molding compound prepared by the present invention. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] The glass fiber used in this application has a diameter of 9-13 μm and a length of 3-50 mm; the calcium carbonate particle size used is 1200 mesh; the carbon black particle size used is 1200 mesh;
[0025] Embodiment 1. A method for preparing an antistatic bulk molding compound composite material comprises the following steps:
[0026] S1. Preparation of modified glass fiber;
[0027] The glass fiber was placed in deionized water, heated to 85°C, stirred and washed for 15 minutes, filtered, dried with hot air at 80°C, and then subjected to low-temperature plasma treatment. The discharge mode during low-temperature plasma treatment was glow discharge, the reaction gas was carbon dioxide, the gas pressure was 3500Pa, the treatment power was 300W, and the treatment time was 5 minutes.
[0028] S12. The glass fiber treated with low-temperature plasma was dispersed in an ethanol aqueous solution with an ethanol concentration of 95wt%, and after stirring and dispersing for 10min, 10% KH-550 by volume of the ethanol aqueous solution was added, the temperature was raised to 75°C, and the reaction was refluxed and stirred for 8h, and the glass fiber was separated by centrifugation, and the glass fiber was washed twice with deionized water, and then dried to constant weight to obtain pretreated glass fiber;
[0029] S13. Disperse 1 part of 4,4-dicarboxylic acid benzophenone in DMF by weight, stir and mix for 15 minutes, add 0.01 part of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, continue to mix for 3 minutes, and then uniformly dropwise add it to 1.5 parts of 1,3-bis(aminopropyl)tetramethyldisiloxane for 1.5 hours. After the addition is completed, heat to 85°C, stir and react for 5 hours, cool to room temperature, and then cool the reaction mixture. The mixed solution was added dropwise to 1.4 parts of 1,6-hexanediol diglycidyl ether again for 3 hours. The mixture was stirred continuously during the addition process. After the addition was completed, the mixture was heated to 75°C and stirred for 5 hours. The mixture was then heated to 135°C and stirred for 0.5 hours. 5 parts of pretreated glass fiber were added. The mixture was ultrasonically shaken for 1.5 hours. The pretreated glass fiber was separated by centrifugation. The surface was washed twice with clean DMF and dried to constant weight to obtain modified glass fiber.
[0030] S2. Preparation of antistatic bulk molding compound composites;
[0031] Weigh 40 parts of bisphenol A type E-51 epoxy resin, 1.5 parts of dicyandiamide, 0.5 parts of benzyltriethylammonium chloride accelerator, 20 parts of calcium carbonate, 5 parts of carbon black and 1.5 parts of calcium stearate by weight, mix and stir evenly, then add 20 parts of modified glass fiber, knead at room temperature for 30 minutes to make the fiber fully impregnated and kneaded evenly to obtain an antistatic bulk molding compound composite material.
[0032] Embodiment 2. A method for preparing an antistatic bulk molding compound composite material, comprising the following steps:
[0033] Compared with Example 1, this embodiment increases the duration of low-temperature plasma treatment in step S1;
[0034] S1. Preparation of modified glass fiber;
[0035] The glass fiber was placed in deionized water, heated to 85°C, stirred and washed for 15 minutes, filtered, dried with hot air at 80°C, and then subjected to low-temperature plasma treatment. The discharge mode during low-temperature plasma treatment was glow discharge, the reaction gas was carbon dioxide, the gas pressure was 3500Pa, the treatment power was 300W, and the treatment time was 15 minutes.
[0036] S12. The glass fiber treated with low-temperature plasma was dispersed in an ethanol aqueous solution with an ethanol concentration of 95wt%, and after stirring and dispersing for 10min, 10% KH-550 by volume of the ethanol aqueous solution was added, the temperature was raised to 75°C, and the reaction was refluxed and stirred for 8h, and the glass fiber was separated by centrifugation, and the glass fiber was washed twice with deionized water, and then dried to constant weight to obtain pretreated glass fiber;
[0037] S13. Disperse 1 part of 4,4-dicarboxylic acid benzophenone in DMF by weight, stir and mix for 15 minutes, add 0.01 part of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, continue to mix for 3 minutes, and then uniformly dropwise add it to 1.5 parts of 1,3-bis(aminopropyl)tetramethyldisiloxane for 1.5 hours. After the addition is completed, heat to 85°C, stir and react for 5 hours, cool to room temperature, and then cool the reaction mixture. The mixed solution was added dropwise to 1.4 parts of 1,6-hexanediol diglycidyl ether again for 3 hours. The mixture was stirred continuously during the addition process. After the addition was completed, the mixture was heated to 75°C and stirred for 5 hours. The mixture was then heated to 135°C and stirred for 0.5 hours. 5 parts of pretreated glass fiber were added. The mixture was ultrasonically shaken for 1.5 hours. The pretreated glass fiber was separated by centrifugation. The surface was washed twice with clean DMF and dried to constant weight to obtain modified glass fiber.
[0038] S2. Preparation of antistatic bulk molding compound composites;
[0039] Weigh 40 parts of bisphenol A type E-51 epoxy resin, 1.5 parts of dicyandiamide, 0.5 parts of benzyltriethylammonium chloride accelerator, 20 parts of calcium carbonate, 5 parts of carbon black and 1.5 parts of calcium stearate by weight, mix and stir evenly, then add 20 parts of modified glass fiber, knead at room temperature for 30 minutes to make the fiber fully impregnated and kneaded evenly to obtain an antistatic bulk molding compound composite material.
[0040] Embodiment 3. A method for preparing an antistatic bulk molding compound composite material, comprising the following steps:
[0041] Compared with Example 1, this example increases the amount of 1,3-bis(aminopropyl)tetramethyldisiloxane added in step S13;
[0042] S1. Preparation of modified glass fiber;
[0043] The glass fiber was placed in deionized water, heated to 85°C, stirred and washed for 15 minutes, filtered, dried with hot air at 80°C, and then subjected to low-temperature plasma treatment. The discharge mode during low-temperature plasma treatment was glow discharge, the reaction gas was carbon dioxide, the gas pressure was 3500Pa, the treatment power was 300W, and the treatment time was 5 minutes.
[0044] S12. The glass fiber treated with low-temperature plasma was dispersed in an ethanol aqueous solution with an ethanol concentration of 95wt%, and after stirring and dispersing for 10min, 10% KH-550 by volume of the ethanol aqueous solution was added, the temperature was raised to 75°C, and the reaction was refluxed and stirred for 8h, and the glass fiber was separated by centrifugation, and the glass fiber was washed twice with deionized water, and then dried to constant weight to obtain pretreated glass fiber;
[0045] S13. Disperse 1 part of 4,4-dicarboxylic acid benzophenone in DMF by weight, stir and mix for 15 minutes, add 0.01 part of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, continue to mix for 3 minutes, and then uniformly add it dropwise to 1.8 parts of 1,3-bis(aminopropyl)tetramethyldisiloxane for 1.5 hours. After the addition is completed, heat to 85°C, stir and react for 5 hours, cool to room temperature, and then cool the reaction mixture. The mixed solution was added dropwise to 1.4 parts of 1,6-hexanediol diglycidyl ether again for 3 hours. The mixture was stirred continuously during the addition process. After the addition was completed, the mixture was heated to 75°C and stirred for 5 hours. The mixture was then heated to 135°C and stirred for 0.5 hours. 5 parts of pretreated glass fiber were added. The mixture was ultrasonically shaken for 1.5 hours. The pretreated glass fiber was separated by centrifugation. The surface was washed twice with clean DMF and dried to constant weight to obtain modified glass fiber.
[0046] S2. Preparation of antistatic bulk molding compound composites;
[0047] Weigh 40 parts of bisphenol A type E-51 epoxy resin, 1.5 parts of dicyandiamide, 0.5 parts of benzyltriethylammonium chloride accelerator, 20 parts of calcium carbonate, 5 parts of carbon black and 1.5 parts of calcium stearate by weight, mix and stir evenly, then add 20 parts of modified glass fiber, knead at room temperature for 30 minutes to make the fiber fully impregnated and kneaded evenly to obtain an antistatic bulk molding compound composite material.
[0048] Embodiment 4. A method for preparing an antistatic bulk molding compound composite material, comprising the following steps:
[0049] Compared with Example 3, this embodiment increases the amount of 1,6-hexanediol diglycidyl ether added in step S13;
[0050] S1. Preparation of modified glass fiber;
[0051] The glass fiber was placed in deionized water, heated to 85°C, stirred and washed for 15 minutes, filtered, dried with hot air at 80°C, and then subjected to low-temperature plasma treatment. The discharge mode during low-temperature plasma treatment was glow discharge, the reaction gas was carbon dioxide, the gas pressure was 3500Pa, the treatment power was 300W, and the treatment time was 5 minutes.
[0052] S12. The glass fiber treated with low-temperature plasma was dispersed in an ethanol aqueous solution with an ethanol concentration of 95wt%, and after stirring and dispersing for 10min, 10% KH-550 by volume of the ethanol aqueous solution was added, the temperature was raised to 75°C, and the reaction was refluxed and stirred for 8h, and the glass fiber was separated by centrifugation, and the glass fiber was washed twice with deionized water, and then dried to constant weight to obtain pretreated glass fiber;
[0053] S13. Disperse 1 part of 4,4-dicarboxylic acid benzophenone in DMF by weight, stir and mix for 15 minutes, add 0.01 part of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, continue to mix for 3 minutes, and then uniformly add it dropwise to 1.8 parts of 1,3-bis(aminopropyl)tetramethyldisiloxane for 1.5 hours. After the addition is completed, heat to 85°C, stir and react for 5 hours, cool to room temperature, and then cool the reaction mixture. The mixed solution was added dropwise to 1.7 parts of 1,6-hexanediol diglycidyl ether for 3 hours. The mixture was stirred continuously during the addition. After the addition was completed, the mixture was heated to 75°C and stirred for 5 hours. The mixture was then heated to 135°C and stirred for 0.5 hours. 5 parts of pretreated glass fiber were added. The mixture was ultrasonically shaken for 1.5 hours. The pretreated glass fiber was separated by centrifugation. The surface was washed twice with clean DMF and dried to constant weight to obtain modified glass fiber.
[0054] S2. Preparation of antistatic bulk molding compound composites;
[0055] Weigh 40 parts of bisphenol A type E-51 epoxy resin, 1.5 parts of dicyandiamide, 0.5 parts of benzyltriethylammonium chloride accelerator, 20 parts of calcium carbonate, 5 parts of carbon black and 1.5 parts of calcium stearate by weight, mix and stir evenly, then add 20 parts of modified glass fiber, knead at room temperature for 30 minutes to make the fiber fully impregnated and kneaded evenly to obtain an antistatic bulk molding compound composite material.
[0056] Comparative Example 1. A method for preparing an antistatic bulk molding compound composite material, comprising the following steps:
[0057] Compared with Example 1, this comparative example does not perform step S13 processing;
[0058] S1. Preparation of modified glass fiber;
[0059] The glass fiber was placed in deionized water, heated to 85°C, stirred and washed for 15 minutes, filtered, dried with hot air at 80°C, and then subjected to low-temperature plasma treatment. The discharge mode during low-temperature plasma treatment was glow discharge, the reaction gas was carbon dioxide, the gas pressure was 3500Pa, the treatment power was 300W, and the treatment time was 5 minutes.
[0060] S12. The glass fiber treated with low-temperature plasma was dispersed in an ethanol aqueous solution with an ethanol concentration of 95wt%, and after stirring and dispersing for 10min, 10% KH-550 by volume of the ethanol aqueous solution was added, the temperature was raised to 75°C, and the reaction was refluxed and stirred for 8h, and the glass fiber was separated by centrifugation, and the glass fiber was washed twice with deionized water, and then dried to constant weight to obtain a modified glass fiber;
[0061] S2. Preparation of antistatic bulk molding compound composites;
[0062] Weigh 40 parts of bisphenol A type E-51 epoxy resin, 1.5 parts of dicyandiamide, 0.5 parts of benzyltriethylammonium chloride accelerator, 20 parts of calcium carbonate, 5 parts of carbon black and 1.5 parts of calcium stearate by weight, mix and stir evenly, then add 20 parts of modified glass fiber, knead at room temperature for 30 minutes to make the fiber fully impregnated and kneaded evenly to obtain an antistatic bulk molding compound composite material.
[0063] Comparative Example 2. A method for preparing an antistatic bulk molding compound composite material, comprising the following steps:
[0064] Compared with Example 1, in step S13 of this embodiment, only 1,6-hexanediol diglycidyl ether was used to treat the pretreated glass fiber;
[0065] S1. Preparation of modified glass fiber;
[0066] The glass fiber was placed in deionized water, heated to 85°C, stirred and washed for 15 minutes, filtered, dried with hot air at 80°C, and then subjected to low-temperature plasma treatment. The discharge mode during low-temperature plasma treatment was glow discharge, the reaction gas was carbon dioxide, the gas pressure was 3500Pa, the treatment power was 300W, and the treatment time was 5 minutes.
[0067] S12. The glass fiber treated with low-temperature plasma was dispersed in an ethanol aqueous solution with an ethanol concentration of 95wt%, and after stirring and dispersing for 10min, 10% KH-550 by volume of the ethanol aqueous solution was added, the temperature was raised to 75°C, and the reaction was refluxed and stirred for 8h, and the glass fiber was separated by centrifugation, and the glass fiber was washed twice with deionized water, and then dried to constant weight to obtain pretreated glass fiber;
[0068] S13. Add 5 parts of pretreated glass fiber to 20 parts of 1,6-hexanediol diglycidyl ether by weight, react with ultrasonic vibration for 1.5 hours, centrifuge the pretreated glass fiber, wash its surface twice with clean DMF, and dry to constant weight to obtain modified glass fiber;
[0069] S2. Preparation of antistatic bulk molding compound composites;
[0070] Weigh 40 parts of bisphenol A type E-51 epoxy resin, 1.5 parts of dicyandiamide, 0.5 parts of benzyltriethylammonium chloride accelerator, 20 parts of calcium carbonate, 5 parts of carbon black and 1.5 parts of calcium stearate by weight, mix and stir evenly, then add 20 parts of modified glass fiber, knead at room temperature for 30 minutes to make the fiber fully impregnated and kneaded evenly to obtain an antistatic bulk molding compound composite material.
[0071] Comparative Example 3. A method for preparing an antistatic bulk molding compound composite material, comprising the following steps:
[0072] Compared with Example 1, this comparative example only used an equal amount of unmodified glass fiber as a replacement;
[0073] Weigh 40 parts of bisphenol A type E-51 epoxy resin, 1.5 parts of dicyandiamide, 0.5 parts of benzyltriethylammonium chloride accelerator, 20 parts of calcium carbonate, 5 parts of carbon black and 1.5 parts of calcium stearate by weight, mix and stir evenly, then add 20 parts of glass fiber, knead at room temperature for 30 minutes to allow the fiber to be fully impregnated and kneaded evenly to obtain an antistatic bulk molding compound composite material.
[0074] Testing: The antistatic bulk molding compound composite materials prepared in Examples 1-4 and Comparative Examples 1-3 were injection molded at an injection pressure of 30 MPa, a post-curing temperature of 160° C., and a curing time of 1.5 h;
[0075] According to GB 1447-2005, the antistatic bulk molding compound composite materials prepared in Examples 1-4 and Comparative Example 3 were injection molded and cured to prepare test specimens, and their tensile properties were tested;
[0076] According to GB 1449-2005, the antistatic bulk molding compound composite materials prepared in Examples 1-4 and Comparative Example 3 were injection molded and cured to prepare test specimens, and their bending strength was tested;
[0077] According to GB / T 1451-2005, the antistatic bulk molding compound composite materials prepared in Examples 1-4 and Comparative Example 3 were injection molded and cured to prepare test specimens, and their impact toughness was tested;
[0078] The antistatic bulk molding compound composite materials prepared in Examples 1-4 and Comparative Example 3 were injection molded and cured to prepare test samples, and then subjected to UV aging according to ISO 4892-3 standard. The test conditions were 340°C and the light wave was 0.76 W / m 2 After irradiation for 304 h, the tensile strength was tested again;
[0079] The test results are shown in the table below;
[0080]
[0081] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an antistatic bulk molding compound composite material, characterized in that: The following steps are involved: S1. Preparation of modified glass fiber; Place the glass fiber in deionized water, heat it to 75-85°C, stir and wash for 10-15 minutes, filter it, dry it with hot air at 80°C, and after constant weight, perform low-temperature plasma treatment on the glass fiber; S12. The glass fiber treated with low-temperature plasma is dispersed in an ethanol aqueous solution with an ethanol concentration of 90-95wt%, and after stirring and dispersing for 10-15min, 5-10% KH-550 by volume of the ethanol aqueous solution is added, the temperature is raised to 75-78°C, and the reaction is refluxed and stirred for 8-12h, and the glass fiber is separated by centrifugation, and the glass fiber is washed with deionized water for 2-3 times, and then dried to constant weight to obtain a pretreated glass fiber; S13. Disperse 4,4-dicarboxylic acid benzophenone in DMF, stir and mix for 15-25 minutes, add 1-ethyl-(3-dimethylaminopropyl)carbodiimide, continue mixing for 3-5 minutes, and then uniformly dropwise add it to 1,3-bis(aminopropyl)tetramethyldisiloxane for 1.5-2.5 hours. After the dropwise addition is completed, heat to 78-92°C, stir and react for 2-8 hours, cool to room temperature, and dropwise add the reaction mixture again. Add to 1,6-hexanediol diglycidyl ether, the dripping time is 3-5h, and the process is continuously stirred. After the dripping is completed, the temperature is raised to 75-85°C, and the reaction is stirred for 2-8h. The temperature is raised to 135°C, and the reaction is continued with stirring for 0.5-1h. The pretreated glass fiber is added, and the ultrasonic oscillation reaction is performed for 1.5-3h. The pretreated glass fiber is separated by centrifugation, and its surface is washed with clean DMF for 2-3 times, and then dried to constant weight to obtain modified glass fiber; S2. Preparation of antistatic bulk molding compound composites; Epoxy resin, latent curing agent, accelerator, inorganic filler, conductive filler and release agent are weighed and mixed according to weight fractions, stirred evenly, and then modified glass fiber is added. After kneading at room temperature for 20-30 minutes, the fiber is fully impregnated and kneaded evenly to obtain an antistatic bulk molding compound material.
2. The method for preparing an antistatic bulk molding compound composite material according to claim 1, characterized in that: The antistatic bulk molding compound composite material is formed by uniformly mixing 20-55 parts of epoxy resin, 1.5-5 parts of latent curing agent, 0.5-1.5 parts of accelerator, 15-45 parts of inorganic filler, 3-10 parts of conductive filler, 1.5-3 parts of release agent and 20-40 parts of chopped glass fiber by weight.
3. The method for preparing an antistatic bulk molding compound composite material according to claim 1, characterized in that: The epoxy resin is any one or more of bisphenol A type E-51 epoxy resin and bisphenol A type E-55 epoxy resin.
4. The method for preparing an antistatic bulk molding compound composite material according to claim 1, characterized in that: The latent curing agent is dicyandiamide; the accelerator is benzyltriethylammonium chloride.
5. The method for preparing an antistatic bulk molding compound composite material according to claim 1, characterized in that: The inorganic filler is any one of white carbon black and calcium carbonate; the conductive filler is carbon black; and the release agent is calcium stearate.
6. The method for preparing an antistatic bulk molding compound composite material according to claim 1, characterized in that: In step S11, during the low-temperature plasma treatment, the discharge mode is glow discharge, the reaction gas is carbon dioxide, the gas pressure is 2000-5000 Pa, the treatment power is 300-1000 W, and the treatment time is 1-15 min.
7. The method for preparing an antistatic bulk molding compound composite material according to claim 1, characterized in that: In step S13, the mass ratio of the 4,4-dicarboxylic acid benzophenone, 1-ethyl-(3-dimethylaminopropyl)carbodiimide, and 1,3-bis(aminopropyl)tetramethyldisiloxane is 1:(0.01-0.03):(1.5-1.8) in parts by weight.
8. The method for preparing an antistatic bulk molding compound composite material according to claim 1, characterized in that: In step S13, the mass ratio of the 4,4-dicarboxylic acid benzophenone, 1,6-hexanediol diglycidyl ether, and the pretreated glass fiber is 1:(1.4-1.7):(5-30) in parts by weight.
9. An antistatic bulk molding compound composite material prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Epoxy resin bulk molding compound and preparation method thereof
CN104140637A
Bulk molding compound for manufacturing automotive brake piston and preparation method thereof
CN105694365A
Anti-falling packaging box for circuit board protection and preparation process of anti-falling packaging box
CN116674279A
Intelligent preparation process of special material for glass fiber reinforced and toughened flame-retardant nylon
CN116834171A
Wave-absorbing bulk molding compound as well as preparation method and application thereof
CN117801469A
Cited By
Processing aid for tensile CPVC (Chlorinated Polyvinyl Chloride) plate and preparation process of processing aid
CN121471590A