Die-cutting-resistant self-adhesive glass cover plate protective film and preparation method thereof

Through the preparation method of self-adhesive glass cover protective film with three-layer structure, combined with modified low-density polyethylene, multi-wall carbon nanotubes and MXene nanosheets, the problem of insufficient performance in the cutting process of the existing self-adhesive film is solved, and the problem of insufficient performance in the cutting process is realized. Excellent mechanical, UV and anti-fouling properties.

CN118956280APending Publication Date: 2024-11-15GUANGDONG QINLE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411011367.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing self-adhesive films have problems with irregular cutting, cracking and debris during the cutting process, resulting in poor die-cutting performance and difficulty in taking into account excellent mechanical properties, UV resistance and anti-fouling properties.

Method used

The preparation method of three-layer structure, including protective layer, intermediate layer and self-adhesive layer, is used to form strong bonds by modifying the combination of low-density polyethylene, multi-wall carbon nanotubes and MXene nanosheets. Combined, it improves hydrophobic and anti-fouling properties and improves the toughness and dispersion of the intermediate layer by poly(ethylene-CO-methyl acrylate-CO-glycidyl methacrylate) modified multi-walled carbon nanotubes.

Benefits of technology

The self-adhesive glass cover protective film is realized in order and stability during cutting, improving mechanical properties, UV resistance and anti-fouling performance, avoiding imperfect cutting and cracking, and improving die-cutting performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956280A_ABST
    Figure CN118956280A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of layered products, and discloses a die-cutting-resistant self-adhesive glass cover plate protective film and a preparation method thereof. The preparation method of the die-cutting-resistant self-adhesive glass cover plate protective film comprises the following steps: mixing metallocene polyethylene and modified low-density polyethylene, and extruding to obtain a protective layer mixture; mixing high-density polyethylene, low-density polyethylene, the modified master batch and polyacrylate, and extruding to obtain a middle-layer mixture; taking low-density polyethylene and a styrene-butadiene-styrene block copolymer, mixing, and extruding to obtain a self-adhesive layer mixture; and preparing the protective layer mixture, the middle layer mixture and the self-adhesive layer mixture into the die-cutting-resistant self-adhesive glass cover plate protective film with a three-layer structure comprising a protective layer, a middle layer and a self-adhesive layer from top to bottom through a three-layer co-extrusion casting machine. The die-cutting-resistant self-adhesive glass cover plate protective film has excellent mechanical properties, hydrophobic antifouling properties and ultraviolet resistance, and is good in die-cutting performance and convenient to process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of layered product preparation, in particular to a die-cutting resistant self-adhesive glass cover plate protective film and a preparation method thereof. Background Art

[0002] With the development of science and technology and the improvement of people's living standards, electronic products are used more and more frequently in people's daily lives. Various electronic products are equipped with display screens, and glass cover plates are technical materials for TV screens. The quality of glass cover plates is directly related to the quality and service life of electronic products. In order to better protect the glass cover plates, a protective film is often covered on its surface. Self-adhesive film is a non-adhesive film that adheres to items by electrostatic adsorption to play a protective role. Due to different usage occasions, in certain occasions, self-adhesive films are required to have excellent mechanical properties as well as good anti-ultraviolet and anti-fouling properties. In addition, self-adhesive films are generally multi-layer structures. Due to the different mechanical properties of the materials of each layer and the insufficient bonding strength between the layers, problems such as uneven cutting, cracking and debris will occur, resulting in poor die-cutting performance. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a method for preparing a die-cutting resistant self-adhesive glass cover protective film, comprising the following steps:

[0004] Step (1), melt-blending metallocene polyethylene and modified low-density polyethylene to obtain a protective layer mixture; wherein the modified low-density polyethylene is obtained by modifying low-density polyethylene with a composite modifier; the preparation method of the composite modifier comprises the following steps:

[0005] Step A1, depositing nano zinc oxide on the surface of silicon dioxide nano particles to obtain composite nano particles;

[0006] Step A2, modifying the composite nanoparticles with 3-aminopropyltriethoxysilane to obtain amino composite nanoparticles; and then modifying the amino composite nanoparticles with phosphoric acid to obtain modified composite nanoparticles;

[0007] Step A3, loading the modified composite nanoparticles on MXene nanosheets to obtain loaded modified MXene nanosheets;

[0008] Step A4, oleic acid reacts with the loaded modified MXene nanosheets to obtain a composite modifier;

[0009] Step (2), melt blending high-density polyethylene, low-density polyethylene, modified masterbatch, and polyacrylate to obtain an intermediate layer mixture;

[0010] Wherein, the modified masterbatch is obtained by reacting modified multi-walled carbon nanotubes and poly(ethylene-CO-methyl acrylate-CO-glycidyl methacrylate); the modified multi-walled carbon nanotubes are obtained by modifying multi-walled carbon nanotubes with benzyl acetic acid;

[0011] Step (3), melt-blending low-density polyethylene and styrene-butadiene-styrene block copolymer to obtain a self-adhesive layer mixture;

[0012] Step (4), the protective layer mixture, the intermediate layer mixture, and the self-adhesive layer mixture are subjected to three-layer co-extrusion blown film, cooled and shaped, and then rolled and packaged to obtain a die-cutting resistant self-adhesive glass cover protective film having a three-layer structure from top to bottom including a protective layer, an intermediate layer, and a self-adhesive layer.

[0013] Preferably, in step (1), the contents of the components in the protective layer mixture are, by weight, 30-50 parts of metallocene polyethylene and 14-25 parts of modified low-density polyethylene.

[0014] Preferably, in the step (1), the preparation method of the modified low-density polyethylene is as follows: low-density polyethylene is added to an extruder at a feed rate of 40-50 kg / h, and then a mixture of dicumyl peroxide and a composite modifier is added at a feed rate of 20-30 g / min, and extruded at a speed of 40-60 rpm at 160-200° C. to obtain the modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, dicumyl peroxide, and composite modifier is 1:(0.002-0.004):(0.1-0.3);

[0015] In the above process, under the initiation of dicumyl peroxide, the composite modifier and the low-density polyethylene undergo polymerization reaction, and the composite modifier is connected to the low-density polyethylene in a chemical grafting manner.

[0016] Preferably, in step (1), the method for preparing the composite modifier comprises the following steps:

[0017] Step A1, mixing n-octyltriethoxysilane, water and ammonia water in a volume ratio of 1:(2.8-3.2):(0.9-1.1) at room temperature at a speed of 200-400 r / min, aging for 3.5-4.5 h, centrifuging, washing and drying to obtain silica nanoparticles;

[0018] Disperse silica nanoparticles in an ethanol aqueous solution, heat to 80-90° C., stir for 10-20 min, then simultaneously add a 1.6 mol / L triethanolamine aqueous solution and a 0.02 mol / L zinc acetate aqueous solution at a drip rate of 1-2 mL / min, continue stirring at 80-90° C. for 50-80 min, centrifuge, wash the obtained solid product with deionized water, dry it, and calcine it at 680-720° C. for 2.5-3.5 h to obtain composite nanoparticles; wherein the ethanol aqueous solution is obtained by mixing ethanol and water in a volume ratio of 3:2; the amount ratio of the silica nanoparticles, the ethanol aqueous solution, the triethanolamine aqueous solution, and the zinc acetate aqueous solution is (0.2-0.4) g:(30-50) mL:(10-20) mL:(20-30) mL;

[0019] In the above process, n-octyltriethoxysilane is first used as a precursor to prepare nano-silica particles, and then zinc acetate is used as a precursor of zinc oxide to deposit nano-zinc oxide on the surface of nano-silica to form composite nano-particles.

[0020] Step A2, adding the composite nanoparticles to ethanol at 60-70° C. to obtain a mixed solution; dissolving 3-aminopropyltriethoxysilane in ethanol, adjusting the pH to 3.8-4.2 with acetic acid, and then adding the above mixed solution, stirring and reacting in an oil bath at 60-80° C. for 40-80 minutes, centrifuging, washing, and drying to obtain amino composite nanoparticles; wherein the mass ratio of the composite nanoparticles to 3-aminopropyltriethoxysilane is (2-3):(0.04-0.08);

[0021] The aminated composite nanoparticles and 85 wt% phosphoric acid aqueous solution are mixed, stirred in an oil bath at 70-90° C. for 40-80 min, centrifuged, the obtained precipitate is washed with water until the pH of the washing solution reaches 5.8-6.2, and vacuum dried at 50-70° C. to constant weight to obtain modified composite nanoparticles; wherein the amount ratio of the aminated composite nanoparticles to the phosphoric acid aqueous solution is (0.2-0.4) g: (10-15) mL;

[0022] In the above process, the silanol bonds formed by the hydrolysis of 3-aminopropyltriethoxysilane react with the hydroxyl groups on the surface of the composite nanomaterial, and amino groups and hydroxyl groups are introduced on the surface of the composite nanoparticles. The amino groups then react with the phosphate groups to obtain modified composite nanoparticles.

[0023] Step A3, adding LiF to a 12 mol / L hydrochloric acid aqueous solution, stirring for 10-20 min, then adding titanium aluminum carbide, stirring and reacting at 40-50° C. for 20-28 h, centrifuging, removing the supernatant, centrifuging and washing the product 2-4 times with a 1 mol / L hydrochloric acid aqueous solution, and then washing with deionized water until the washing liquid is neutral to obtain a solid product; wherein the amount ratio of LiF, hydrochloric acid aqueous solution, and titanium aluminum carbide is (1.6-3.2) g: (30-50) mL: (1-2) g;

[0024] The solid product was added to 0°C ice water, and ultrasonically exfoliated for 100-150 min in a nitrogen atmosphere, centrifuged, and dried to obtain MXene nanosheets; the mass ratio of the solid product to ice water was (1-2): (100-200);

[0025] The modified composite nanoparticles, MXene nanosheets, and deionized water are mixed in a mass ratio of (1-1.5):1:(50-80), reacted at 110-130° C. for 11-13 h, centrifuged, washed, and freeze-dried to obtain loaded modified MXene nanosheets;

[0026] In the above process, LiF and titanium aluminum carbide are used as raw materials and then ultrasonic stripping is performed to obtain MXene nanosheets; the modified composite nanoparticles and MXene nanosheets form a strong binding effect through hydrogen bonds and Ti-OP covalent bonds, and the modified composite nanoparticles are loaded on the MXene nanosheets.

[0027] Step A4, dissolving oleic acid in dimethyl sulfoxide, adding the loaded modified MXene nanosheets, reacting for 5-7 hours under the conditions of vacuum degree of 40-50 Pa and temperature of 160-170° C., centrifuging, washing, and drying to obtain a composite modifier; wherein the mass ratio of oleic acid, dimethyl sulfoxide, and loaded modified MXene nanosheets is (0.8-1.2):(10-15):1;

[0028] In the above process, the carboxyl groups in oleic acid undergo esterification reaction with the hydroxyl groups on the surface of the modified MXene nanosheets, introducing hydrophobic alkyl chains and C=C double bonds on the modified MXene nanosheets.

[0029] Preferably, in step (2), the contents of the components in the intermediate layer mixture are, by weight: 15-25 parts of high-density polyethylene, 28-40 parts of low-density polyethylene, 1.5-3.5 parts of modified masterbatch, and 10-15 parts of polyacrylate;

[0030] Preferably, in the step (2), the preparation method of the modified masterbatch is: mixing the modified multi-walled carbon nanotubes and poly(ethylene-co-methyl acrylate-co-glycidyl methacrylate) in a mass ratio of 1:(3.5-4.5), and extruding at 180-210° C. and a rotation speed of 150-200 rpm to obtain the modified masterbatch;

[0031] Preferably, in the step (2), the preparation method of the modified multi-walled carbon nanotubes is as follows: multi-walled carbon nanotubes and benzyl acetic acid are mixed in a mass ratio of 1:(0.8-1.2), and ball milled for 40-80 min at a ball-to-material ratio of (900-1000):1 and a rotation speed of 250-350 rpm to obtain modified multi-walled carbon nanotubes;

[0032] In the above process, multi-walled carbon nanotubes and benzyl acetic acid are combined through π-π interaction, carboxyl groups are introduced on the surface of multi-walled carbon nanotubes, and the carboxyl groups react with the epoxy groups in poly(ethylene-CO-methyl acrylate-CO-glycidyl methacrylate) to obtain a modified masterbatch.

[0033] Preferably, in step (3), the contents of the components in the self-adhesive layer mixture are, by weight, 32-58 parts of low-density polyethylene and 16-35 parts of styrene-butadiene-styrene block copolymer.

[0034] Preferably, in step (4), the thickness of the protective layer is 30-50 μm, the thickness of the intermediate layer is 20-40 μm, and the thickness of the self-adhesive layer is 15-35 μm; the film blowing conditions are: the head temperature is 170-210°C, the traction ratio is 4-6, and the blowing ratio is 2-5; the cooling method for cooling and shaping is air cooling, and the air cooling temperature is 5-20°C.

[0035] The die-cutting resistant self-adhesive glass cover plate protective film is prepared by the method for preparing the die-cutting resistant self-adhesive glass cover plate protective film.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] 1. The present invention composites hydrophobic silica nanoparticles with zinc oxide nanoparticles having dual functions of ultraviolet protection and hydrophobicity to obtain composite nanoparticles; the composite nanoparticles are then loaded on the surface of MXene nanosheets with excellent ultraviolet shielding performance through hydrogen bonds and covalent bonds. At the same time, the inorganic material itself has excellent mechanical properties, so the loaded modified MXene nanosheets can improve the hydrophobic and antifouling properties, anti-ultraviolet properties and mechanical properties of the protective layer; further, the loaded modified MXene nanosheets are modified by oleic acid, which not only introduces hydrophobic chains on the surface of the loaded modified MXene nanosheets to improve its hydrophobic and antifouling properties, but also provides carbon-carbon double bonds that react with low-density polyethylene, so that the loaded modified MXene nanosheets can be connected to the low-density polyethylene in the form of chemical bonds, thereby being evenly and stably dispersed in the low-density polyethylene, thereby further improving the hydrophobic and antifouling properties, anti-ultraviolet properties and mechanical properties of the protective layer.

[0038] 2. The modified masterbatch of the present invention is obtained by modifying multi-walled carbon nanotubes with benzyl acetic acid and then reacting with poly(ethylene-CO-methyl acrylate-CO-glycidyl methacrylate). The addition of multi-walled carbon nanotubes with excellent mechanical properties can effectively improve the mechanical properties of the polymer; and the high toughness of poly(ethylene-CO-methyl acrylate-CO-glycidyl methacrylate) after modifying the multi-walled carbon nanotubes significantly improves the toughness of the intermediate layer, and due to the similarity between the main chain structure of poly(ethylene-CO-methyl acrylate-CO-glycidyl methacrylate) and polyethylene, the dispersibility of the multi-walled carbon nanotubes in the polyethylene material is improved through intermolecular entanglement, and the connection strength between the multi-walled carbon nanotubes and the polyethylene material is enhanced.

[0039] 3. The present invention adds polyacrylate to the middle layer mixture to improve the bonding strength between the middle layer and the protective layer and the self-adhesive layer. In addition, due to the excellent mechanical properties of each layer material, when the overall protective film is cut, there will be no problems of uneven cutting, cracking, or debris at the cutting edge. The die-cutting performance is good and processing is convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a process flow chart of a method for preparing a die-cutting resistant self-adhesive glass cover protective film of the present invention;

[0041] Figure 2 It is a comparison diagram of water contact angle test of die-cutting resistant self-adhesive glass cover protective films of Examples 2-4 of the present invention and Comparative Examples 4-9;

[0042] Figure 3 It is a comparison chart of tensile strength tests of die-cutting resistant self-adhesive glass cover protective films of Examples 2-4 of the present invention and Comparative Examples 4-9;

[0043] Figure 4 It is a comparison chart of the tensile strength retention rate test of the die-cutting resistant self-adhesive glass cover protective films of Examples 2-4 of the present invention and Comparative Examples 4-9. DETAILED DESCRIPTION

[0044] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0045] Example 1

[0046] This embodiment discloses a method for preparing a composite modifier, comprising the following steps:

[0047] Step A1, n-octyltriethoxysilane, water, and ammonia water are stirred and mixed at a volume ratio of 1:3:1 at room temperature at a speed of 300r / min, aged for 4h, centrifuged, and the obtained solid product is washed with ethanol and then dried to obtain silica nanoparticles; 0.3g of silica nanoparticles are dispersed in 40mL of ethanol aqueous solution, heated to 85°C, stirred for 15min, and then 15mL of 1.6mol / L triethanolamine aqueous solution and 25mL of 0.02mol / L zinc acetate aqueous solution are added dropwise at a drop rate of 1.5mL / min, and stirring is continued at 85°C for 65min, centrifuged, and the obtained solid product is washed with deionized water and then dried, and calcined at 700°C for 3h to obtain composite nanoparticles; wherein the ethanol aqueous solution is obtained by mixing ethanol and water in a volume ratio of 3:2;

[0048] Step A2, adding 0.25g of composite nanoparticles to 4mL of ethanol at 65°C to obtain a mixed solution; dissolving 0.006g of 3-aminopropyltriethoxysilane in 12mL of ethanol, adjusting the pH to 4 with acetic acid, and then adding the above mixed solution, stirring and reacting in an oil bath at 70°C for 60min, centrifuging, washing the obtained precipitate with water 4 times, and drying to obtain amino composite nanoparticles; mixing 0.3g of amino composite nanoparticles and 12.5mL of 85wt% phosphoric acid aqueous solution, stirring and reacting in an oil bath at 80°C for 60min, centrifuging, washing the obtained precipitate with water until the pH of the washing solution reaches 6, and vacuum drying at 60°C to constant weight to obtain modified composite nanoparticles;

[0049] Step A3, adding 2.4g LiF to 40mL 12mol / L hydrochloric acid aqueous solution, stirring for 15min, then adding 1.5g titanium aluminum carbide, stirring and reacting at 45°C for 24h, centrifuging, removing the supernatant, centrifuging and washing the product 3 times with 1mol / L hydrochloric acid aqueous solution, and then washing with deionized water until the washing liquid is neutral to obtain a solid product, adding 1.5g of the solid product to 150mL 0°C ice water, ultrasonically exfoliating for 120min in a nitrogen atmosphere, centrifuging, and drying to obtain MXene nanosheets; the modified composite nanoparticles, MXene nanosheets, and deionized water are mixed in a mass ratio of 1.2:1:65, reacting at 120°C for 12h, centrifuging, washing, and freeze-drying to obtain loaded modified MXene nanosheets;

[0050] Step A4, dissolving oleic acid in dimethyl sulfoxide, adding loaded modified MXene nanosheets, reacting for 6 hours under vacuum conditions of 45 Pa and 165 ° C, centrifuging, washing, and drying to obtain a composite modifier; wherein the mass ratio of oleic acid, dimethyl sulfoxide, and loaded modified MXene nanosheets is 1:12.5:1.

[0051] Example 2

[0052] This embodiment discloses a method for preparing a die-cutting resistant self-adhesive glass cover protective film, comprising the following steps:

[0053] Step (1), adding low-density polyethylene to an extruder at a feed rate of 40 kg / h, and then adding a mixture of dicumyl peroxide and a composite modifier at a feed rate of 20 g / min, and extruding at a speed of 60 rpm at 160° C. to obtain modified low-density polyethylene; wherein the mass ratio of the low-density polyethylene, dicumyl peroxide, and the composite modifier is 1:0.002:0.1;

[0054] In parts by weight, 30 parts of metallocene polyethylene and 14 parts of modified low-density polyethylene are melt-blended to obtain a protective layer mixture;

[0055] Step (2), mixing multi-walled carbon nanotubes and benzyl acetic acid in a mass ratio of 1:0.8, ball milling for 80 min at a ball-to-material ratio of 900:1 and a rotation speed of 350 rpm to obtain modified multi-walled carbon nanotubes; mixing modified multi-walled carbon nanotubes and poly(ethylene-co-methyl acrylate-co-glycidyl methacrylate) in a mass ratio of 1:3.5, extruding at 180° C. at a rotation speed of 200 rpm to obtain a modified masterbatch;

[0056] In parts by weight, 15 parts of high-density polyethylene, 28 parts of low-density polyethylene, 1.5 parts of modified masterbatch, and 10 parts of polyacrylate are melt-blended to obtain an intermediate layer mixture;

[0057] Step (3), taking 32 parts of low-density polyethylene and 16 parts of styrene-butadiene-styrene block copolymer by weight and melt-blending to obtain a self-adhesive layer mixture;

[0058] Step (4), subjecting the protective layer mixture, the intermediate layer mixture and the self-adhesive layer mixture to three-layer co-extrusion blow film, cooling and shaping, and then rolling and packaging to obtain a die-cutting resistant self-adhesive glass cover protective film having a three-layer structure from top to bottom comprising a protective layer, an intermediate layer and a self-adhesive layer; wherein the thickness of the protective layer is 30 μm, the thickness of the intermediate layer is 20 μm, and the thickness of the self-adhesive layer is 15 μm; the film blowing conditions are: the head temperature is 170°C, the traction ratio is 4, and the blowing ratio is 2; the cooling method for cooling and shaping is air cooling, and the air cooling temperature is 5°C.

[0059] Example 3

[0060] This embodiment discloses a method for preparing a die-cutting resistant self-adhesive glass cover protective film, comprising the following steps:

[0061] Step (1), adding low-density polyethylene to an extruder at a feed rate of 50 kg / h, and then adding a mixture of dicumyl peroxide and a composite modifier at a feed rate of 30 g / min, and extruding at a speed of 40 rpm at 200° C. to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, dicumyl peroxide, and composite modifier is 1:0.004:0.3;

[0062] In parts by weight, 50 parts of metallocene polyethylene and 25 parts of modified low-density polyethylene are melt-blended to obtain a protective layer mixture;

[0063] Step (2), mixing multi-walled carbon nanotubes and benzyl acetic acid in a mass ratio of 1:1.2, ball milling for 40 minutes under the conditions of a ball-to-material ratio of 1000:1 and a rotation speed of 350 rpm to obtain modified multi-walled carbon nanotubes; mixing the modified multi-walled carbon nanotubes and poly (ethylene-co-methyl acrylate-co-glycidyl methacrylate) in a mass ratio of 1:4.5, extruding at 210° C. at a rotation speed of 150 rpm to obtain a modified masterbatch;

[0064] In parts by weight, 25 parts of high-density polyethylene, 40 parts of low-density polyethylene, 3.5 parts of modified masterbatch, and 15 parts of polyacrylate are melt-blended to obtain an intermediate layer mixture;

[0065] Step (3), taking 58 parts of low-density polyethylene and 35 parts of styrene-butadiene-styrene block copolymer by weight and melt-blending to obtain a self-adhesive layer mixture;

[0066] Step (4), subjecting the protective layer mixture, the intermediate layer mixture and the self-adhesive layer mixture to three-layer co-extrusion blow film, cooling and shaping, and then rolling and packaging to obtain a die-cutting resistant self-adhesive glass cover protective film having a three-layer structure from top to bottom comprising a protective layer, an intermediate layer and a self-adhesive layer; wherein the thickness of the protective layer is 50 μm, the thickness of the intermediate layer is 40 μm, and the thickness of the self-adhesive layer is 35 μm; the film blowing conditions are: the head temperature is 210°C, the traction ratio is 6, and the blowing ratio is 5; the cooling method for cooling and shaping is air cooling, and the air cooling temperature is 20°C.

[0067] Example 4

[0068] This embodiment discloses a method for preparing a die-cutting resistant self-adhesive glass cover protective film, comprising the following steps:

[0069] Step (1), adding low-density polyethylene to an extruder at a feed rate of 45 kg / h, and then adding a mixture of dicumyl peroxide and a composite modifier at a feed rate of 25 g / min, and extruding at a speed of 50 rpm at 180° C. to obtain modified low-density polyethylene; wherein the mass ratio of low-density polyethylene, dicumyl peroxide, and composite modifier is 1:0.003:0.2;

[0070] In parts by weight, 40 parts of metallocene polyethylene and 20 parts of modified low-density polyethylene are mixed and extruded to obtain a protective layer mixture;

[0071] Step (2), mixing multi-walled carbon nanotubes and benzyl acetic acid in a mass ratio of 1:1, ball milling for 60 minutes under the conditions of a ball-to-material ratio of 950:1 and a rotation speed of 280 rpm to obtain modified multi-walled carbon nanotubes; mixing the modified multi-walled carbon nanotubes and poly (ethylene-co-methyl acrylate-co-glycidyl methacrylate) in a mass ratio of 1:4, extruding at 190° C. and a rotation speed of 180 rpm to obtain a modified masterbatch;

[0072] In parts by weight, 20 parts of high-density polyethylene, 34 parts of low-density polyethylene, 2.5 parts of modified masterbatch, and 12.5 parts of polyacrylate are mixed and extruded to obtain an intermediate layer mixture;

[0073] Step (3), by weight, 45 parts of low-density polyethylene and 25 parts of styrene-butadiene-styrene block copolymer are mixed and extruded to obtain a self-adhesive layer mixture;

[0074] Step (4), subjecting the protective layer mixture, the intermediate layer mixture, and the self-adhesive layer mixture to three-layer co-extrusion blow film, cooling and shaping, and then rolling and packaging to obtain a die-cutting resistant self-adhesive glass cover protective film having a three-layer structure from top to bottom comprising a protective layer, an intermediate layer, and a self-adhesive layer; wherein the thickness of the protective layer is 40 μm, the thickness of the intermediate layer is 30 μm, and the thickness of the self-adhesive layer is 25 μm; the film blowing conditions are: the head temperature is 190°C, the traction ratio is 5, and the blowing ratio is 3.5; the cooling method for cooling and shaping is air cooling, and the air cooling temperature is 10°C.

[0075] The composite modifier in Examples 2-4 adopts the composite modifier prepared in Example 1.

[0076] Comparative Example 1

[0077] Comparative Example 1 Compared with Example 1, in the process of preparing the loaded modified MXene nanosheets in Comparative Example 1, modified silica nanoparticles are used instead of modified composite nanoparticles, that is, zinc oxide nanoparticles are not deposited on the surface of the silica nanoparticles, and other conditions remain unchanged.

[0078] Comparative Example 2

[0079] Compared with Example 1, in the process of preparing the composite modifier, Comparative Example 2 uses MXene nanosheets instead of loaded modified MXene nanosheets, and other conditions remain unchanged.

[0080] Comparative Example 3

[0081] Comparative Example 3 Compared with Example 1, in the process of preparing the composite modifier, the modified composite nanoparticles are used instead of the loaded modified MXene nanosheets, and other conditions remain unchanged.

[0082] Comparative Example 4

[0083] Comparative Example 4 Compared with Example 4, Comparative Example 4 uses the composite modifier prepared in Comparative Example 1, and other conditions remain unchanged.

[0084] Comparative Example 5

[0085] Comparative Example 5 Compared with Example 4, Comparative Example 5 uses the composite modifier prepared in Comparative Example 2, and other conditions remain unchanged.

[0086] Comparative Example 6

[0087] Comparative Example 6 Compared with Example 4, Comparative Example 6 uses the composite modifier prepared in Comparative Example 3, and other conditions remain unchanged.

[0088] Comparative Example 7

[0089] Compared with Example 4, Comparative Example 7 uses loaded modified MXene nanosheets instead of the composite modifier in the process of preparing modified low-density polyethylene, and other conditions remain unchanged.

[0090] Comparative Example 8

[0091] Compared with Example 4, in Comparative Example 8, modified multi-walled carbon nanotubes are used instead of modified masterbatch in the process of preparing the intermediate layer mixture, and other conditions remain unchanged.

[0092] Comparative Example 9

[0093] Comparative Example 9 Compared with Example 4, in Comparative Example 9, no modified masterbatch was added during the preparation of the intermediate layer mixture, and other conditions remained unchanged.

[0094] In the above embodiments and comparative examples, multi-walled carbon nanotubes, inner diameter: 5-10nm, outer diameter: 10-20nm, length 10-30μm, from Shanghai Yien Chemical Technology Co., Ltd.; low-density polyethylene, brand 868-000, melt index 45-50g / 10min, from Dongguan Quanneng Plastic Raw Materials Co., Ltd.; poly (ethylene-CO-methyl acrylate-CO-glycidyl methacrylate), CAS No. 51541-08-3, from Shanghai Yuanye Biotechnology Co., Ltd.; high-density polyethylene, brand HHM5502LW, melt flow rate 0.34g / 10min, from Shenzhen Zhengrui Plastic Co., Ltd.; metallocene polyethylene, brand SP2320, melt flow rate 1.9g / 10min, from Shanghai Haowei New Materials Co., Ltd.; polyacrylate, from Jining Sanshi Biotechnology Co., Ltd.; styrene-butadiene-styrene block copolymer, brand: Maoming Petrochemical. Product name: Thermoplastic elastomer SBS, model: YH-796, from Guangzhou Zhisheng Yousu Petrochemical Co., Ltd.

[0095] Experimental example

[0096] The performance tests were conducted on the die-cutting resistant self-adhesive glass cover protective films of Examples 2-4 and Comparative Examples 4-9.

[0097] 1. Tensile performance test: Use the standard "GB13022-1991 Plastic Film Tensile Performance Test Method" to test and obtain the corresponding tensile strength.

[0098] 2. Anti-ultraviolet performance test: Place each group of samples in a UV box equipped with a 300W UV-A lamp (the wavelength range of the UV lamp is 280-350nm), place the samples 40cm away from the lamp for irradiation for 96h, measure and calculate the tensile strength retention rate of each group of samples to characterize the anti-ultraviolet performance.

[0099] 3. Water contact angle test: Use the feeler meter JC2000D to measure the water contact angle.

[0100] The test results are shown in Table 1:

[0101] Table 1

[0102] Water contact angle / ° Tensile strength / MPa Tensile strength retention rate / % Example 2 141.9 55.3 97.7 Example 3 143.4 56.8 98.6 Example 4 142.5 55.9 98.1 Comparative Example 4 136.6 53.4 96.7 Comparative Example 5 132.1 51.0 96.6 Comparative Example 6 143.3 49.2 96.3 Comparative Example 7 122.4 54.8 97.4 Comparative Example 8 142.5 54.6 98.0 Comparative Example 9 142.4 50.5 98.1

[0103] It can be seen from the test results in Table 1 that the die-cutting resistant self-adhesive glass cover protective films prepared in Examples 2-4 of the present invention have excellent mechanical properties, hydrophobic antifouling properties and anti-ultraviolet properties.

[0104] Hydrophobicity analysis: From the comparison between Comparative Examples 4-7 and Example 4, it can be seen that zinc oxide nanoparticles, silicon dioxide nanoparticles, and oleic acid can improve the hydrophobicity of the membrane material due to their own hydrophobicity, thereby making the membrane material have anti-fouling properties, while the MXene nanosheets, which are hydrophilic in themselves, will cause the hydrophobicity and anti-fouling properties of the membrane material to decrease.

[0105] Mechanical properties analysis: From the comparison of Comparative Examples 4-6 and Comparative Example 9 with Example 4, it can be seen that the inorganic nanomaterials zinc oxide nanoparticles, silica nanoparticles, MXene nanosheets, and modified multi-walled carbon nanotubes have a positive effect on improving the mechanical properties of the membrane material; from the comparison of Comparative Example 7 with Example 4, it can be seen that oleic acid improves the dispersion effect of the loaded modified MXene nanosheets, thereby improving the mechanical properties of the membrane material; from the comparison of Comparative Example 8 with Example 4, it can be seen that poly(ethylene-CO-methyl acrylate-CO-glycidyl methacrylate) improves the dispersibility of multi-walled carbon nanotubes in polyethylene materials and enhances the connection strength between multi-walled carbon nanotubes and polyethylene materials through intermolecular entanglement, thereby improving the mechanical properties of the membrane material.

[0106] Analysis of anti-ultraviolet performance: From the comparison of comparative examples 4-6 with embodiment 4, it can be seen that the nano zinc oxide particles and MXene nanosheets with ultraviolet shielding absorption effect can enable the membrane material to maintain a very high tensile strength after ultraviolet irradiation, reflecting excellent anti-ultraviolet performance. From the comparison of comparative example 7 with embodiment 4, it can be seen that oleic acid, as a connecting intermediate between the loaded modified MXene nanosheets and the low-density polyethylene, improves the dispersion effect of the loaded modified MXene nanosheets, thereby improving the anti-ultraviolet performance of the membrane material.

[0107] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a die-cutting resistant self-adhesive glass cover protective film, characterized in that: The following steps are involved: Step (1), melt-blending metallocene polyethylene and modified low-density polyethylene to obtain a protective layer mixture; wherein the modified low-density polyethylene is obtained by modifying low-density polyethylene with a composite modifier; the preparation method of the composite modifier comprises the following steps: Step A1, depositing nano zinc oxide on the surface of silicon dioxide nano particles to obtain composite nano particles; Step A2, modifying the composite nanoparticles with 3-aminopropyltriethoxysilane to obtain amino composite nanoparticles; and then modifying the amino composite nanoparticles with phosphoric acid to obtain modified composite nanoparticles; Step A3, loading the modified composite nanoparticles on MXene nanosheets to obtain loaded modified MXene nanosheets; Step A4, oleic acid reacts with the loaded modified MXene nanosheets to obtain a composite modifier; Step (2), melt blending high-density polyethylene, low-density polyethylene, modified masterbatch, and polyacrylate to obtain an intermediate layer mixture; Wherein, the modified masterbatch is obtained by reacting modified multi-walled carbon nanotubes and poly(ethylene-CO-methyl acrylate-CO-glycidyl methacrylate); the modified multi-walled carbon nanotubes are obtained by modifying multi-walled carbon nanotubes with benzyl acetic acid; Step (3), melt-blending low-density polyethylene and styrene-butadiene-styrene block copolymer to obtain a self-adhesive layer mixture; Step (4), the protective layer mixture, the intermediate layer mixture, and the self-adhesive layer mixture are subjected to three-layer co-extrusion blown film, cooled and shaped, and then rolled and packaged to obtain a die-cutting resistant self-adhesive glass cover protective film having a three-layer structure from top to bottom including a protective layer, an intermediate layer, and a self-adhesive layer.

2. The method for preparing the die-cutting resistant self-adhesive glass cover protective film according to claim 1, characterized in that: In the step (1), the content of each component in the protective layer mixture is, by weight, 30-50 parts of metallocene polyethylene and 14-25 parts of modified low-density polyethylene.

3. The method for preparing the die-cutting resistant self-adhesive glass cover protective film according to claim 1, characterized in that: In the step (1), the preparation method of the modified low-density polyethylene is as follows: low-density polyethylene is added to an extruder at a feed rate of 40-50 kg / h, and then a mixture of dicumyl peroxide and a composite modifier is added at a feed rate of 20-30 g / min, and extruded at a speed of 40-60 rpm at 160-200° C. to obtain the modified low-density polyethylene; wherein the mass ratio of the low-density polyethylene, dicumyl peroxide, and the composite modifier is 1:(0.002-0.004):(0.1-0.3).

4. The method for preparing the die-cutting resistant self-adhesive glass cover protective film according to claim 1, characterized in that: In the step (1), the method for preparing the composite modifier comprises the following steps: Step A1, mixing n-octyltriethoxysilane, water and ammonia water in a volume ratio of 1:(2.8-3.2):(0.9-1.1) at room temperature at a speed of 200-400 r / min, aging for 3.5-4.5 h, centrifuging, washing and drying to obtain silica nanoparticles; Disperse silicon dioxide nanoparticles in an ethanol aqueous solution, heat to 80-90° C., stir for 10-20 min, then simultaneously add a 1.6 mol / L triethanolamine aqueous solution and a 0.02 mol / L zinc acetate aqueous solution at a drip rate of 1-2 mL / min, continue stirring at 80-90° C. for 50-80 min, centrifuge, wash the obtained solid product with deionized water, dry it, and calcine it at 680-720° C. for 2.5-3.5 h to obtain composite nanoparticles; wherein the ethanol aqueous solution is obtained by mixing ethanol and water in a volume ratio of 3:2; the amount ratio of silicon oxide nanoparticles, ethanol aqueous solution, triethanolamine aqueous solution, and zinc acetate aqueous solution is (0.2-0.4) g:(30-50) mL:(10-20) mL:(20-30) mL; Step A2, adding the composite nanoparticles to ethanol at 60-70° C. to obtain a mixed solution; dissolving 3-aminopropyltriethoxysilane in ethanol, adjusting the pH to 3.8-4.2 with acetic acid, and then adding the above mixed solution, stirring and reacting in an oil bath at 60-80° C. for 40-80 minutes, centrifuging, washing, and drying to obtain amino composite nanoparticles; wherein the mass ratio of the composite nanoparticles to 3-aminopropyltriethoxysilane is (2-3):(0.04-0.08); The aminated composite nanoparticles and 85 wt% phosphoric acid aqueous solution are mixed, stirred in an oil bath at 70-90° C. for 40-80 min, centrifuged, and the obtained precipitate is washed with water until the pH of the washing solution reaches 5.8-6.2, and dried to obtain modified composite nanoparticles; wherein the amount ratio of the aminated composite nanoparticles to the phosphoric acid aqueous solution is (0.2-0.4) g: (10-15) mL; Step A3, adding LiF to a 12 mol / L hydrochloric acid aqueous solution, stirring for 10-20 min, then adding titanium aluminum carbide, stirring and reacting at 40-50° C. for 20-28 h, centrifuging, removing the supernatant, centrifuging and washing the product 2-4 times with a 1 mol / L hydrochloric acid aqueous solution, and then washing with deionized water until the washing liquid is neutral to obtain a solid product; wherein the amount ratio of LiF, hydrochloric acid aqueous solution, and titanium aluminum carbide is (1.6-3.2) g: (30-50) mL: (1-2) g; The solid product was added to 0°C ice water, and ultrasonically exfoliated for 100-150 min in a nitrogen atmosphere, centrifuged, and dried to obtain MXene nanosheets; the mass ratio of the solid product to ice water was (1-2): (100-200); The modified composite nanoparticles, MXene nanosheets, and deionized water are mixed in a mass ratio of (1-1.5):1:(50-80), reacted at 110-130° C. for 11-13 h, centrifuged, washed, and freeze-dried to obtain loaded modified MXene nanosheets; Step A4, dissolving oleic acid in dimethyl sulfoxide, adding loaded modified MXene nanosheets, reacting for 5-7 hours under vacuum conditions of 40-50 Pa and 160-170 ° C, centrifuging, washing, and drying to obtain a composite modifier; wherein the mass ratio of oleic acid, dimethyl sulfoxide, and loaded modified MXene nanosheets is (0.8-1.2):(10-15):

1.

5. The method for preparing the die-cutting resistant self-adhesive glass cover protective film according to claim 1, characterized in that: In the step (2), the contents of the components in the intermediate layer mixture are, by weight, 15-25 parts of high-density polyethylene, 28-40 parts of low-density polyethylene, 1.5-3.5 parts of modified masterbatch, and 10-15 parts of polyacrylate.

6. The method for preparing the die-cutting resistant self-adhesive glass cover protective film according to claim 1, characterized in that: In the step (2), the modified masterbatch is prepared by mixing modified multi-walled carbon nanotubes and poly(ethylene-co-methyl acrylate-co-glycidyl methacrylate) in a mass ratio of 1:(3.5-4.5), and extruding at 180-210° C. and a rotation speed of 150-200 rpm to obtain the modified masterbatch.

7. The method for preparing the die-cutting resistant self-adhesive glass cover protective film according to claim 1, characterized in that: In the step (2), the preparation method of the modified multi-walled carbon nanotubes is as follows: multi-walled carbon nanotubes and benzyl acetic acid are mixed in a mass ratio of 1:(0.8-1.2), and ball milled for 40-80 minutes at a ball-to-material ratio of (900-1000):1 and a rotation speed of 250-350 rpm to obtain modified multi-walled carbon nanotubes.

8. The method for preparing the die-cutting resistant self-adhesive glass cover protective film according to claim 1, characterized in that: In the step (3), the contents of the components in the self-adhesive layer mixture are, by weight, 32-58 parts of low-density polyethylene and 16-35 parts of styrene-butadiene-styrene block copolymer.

9. The method for preparing the die-cutting resistant self-adhesive glass cover protective film according to claim 1, characterized in that: In the step (4), the thickness of the protective layer is 30-50 μm, the thickness of the intermediate layer is 20-40 μm, and the thickness of the self-adhesive layer is 15-35 μm; the film blowing conditions are: the head temperature is 170-210°C, the traction ratio is 4-6, and the blowing ratio is 2-5; the cooling method for cooling and shaping is air cooling, and the air cooling temperature is 5-20°C.

10. A die-cutting resistant self-adhesive glass cover protective film prepared by the method for preparing a die-cutting resistant self-adhesive glass cover protective film according to any one of claims 1 to 9.

Citation Information

Cited By

  • Polymer protective film and preparation method and application thereof

    CN119859475A

  • High-barrier flexible heating carbon crystal protective film

    CN120944464A