Automobile windshield glass sealant and preparation process thereof

By using materials and processes such as polyester polyols with specific ratios in automotive windshield sealants, sealants with high tensile strength and wear resistance are prepared, which solves the problem of cracking and water seepage of existing sealants. Improves service life and adhesion, and achieves stable sealing performance and noise reduction effect.

CN118956320APending Publication Date: 2024-11-15SHANGHAI DELIAN CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191535.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing automotive windshield sealants are prone to cracking, degradation of noise isolation performance and water seepage during use, resulting in short service life and insufficient adhesion to various materials.

Method used

Sealants are prepared in specific proportions using polyester polyols, liquid polyether polyols, polymethyltriethoxysilanes, composite modified acrylic resins, stearic acid, carbon black, fillers, antioxidants, isocyanates and catalysts. It is also prepared by a twin screw extruder and a reduced pressure distillation process to form a sealant with high tensile strength, elasticity and wear resistance.

Benefits of technology

It improves the cohesiveness and bonding properties of sealants, enhances the adhesion to various materials, extends the service life, ensures the stable sealing performance of automobile windshield, reduces noise and water penetration, and complies with green environmental protection standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956320A_ABST
    Figure CN118956320A_ABST
Patent Text Reader

Abstract

The invention discloses an automobile windshield glass sealant and a preparation process thereof, and relates to the technical field of sealants, and the automobile windshield glass sealant is prepared from the following components: polyester polyol, liquid polyether polyol, polymethyl triethoxysilane, composite modified acrylic resin, stearic acid, carbon black, a filler, an antioxidant, dimethyl thio toluenediamine, isocyanate and a catalyst. The sealant prepared by the invention not only can be applied to automobile windshields, but also can be applied to the field of building sealing. The sealant prepared by the invention has high tensile strength, excellent elasticity, wear resistance, oil resistance and cold resistance, when the sealant is used in an automobile windshield, an automobile can still keep stable sealing performance in various complex environments, and the environmental adaptability of the automobile is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sealants, in particular to a sealant for automobile windshields. Background Art

[0002] The car windshield plays a vital role in the vehicle. Its main function is to protect the occupants from the external environment such as wind, rain, dust, etc., while ensuring that the driver has a clear view during driving.

[0003] During driving, the windshield can prevent natural factors such as wind, sand, rain and snow from directly impacting the people in the car, ensuring the comfort and safety of the driver and passengers.

[0004] The windshields of modern cars are mostly made of laminated glass or regional tempered glass. These materials not only have sufficient strength, but also can effectively prevent light refraction, allowing the driver to obtain a clearer view of the front and improve driving safety.

[0005] A good windshield design can isolate the noise outside the car to a certain extent, create a quieter environment inside the car, and help the driver concentrate on driving.

[0006] It can be seen that the car windshield is one of the important components to ensure driving safety and improve the driving experience. The car windshield and the car are bonded and sealed with sealants. Therefore, the performance of the sealant used is directly related to the car windshield's function of isolating noise, water, etc. If the sealant cracks, not only the noise isolation performance of the car windshield will be greatly reduced, but also water seepage will easily occur. Therefore, it is necessary to improve the performance quality of the sealant to extend its service life.

[0007] Based on this, a car windshield sealant is provided to solve the existing technical problems. Summary of the invention

[0008] The purpose of the present invention is to provide an automobile windshield sealant and a preparation process thereof, so as to solve the deficiencies in the prior art.

[0009] The technical solution adopted by the present invention is as follows:

[0010] A car windshield sealant, comprising the following ingredients by weight: 60-65 parts of polyester polyol, 50-58 parts of liquid polyether polyol, 1-2 parts of polymethyltriethoxysilane, 10-13 parts of composite modified acrylic resin, 1-1.8 parts of stearic acid, 2-3 parts of carbon black, 1-1.8 parts of filler, 1-2 parts of antioxidant, 2-3 parts of dimethylthiotoluenediamine, 15-20 parts of isocyanate, and 1-1.2 parts of catalyst;

[0011] The antioxidant is antioxidant 1010;

[0012] Among them, the molecular weight of the liquid polyether polyol is 3500.

[0013] As a further technical solution, the preparation method of the composite modified acrylic resin is:

[0014] The modifier, nano silicon carbide and acrylic resin are sequentially added into a twin-screw extruder, melt-extruded to form a sheet, cooled to room temperature, and then the cooled sheet is crushed to obtain a composite modified acrylic resin;

[0015] Wherein, the mixing ratio of the modifier, nano silicon carbide and acrylic resin is: 3-5:10-14:70-80;

[0016] The process conditions of the twin-screw extruder are: the temperature of zone 1 is 125°C, the temperature of zone 2 is 130°C, the temperature of zone 3 is 140°C, the temperature of zone 4 is 150°C, and the temperature of zone 5 is 155°C.

[0017] As a further technical solution, the preparation method of the modifier is:

[0018] First, castor oil and thioethanol are added to a reactor in sequence, an inert gas is introduced into the reactor, the air in the reactor is exhausted, and then azobisisobutyronitrile is added, the temperature in the reactor is adjusted to 85° C., the reactor is stirred and reacted for 4 hours, and then the temperature is further increased to 102° C., the reaction is continued to be stirred for 3 hours, and then the temperature is lowered to 50° C., ethyl acetate is added to the reactor, stirred for 30 minutes, and then washed with water and dried to obtain a reaction material solution;

[0019] The reaction solution is subjected to reduced pressure distillation to remove ethyl acetate to obtain a modifier.

[0020] As a further technical solution, the castor oil and mercaptoethanol are mixed in a mass ratio of 5:1;

[0021] The castor oil and azobisisobutyronitrile are mixed in a mass ratio of 15:1.

[0022] As a further technical solution: the inert gas is nitrogen or neon.

[0023] As a further technical solution, the mass ratio of the added ethyl acetate to the castor oil is 1.2:1.

[0024] As a further technical solution: the filler is a mixture of nano calcium carbonate and nano silicon dioxide;

[0025] Among them, the mixing mass ratio of nano calcium carbonate and nano silicon dioxide is 2:1.

[0026] A preparation process of automobile windshield sealant comprises the following steps:

[0027] S1 weighs the components according to mass ratio: polyester polyol, liquid polyether polyol, polymethyltriethoxysilane, composite modified acrylic resin, antioxidant, dimethylthiotoluenediamine, isocyanate, and catalyst;

[0028] S2: polyester polyol, liquid polyether polyol, polymethyltriethoxysilane, stearic acid, carbon black, filler, and antioxidant are added to the reaction kettle in sequence, heated to 130°C, stirred for 40 minutes, and then the composite modified acrylic resin is added, and stirring is continued for 40 minutes;

[0029] Among them, the speed of heat preservation and stirring is 500r / min;

[0030] S3: Vacuum the reactor for 3 hours, then adjust the temperature to 120°C, add stearic acid, dimethylthiotoluene diamine, carbon black, and filler into the reactor, stir for 1 hour, then adjust the temperature to 112°C, add isocyanate into the reactor, stir for 10 minutes, then adjust the temperature in the reactor to 122°C, keep warm and stir for 30 minutes, finally add the catalyst, stir and react for 2 hours, and discharge the material to obtain;

[0031] Among them, the stirring speed is 800r / min;

[0032] Among them, evacuate to a vacuum degree of -0.01MPa.

[0033] As a further technical solution: the catalyst is stannous octoate.

[0034] Beneficial effects:

[0035] The sealant prepared by the invention can be applied not only to automobile windshields, but also to the field of building sealing.

[0036] The sealant prepared by the invention has high tensile strength, excellent elasticity, wear resistance, oil resistance and cold resistance. When used in a car windshield, the sealant can enable the car to maintain stable sealing performance in various complex environments, thereby broadening the environmental adaptability of the car.

[0037] The sealant prepared by the present invention has the advantage of wide material adaptability and can have good adhesion to various materials, especially to metal, glass, plastic and the like.

[0038] The sealant of the present invention will not generate harmful substances during and after curing, does not contain organic solvents, and will not volatilize organic matter, thus conforming to the contemporary green environmental protection theme.

[0039] When the sealant of the present invention is applied to a car windshield, it can ensure a firm connection between the windshield and the car body, effectively prevent loosening or falling off due to vibration or impact, and maintain stable sealing for a long time.

[0040] The present invention introduces a composite modified acrylic resin, and the functional groups on the acrylic resin can react chemically with the isocyanate groups (-NCO) in the polyurethane to form a strong chemical bond, thereby greatly enhancing the cohesive force and bonding performance of the prepared sealant.

[0041] By introducing the composite modified acrylic resin, the dispersion uniformity of the filler in the sealant system can be effectively improved, the occurrence of phase separation can be reduced, and the coordination of the various components in the sealant can be greatly improved, thereby forming a denser network structure during the curing process, thereby improving its air tightness.

[0042] The introduction of composite modified acrylic resin can also improve the mechanical properties of the sealant, including tensile strength and shear performance, so that it can better resist external stress and deformation and maintain the integrity of the sealant structure, thereby effectively ensuring the isolation between the interior and exterior of the car and achieving excellent noise reduction effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a statistical chart of the shear strength of each sample tested. DETAILED DESCRIPTION

[0044] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] Example 1

[0046] A preparation process of automobile windshield sealant comprises the following steps:

[0047] S1 weighs the following components by mass ratio: 60 parts of polyester polyol, 50 parts of liquid polyether polyol, 1 part of polymethyltriethoxysilane, 10 parts of composite modified acrylic resin, 1 part of stearic acid, 2 parts of carbon black, 1 part of filler, 1 part of antioxidant, 2 parts of dimethylthiotoluenediamine, 15 parts of isocyanate, and 1 part of catalyst;

[0048] The antioxidant is antioxidant 1010;

[0049] Among them, the molecular weight of the liquid polyether polyol is 3500.

[0050] The preparation method of the composite modified acrylic resin is as follows:

[0051] The modifier, nano silicon carbide and acrylic resin are sequentially added into a twin-screw extruder, melt-extruded to form a sheet, cooled to room temperature, and then the cooled sheet is crushed to obtain a composite modified acrylic resin;

[0052] Wherein, the mixing ratio of the modifier, nano silicon carbide and acrylic resin is: 3:10:70;

[0053] The process conditions of the twin-screw extruder are: the temperature of zone 1 is 125°C, the temperature of zone 2 is 130°C, the temperature of zone 3 is 140°C, the temperature of zone 4 is 150°C, and the temperature of zone 5 is 155°C.

[0054] The preparation method of the modifier is:

[0055] First, castor oil and thioethanol are added to a reactor in sequence, an inert gas is introduced into the reactor, the air in the reactor is exhausted, and then azobisisobutyronitrile is added, the temperature in the reactor is adjusted to 85° C., the reactor is stirred and reacted for 4 hours, and then the temperature is further increased to 102° C., the reaction is continued to be stirred for 3 hours, and then the temperature is lowered to 50° C., ethyl acetate is added to the reactor, stirred for 30 minutes, and then washed with water and dried to obtain a reaction material solution;

[0056] The reaction solution is subjected to reduced pressure distillation to remove ethyl acetate to obtain a modifier.

[0057] The mass ratio of castor oil and thioethanol is 5:1;

[0058] The castor oil and azobisisobutyronitrile are mixed in a mass ratio of 15:1.

[0059] The inert gas is nitrogen.

[0060] The mass ratio of ethyl acetate added to castor oil was 1.2:1.

[0061] The filler is a mixture of nano calcium carbonate and nano silicon dioxide;

[0062] The mixing mass ratio of nano calcium carbonate to nano silicon dioxide is 2:1;

[0063] S2: polyester polyol, liquid polyether polyol, polymethyltriethoxysilane, stearic acid, carbon black, filler, and antioxidant are added to the reaction kettle in sequence, heated to 130°C, stirred for 40 minutes, and then the composite modified acrylic resin is added, and stirring is continued for 40 minutes;

[0064] Among them, the speed of heat preservation and stirring is 500r / min;

[0065] S3: Vacuum the reactor for 3 hours, then adjust the temperature to 120°C, add stearic acid, dimethylthiotoluene diamine, carbon black, and filler into the reactor, stir for 1 hour, then adjust the temperature to 112°C, add isocyanate into the reactor, stir for 10 minutes, then adjust the temperature in the reactor to 122°C, keep warm and stir for 30 minutes, finally add the catalyst, stir and react for 2 hours, and discharge the material to obtain;

[0066] Among them, the stirring speed is 800r / min;

[0067] Among them, evacuate to a vacuum degree of -0.01MPa.

[0068] The catalyst is stannous octoate.

[0069] Example 2

[0070] A preparation process of automobile windshield sealant comprises the following steps:

[0071] S1 weighs the following components by mass ratio: 62 parts of polyester polyol, 53 parts of liquid polyether polyol, 1.5 parts of polymethyltriethoxysilane, 12 parts of composite modified acrylic resin, 1.2 parts of stearic acid, 2.5 parts of carbon black, 1.3 parts of filler, 1.5 parts of antioxidant, 2.6 parts of dimethylthiotoluenediamine, 16 parts of isocyanate, and 1.1 parts of catalyst;

[0072] The antioxidant is antioxidant 1010;

[0073] Among them, the molecular weight of the liquid polyether polyol is 3500.

[0074] The preparation method of the composite modified acrylic resin is as follows:

[0075] The modifier, nano silicon carbide and acrylic resin are sequentially added into a twin-screw extruder, melt-extruded to form a sheet, cooled to room temperature, and then the cooled sheet is crushed to obtain a composite modified acrylic resin;

[0076] Wherein, the mixing ratio of the modifier, nano silicon carbide and acrylic resin is: 3.5:12:75;

[0077] The process conditions of the twin-screw extruder are: the temperature of zone 1 is 125°C, the temperature of zone 2 is 130°C, the temperature of zone 3 is 140°C, the temperature of zone 4 is 150°C, and the temperature of zone 5 is 155°C.

[0078] The preparation method of the modifier is:

[0079] First, castor oil and thioethanol are added to a reactor in sequence, an inert gas is introduced into the reactor, the air in the reactor is exhausted, and then azobisisobutyronitrile is added, the temperature in the reactor is adjusted to 85° C., the reactor is stirred and reacted for 4 hours, and then the temperature is further increased to 102° C., the reaction is continued to be stirred for 3 hours, and then the temperature is lowered to 50° C., ethyl acetate is added to the reactor, stirred for 30 minutes, and then washed with water and dried to obtain a reaction material solution;

[0080] The reaction solution is subjected to reduced pressure distillation to remove ethyl acetate to obtain a modifier.

[0081] The mass ratio of castor oil and thioethanol is 5:1;

[0082] The castor oil and azobisisobutyronitrile are mixed in a mass ratio of 15:1.

[0083] The inert gas is nitrogen.

[0084] The mass ratio of ethyl acetate added to castor oil was 1.2:1.

[0085] The filler is a mixture of nano calcium carbonate and nano silicon dioxide;

[0086] The mixing mass ratio of nano calcium carbonate to nano silicon dioxide is 2:1;

[0087] S2: polyester polyol, liquid polyether polyol, polymethyltriethoxysilane, stearic acid, carbon black, filler, and antioxidant are added to the reaction kettle in sequence, heated to 130°C, stirred for 40 minutes, and then the composite modified acrylic resin is added, and stirring is continued for 40 minutes;

[0088] Among them, the speed of heat preservation and stirring is 500r / min;

[0089] S3: Vacuum the reactor for 3 hours, then adjust the temperature to 120°C, add stearic acid, dimethylthiotoluene diamine, carbon black, and filler into the reactor, stir for 1 hour, then adjust the temperature to 112°C, add isocyanate into the reactor, stir for 10 minutes, then adjust the temperature in the reactor to 122°C, keep warm and stir for 30 minutes, finally add the catalyst, stir and react for 2 hours, and discharge the material to obtain;

[0090] Among them, the stirring speed is 800r / min;

[0091] Among them, evacuate to a vacuum degree of -0.01MPa.

[0092] The catalyst is stannous octoate.

[0093] Example 3

[0094] A preparation process of automobile windshield sealant comprises the following steps:

[0095] S1 weighs the following components by mass ratio: 63 parts of polyester polyol, 54 parts of liquid polyether polyol, 1.6 parts of polymethyltriethoxysilane, 12 parts of composite modified acrylic resin, 1.5 parts of stearic acid, 2.8 parts of carbon black, 1.1 parts of filler, 1.5 parts of antioxidant, 2.4 parts of dimethylthiotoluenediamine, 18 parts of isocyanate, and 1.2 parts of catalyst;

[0096] The antioxidant is antioxidant 1010;

[0097] Among them, the molecular weight of the liquid polyether polyol is 3500.

[0098] The preparation method of the composite modified acrylic resin is as follows:

[0099] The modifier, nano silicon carbide and acrylic resin are sequentially added into a twin-screw extruder, melt-extruded to form a sheet, cooled to room temperature, and then the cooled sheet is crushed to obtain a composite modified acrylic resin;

[0100] Wherein, the mixing ratio of the modifier, nano silicon carbide and acrylic resin is: 4:13:76;

[0101] The process conditions of the twin-screw extruder are: the temperature of zone 1 is 125°C, the temperature of zone 2 is 130°C, the temperature of zone 3 is 140°C, the temperature of zone 4 is 150°C, and the temperature of zone 5 is 155°C.

[0102] The preparation method of the modifier is:

[0103] First, castor oil and thioethanol are added to a reactor in sequence, an inert gas is introduced into the reactor, the air in the reactor is exhausted, and then azobisisobutyronitrile is added, the temperature in the reactor is adjusted to 85° C., the reactor is stirred and reacted for 4 hours, and then the temperature is further increased to 102° C., the reaction is continued to be stirred for 3 hours, and then the temperature is lowered to 50° C., ethyl acetate is added to the reactor, stirred for 30 minutes, and then washed with water and dried to obtain a reaction material solution;

[0104] The reaction solution is subjected to reduced pressure distillation to remove ethyl acetate to obtain a modifier.

[0105] The mass ratio of castor oil and thioethanol is 5:1;

[0106] The castor oil and azobisisobutyronitrile are mixed in a mass ratio of 15:1.

[0107] The inert gas is nitrogen.

[0108] The mass ratio of ethyl acetate added to castor oil was 1.2:1.

[0109] The filler is a mixture of nano calcium carbonate and nano silicon dioxide;

[0110] The mixing mass ratio of nano calcium carbonate to nano silicon dioxide is 2:1;

[0111] S2: polyester polyol, liquid polyether polyol, polymethyltriethoxysilane, stearic acid, carbon black, filler, and antioxidant are added to the reaction kettle in sequence, heated to 130°C, stirred for 40 minutes, and then the composite modified acrylic resin is added, and stirring is continued for 40 minutes;

[0112] Among them, the speed of heat preservation and stirring is 500r / min;

[0113] S3: Vacuum the reactor for 3 hours, then adjust the temperature to 120°C, add stearic acid, dimethylthiotoluene diamine, carbon black, and filler into the reactor, stir for 1 hour, then adjust the temperature to 112°C, add isocyanate into the reactor, stir for 10 minutes, then adjust the temperature in the reactor to 122°C, keep warm and stir for 30 minutes, finally add the catalyst, stir and react for 2 hours, and discharge the material to obtain;

[0114] Among them, the stirring speed is 800r / min;

[0115] Among them, evacuate to a vacuum degree of -0.01MPa.

[0116] The catalyst is stannous octoate.

[0117] Example 4

[0118] A preparation process of automobile windshield sealant comprises the following steps:

[0119] S1 weighs the following components by mass ratio: 64 parts of polyester polyol, 52 parts of liquid polyether polyol, 1.5 parts of polymethyltriethoxysilane, 12 parts of composite modified acrylic resin, 1.8 parts of stearic acid, 2 parts of carbon black, 1.8 parts of filler, 2 parts of antioxidant, 2.5 parts of dimethylthiotoluenediamine, 18 parts of isocyanate, and 1.1 parts of catalyst;

[0120] The antioxidant is antioxidant 1010;

[0121] Among them, the molecular weight of the liquid polyether polyol is 3500.

[0122] The preparation method of the composite modified acrylic resin is as follows:

[0123] The modifier, nano silicon carbide and acrylic resin are sequentially added into a twin-screw extruder, melt-extruded to form a sheet, cooled to room temperature, and then the cooled sheet is crushed to obtain a composite modified acrylic resin;

[0124] Wherein, the mixing ratio of the modifier, nano silicon carbide and acrylic resin is: 4.5:12:75;

[0125] The process conditions of the twin-screw extruder are: the temperature of zone 1 is 125°C, the temperature of zone 2 is 130°C, the temperature of zone 3 is 140°C, the temperature of zone 4 is 150°C, and the temperature of zone 5 is 155°C.

[0126] The preparation method of the modifier is:

[0127] First, castor oil and thioethanol are added to a reactor in sequence, an inert gas is introduced into the reactor, the air in the reactor is exhausted, and then azobisisobutyronitrile is added, the temperature in the reactor is adjusted to 85° C., the reactor is stirred and reacted for 4 hours, and then the temperature is further increased to 102° C., the reaction is continued to be stirred for 3 hours, and then the temperature is lowered to 50° C., ethyl acetate is added to the reactor, stirred for 30 minutes, and then washed with water and dried to obtain a reaction material solution;

[0128] The reaction solution is subjected to reduced pressure distillation to remove ethyl acetate to obtain a modifier.

[0129] The mass ratio of castor oil and thioethanol is 5:1;

[0130] The castor oil and azobisisobutyronitrile are mixed in a mass ratio of 15:1.

[0131] The inert gas is nitrogen or neon.

[0132] The mass ratio of ethyl acetate added to castor oil was 1.2:1.

[0133] The filler is a mixture of nano calcium carbonate and nano silicon dioxide;

[0134] The mixing mass ratio of nano calcium carbonate to nano silicon dioxide is 2:1;

[0135] S2: polyester polyol, liquid polyether polyol, polymethyltriethoxysilane, stearic acid, carbon black, filler, and antioxidant are added to the reaction kettle in sequence, heated to 130°C, stirred for 40 minutes, and then the composite modified acrylic resin is added, and stirring is continued for 40 minutes;

[0136] Among them, the speed of heat preservation and stirring is 500r / min;

[0137] S3: Vacuum the reactor for 3 hours, then adjust the temperature to 120°C, add stearic acid, dimethylthiotoluene diamine, carbon black, and filler into the reactor, stir for 1 hour, then adjust the temperature to 112°C, add isocyanate into the reactor, stir for 10 minutes, then adjust the temperature in the reactor to 122°C, keep warm and stir for 30 minutes, finally add the catalyst, stir and react for 2 hours, and discharge the material to obtain;

[0138] Among them, the stirring speed is 800r / min;

[0139] Among them, evacuate to a vacuum degree of -0.01MPa.

[0140] The catalyst is stannous octoate.

[0141] Example 5

[0142] A preparation process of automobile windshield sealant comprises the following steps:

[0143] S1 weighs the following components by mass ratio: 65 parts of polyester polyol, 58 parts of liquid polyether polyol, 2 parts of polymethyltriethoxysilane, 13 parts of composite modified acrylic resin, 1.8 parts of stearic acid, 3 parts of carbon black, 1.8 parts of filler, 2 parts of antioxidant, 3 parts of dimethylthiotoluenediamine, 20 parts of isocyanate, and 1.2 parts of catalyst;

[0144] The antioxidant is antioxidant 1010;

[0145] Among them, the molecular weight of the liquid polyether polyol is 3500.

[0146] The preparation method of the composite modified acrylic resin is as follows:

[0147] The modifier, nano silicon carbide and acrylic resin are sequentially added into a twin-screw extruder, melt-extruded to form a sheet, cooled to room temperature, and then the cooled sheet is crushed to obtain a composite modified acrylic resin;

[0148] Wherein, the mixing ratio of the modifier, nano silicon carbide and acrylic resin is: 5:14:80;

[0149] The process conditions of the twin-screw extruder are: the temperature of zone 1 is 125°C, the temperature of zone 2 is 130°C, the temperature of zone 3 is 140°C, the temperature of zone 4 is 150°C, and the temperature of zone 5 is 155°C.

[0150] The preparation method of the modifier is:

[0151] First, castor oil and thioethanol are added to a reactor in sequence, an inert gas is introduced into the reactor, the air in the reactor is exhausted, and then azobisisobutyronitrile is added, the temperature in the reactor is adjusted to 85° C., the reactor is stirred and reacted for 4 hours, and then the temperature is further increased to 102° C., the reaction is continued to be stirred for 3 hours, and then the temperature is lowered to 50° C., ethyl acetate is added to the reactor, stirred for 30 minutes, and then washed with water and dried to obtain a reaction material solution;

[0152] The reaction solution is subjected to reduced pressure distillation to remove ethyl acetate to obtain a modifier.

[0153] The mass ratio of castor oil and thioethanol is 5:1;

[0154] The castor oil and azobisisobutyronitrile are mixed in a mass ratio of 15:1.

[0155] The inert gas is nitrogen.

[0156] The mass ratio of ethyl acetate added to castor oil was 1.2:1.

[0157] The filler is a mixture of nano calcium carbonate and nano silicon dioxide;

[0158] The mixing mass ratio of nano calcium carbonate to nano silicon dioxide is 2:1;

[0159] S2: polyester polyol, liquid polyether polyol, polymethyltriethoxysilane, stearic acid, carbon black, filler, and antioxidant are added to the reaction kettle in sequence, heated to 130°C, stirred for 40 minutes, and then the composite modified acrylic resin is added, and stirring is continued for 40 minutes;

[0160] Among them, the speed of heat preservation and stirring is 500r / min;

[0161] S3: Vacuum the reactor for 3 hours, then adjust the temperature to 120°C, add stearic acid, dimethylthiotoluene diamine, carbon black, and filler into the reactor, stir for 1 hour, then adjust the temperature to 112°C, add isocyanate into the reactor, stir for 10 minutes, then adjust the temperature in the reactor to 122°C, keep warm and stir for 30 minutes, finally add the catalyst, stir and react for 2 hours, and discharge the material to obtain;

[0162] Among them, the stirring speed is 800r / min;

[0163] Among them, evacuate to a vacuum degree of -0.01MPa.

[0164] The catalyst is stannous octoate.

[0165] Comparative Example 1:

[0166] Based on Example 1, no composite modified acrylic resin is added, and the rest of the technical solutions remain unchanged.

[0167] Comparative Example 2:

[0168] Based on Example 1, the composite modified acrylic resin is replaced by untreated acrylic resin, and the rest of the technical solutions remain unchanged.

[0169] test:

[0170] The shear strength of the samples of the embodiment and the comparative example was tested after curing: the test was carried out in accordance with the GB / T 24498-2009 standard.

[0171] The bonding substrates used were glass and 304 stainless steel. The shear strength of the bonded materials was tested using an electronic universal testing machine. The glue coating area was 20 mm × 10 mm, and the shear rate was 5 mm / min.

[0172] The sample was tested after being left at 23℃ and 55%RH for 7 days:

[0173] Table 1

[0174] Shear strength / MPa Example 1 0.86 Example 2 0.85 Example 3 0.93 Example 4 0.81 Example 5 0.92 Comparative Example 1 0.61 Comparative Example 2 0.68

[0175] It can be seen from Table 1 that the sealant prepared by the present invention has a higher shear strength.

[0176] Tensile strength and elongation at break: measured in accordance with GB / T 13477.8-2017. The sample was tested after standing for 7 days at 23°C and 55% RH:

[0177] Table 2

[0178] Tensile strength MPa Example 1 6.14 Example 2 6.23 Example 3 6.18 Example 4 6.11 Example 5 6.05 Comparative Example 1 4.13 Comparative Example 2 4.96

[0179] It can be seen from Table 2 that the sealant prepared by the present invention has excellent tensile properties. The water vapor transmission rates of the examples and comparative samples were tested with reference to JC / T914-2014; the samples were tested after standing for 7 days under the environmental conditions of 23°C and 55% RH:

[0180] Table 3

[0181]

[0182]

[0183] It can be seen from Table 3 that the sealant prepared in the present invention has excellent sealing performance.

[0184] According to GB 16776-2005, the UV aging test was carried out on the samples of the embodiment and the comparative example. Under the xenon lamp or equivalent light source conforming to GB / T 16422.2, the irradiation intensity in the wavelength range of 300nm to 400nm should be (60±5)W / m 2 , the irradiation time is 1008 hours, and after aging, the water vapor transmission rate is tested;

[0185] The sample was tested after being left at 23°C and 55% RH for 7 days:

[0186] Table 4

[0187] <![CDATA[Water vapor transmission rate g / m 2 ·d]]> Example 1 0.312 Example 2 0.308 Example 3 0.303 Example 4 0.315 Example 5 0.310 Comparative Example 1 0.736 Comparative Example 2 0.614

[0188] It can be seen from Table 4 that after a long period of aging treatment, the sealant prepared by the present invention has excellent aging resistance.

[0189] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.

Claims

1. A car windshield sealant, characterized in that: The composition comprises the following ingredients by weight: 60-65 parts of polyester polyol, 50-58 parts of liquid polyether polyol, 1-2 parts of polymethyltriethoxysilane, 10-13 parts of composite modified acrylic resin, 1-1.8 parts of stearic acid, 2-3 parts of carbon black, 1-1.8 parts of filler, 1-2 parts of antioxidant, 2-3 parts of dimethylthiotoluenediamine, 15-20 parts of isocyanate, and 1-1.2 parts of catalyst; The antioxidant is antioxidant 1010; Among them, the molecular weight of the liquid polyether polyol is 3500.

2. The automobile windshield sealant according to claim 1, characterized in that: The composite modified acrylic resin preparation method is: The modifier, nano silicon carbide and acrylic resin are sequentially added into a twin-screw extruder, melt-extruded to form a sheet, cooled to room temperature, and then the cooled sheet is crushed to obtain a composite modified acrylic resin; Wherein, the mixing ratio of the modifier, nano silicon carbide and acrylic resin is: 3-5:10-14:70-80; The process conditions of the twin-screw extruder are: the temperature of zone 1 is 125°C, the temperature of zone 2 is 130°C, the temperature of zone 3 is 140°C, the temperature of zone 4 is 150°C, and the temperature of zone 5 is 155°C.

3. The automobile windshield sealant according to claim 2, characterized in that: The preparation method of the modifier is: First, castor oil and thioethanol are added to a reactor in sequence, an inert gas is introduced into the reactor, the air in the reactor is exhausted, and then azobisisobutyronitrile is added, the temperature in the reactor is adjusted to 85° C., the reactor is stirred and reacted for 4 hours, and then the temperature is further increased to 102° C., the reaction is continued to be stirred for 3 hours, and then the temperature is lowered to 50° C., ethyl acetate is added to the reactor, stirred for 30 minutes, and then washed with water and dried to obtain a reaction material solution; The reaction solution is subjected to reduced pressure distillation to remove ethyl acetate to obtain a modifier.

4. The automobile windshield sealant according to claim 3, characterized in that: The castor oil and mercaptoethanol mixed mass ratio is 5:1; The castor oil and azobisisobutyronitrile are mixed in a mass ratio of 15:

1.

5. The automobile windshield sealant according to claim 3, characterized in that: The inert gas is nitrogen or neon.

6. The automobile windshield sealant according to claim 3, characterized in that: The mass ratio of the added ethyl acetate to the castor oil is 1.2:

1.

7. The automobile windshield sealant according to claim 3, characterized in that: The filler is a mixture of nano calcium carbonate and nano silicon dioxide; Among them, the mixing mass ratio of nano calcium carbonate and nano silicon dioxide is 2:

1.

8. The process for preparing a car windshield sealant according to claim 1, characterized in that: The following steps are involved: S1 weighs the components according to mass ratio: polyester polyol, liquid polyether polyol, polymethyltriethoxysilane, composite modified acrylic resin, antioxidant, dimethylthiotoluenediamine, isocyanate, and catalyst; S2: polyester polyol, liquid polyether polyol, polymethyltriethoxysilane, stearic acid, carbon black, filler, and antioxidant are added to the reaction kettle in sequence, heated to 130°C, stirred for 40 minutes, and then the composite modified acrylic resin is added, and stirring is continued for 40 minutes; Among them, the speed of heat preservation and stirring is 500r / min; S3: Vacuum the reactor for 3 hours, then adjust the temperature to 120°C, add stearic acid, dimethylthiotoluene diamine, carbon black, and filler into the reactor, stir for 1 hour, then adjust the temperature to 112°C, add isocyanate into the reactor, stir for 10 minutes, then adjust the temperature in the reactor to 122°C, keep warm and stir for 30 minutes, finally add the catalyst, stir and react for 2 hours, and discharge the material to obtain; Among them, the stirring speed is 800r / min; Among them, evacuate to a vacuum degree of -0.01MPa.