Double-network structure binder for silicon-based negative electrode of lithium ion battery as well as preparation method and application of double-network structure binder

By using dual network structure adhesive in the silicon-based anode of lithium-ion batteries, a complex crosslinking structure is formed through hydrogen bond crosslinking, the problem of poor mechanical properties of a single linear structure adhesive is solved, and the cycle stability of the battery is significantly improved and capacity retention rate, extending battery life.

CN118956338AActive Publication Date: 2024-11-15GUANGDONG UNIV OF TECH

Patent Information

Application Number
CN202411050711.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Due to poor mechanical properties, the single linear structure adhesive of silicon-based negative electrode of existing lithium-ion batteries is difficult to withstand the volume expansion of silicon oxygen particles during charging and discharging, resulting in unstable electrode structure and degradation of electrochemical performance.

Method used

Using dual network structure adhesive, the high elastic soft network LT is introduced into the hard network SG, and a complex crosslinking structure is formed through hydrogen bond crosslinking, providing higher mechanical properties and self-healing ability, effectively suppressing electrode volume Expansion.

Benefits of technology

The cycle stability and battery capacity retention rate of the silicon-based negative electrode of lithium-ion batteries are significantly improved, the cycle life of the battery is extended, and the interface bonding ability with silicon particles is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956338A_ABST
    Figure CN118956338A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium batteries, and discloses a double-network-structure binder for a silicon-based negative electrode of a lithium ion battery and a preparation method and application of the double-network-structure binder. The adhesive with the double-network structure is abbreviated as SGLT and is prepared by dissolving sericin in water, adding glutaraldehyde and an HCl solution to prepare an SG solution, then adding tannic acid and lipoic acid, carrying out in-situ polymerization at 120-180 DEG C, and enabling the tannic acid and the lipoic acid to form network LT based on a network SG. According to the invention, the hard network SG is formed through crosslinking, then the network LT is formed based on the network SG, and the hard network SG is used as a stable skeleton, so that the volume expansion of the electrode structure is effectively inhibited. The high-elasticity soft LT network serves as a buffer layer, and stress generated by volume expansion in the electrode is relieved. The binder has excellent mechanical properties, effectively inhibits the volume expansion of the SiOx negative electrode in the charge-discharge cycle process, and ensures the cycle stability of the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium batteries, and in particular, relates to a double network structure binder for a silicon-based negative electrode of a lithium ion battery, and a preparation method and application thereof. Background Art

[0002] With the development of new energy electric vehicles, the development of high specific energy, high power and long life negative electrode materials has become one of the research hotspots of lithium-ion batteries. At present, the negative electrode material of commercial lithium-ion batteries is mainly graphite, and its theoretical specific capacity is only 372mAh / g. Among them, silicon oxide (SiO2) with high theoretical specific capacity (2600mAh / g) and low working voltage is the most popular. x ) negative electrode materials have attracted much attention. However, in the reversible process of lithium removal and lithium insertion, SiO x The material will experience significant volume expansion and form an unstable solid electrolyte interface film (SEI film), leading to problems such as silicon oxide particle rupture, destruction of the conductive network and battery capacity decay, which in turn affects the battery cycle life and capacity.

[0003] Among many solutions, optimizing binders has been proven to be an economical and efficient approach. The traditional binder polyvinylidene fluoride (PVDF) is not suitable for silicon-based negative electrodes because of its weak van der Waals force with silicon and oxygen, and it is difficult to withstand the huge volume expansion of silicon-oxygen negative electrodes during charging and discharging. In addition, the silicon-based negative electrode binder with a single linear structure (such as a linear polymer chain) is prone to irreversible sliding during the continuous volume change of the silicon-oxygen negative electrode due to weak interchain interactions, which can lead to cracks in the pole piece and decreased electrochemical performance. The first choice for silicon-based negative electrode binders is elastic polymers, because silicon-based negative electrodes undergo huge volume changes during charging and discharging. The soft elastic polymer binder itself lacks sufficient rigidity, which causes the thickness of the silicon-based negative electrode to change significantly during charging and discharging. Plastic polymer binders can effectively constrain the volume change of silicon-based negative electrodes, stabilize the thickness of silicon-based negative electrodes, and thus maintain the electrode structure. Therefore, designing a binder with a multiple network composite structure will effectively alleviate the huge volume expansion problem of silicon-oxygen negative electrodes during charging and discharging, ensure the integrity of the electrode structure, and then ensure SiO x Electrochemical stability and cycling performance of the negative electrode. Summary of the invention

[0004] The present invention aims to solve the problem in the prior art that "the single linear structure silicon negative electrode binder is a linear polymer chain, the interaction between the chains is weak, the mechanical properties are poor, and irreversible sliding easily occurs during the continuous volume change of the silicon-oxygen negative electrode, which leads to cracks in the electrode piece and reduced electrochemical performance." The primary purpose is to provide a double network structure binder for lithium-ion battery silicon-based negative electrode. The binder forms a more complex and stable cross-linked structure by adding another complementary network to one network structure, which can effectively alleviate the SiO x The volume expansion problem of the negative electrode during the charge and discharge process. The hard network SG in the dual network acts as a stable skeleton to effectively suppress the volume expansion problem of the electrode structure. The highly elastic soft LT network acts as a buffer layer to relieve the stress generated by the volume expansion inside the electrode. The dual network structure binder has excellent mechanical properties, which can effectively suppress the SiO x The volume expansion of the negative electrode during the charge and discharge cycle ensures the cycle stability of the electrode.

[0005] Another object of the present invention is to provide a method for preparing the above-mentioned double network structure binder for lithium ion battery silicon-based negative electrode. The method forms a double network structure binder SGLT with elastic / plastic effect through hydrogen bond crosslinking of SG and LT.

[0006] Another object of the present invention is to provide an application of the above-mentioned double network structure binder for silicon-based negative electrodes of lithium-ion batteries.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] A double network structure binder for a silicon-based negative electrode of a lithium-ion battery, the double network structure binder is abbreviated as SGLT, and is prepared by first dissolving sericin in water, adding glutaraldehyde and HCl solution to obtain SG solution, then adding tannic acid and thioctic acid, and performing in-situ polymerization at 120-180° C. Tannic acid and thioctic acid form network LT based on network SG.

[0009] Preferably, the mass ratio of the sericin, glutaraldehyde, tannic acid and lipoic acid is 1:(0.062-0.125):(0.2-1):(0.01-0.04); the mass ratio of glutaraldehyde and HCl solution is (2-6):1.

[0010] Preferably, the mass ratio of the sericin to water is 1:(20-50); the molecular weight of the sericin is 2000-100000; and the concentration of the HCl solution is 10-16 mol / L.

[0011] Preferably, the in-situ polymerization time is 2 to 4 hours.

[0012] The preparation method of the double-network structure binder for the silicon-based anode of a lithium-ion battery includes the following steps:

[0013] S1. Stir sericin in water, then add glutaraldehyde and a group activator to carry out a cross-linking reaction to obtain an SG solution;

[0014] S2. Add tannic acid and lipoic acid to the SG solution, and carry out in-situ polymerization at 120-180 °C. Tannic acid and lipoic acid form a network LT based on the network SG to obtain a binder with a double-network structure.

[0015] A negative electrode is prepared by mixing the double-network structure binder, an active substance SiO x , where 0 < x < 2, a conductive agent, and water, then stirring with water to obtain a uniformly dispersed electrode paste. Coating the electrode paste on a copper foil and carrying out in-situ polymerization at 120-180 °C, and drying.

[0016] Preferably, the conductive agent is conductive carbon black, carbon nanotubes, or conductive graphite; the mass ratio of the active substance SiO x , the conductive agent, and the double-network structure binder is (7-8):(1-2):1; the stirring time is 6-8 h, the drying temperature is 60-80 °C, and the drying time is 12-36 h.

[0017] The application of the negative electrode in a lithium-ion battery.

[0018] In the present invention, since sericin rich in polar amino acids has hydrophilicity and residue sites that are easily modified, it is relatively uniformly distributed when dissolved in water; glutaraldehyde is a homobifunctional cross-linking agent, which is easily soluble in water and can be used as a protein cross-linking agent. The cross-linking characteristics are high activity, fast reaction, high binding amount, and stable product. Lipoic acid is a biomolecule with a special structure, including two types of dynamic bonds: the dynamic covalent disulfide bond in the five-membered ring and the non-covalent hydrogen bond of the carboxyl group. The double-network structure binder utilizes non-covalent interactions between molecules, such as hydrogen bonds, van der Waals forces, and ionic interactions, etc., to achieve an efficient adhesion effect. Through hydrogen bond cross-linking of the SG network and the LT network, a binder SGLT with a double-network structure is formed, improving the mechanical strength of the binder and realizing the cycle stability of the silicon-based anode.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The binder SGLT of the present invention has a double-network structure with elastic / plastic effects. This is because tannic acid and lipoic acid form a network LT based on the network SG, and a double-network structure is formed through a hydrogen bond cross-linking reaction. The interaction between the network SG and the network LT has higher mechanical properties, enabling the electrode to maintain good integrity during cycling.

[0021] 2. The double network structure adhesive of the present invention and SiO x There are abundant binding sites between particles, making the binder x The particles have strong interfacial bonding ability, SiO x The negative electrode can better withstand the volume change during the charge and discharge process of the electrode, and the two networks are cross-linked by hydrogen bonds. Therefore, due to the self-healing properties, bonding ability and mechanical strength of the binder, it is suitable for SiO x The negative electrode achieved stable long-cycle performance.

[0022] 3. The lipoic acid in the double network structure binder of the present invention contains a reversible dynamic covalent disulfide bond, which can be reformed after breaking. The double network structure formed by cross-linking the two networks with each other through hydrogen bonds can maximize the mechanical properties of the binder and effectively inhibit the SiO2 formation during the charge and discharge process of the electrode. x The volume expansion of the negative electrode material makes SiO x The negative electrode exhibits good cycling stability.

[0023] 4. The tannic acid and lipoic acid of the present invention are cross-linked to form a highly elastic soft network LT, which is combined with sericin, glutaraldehyde solution and hydrochloric acid to form a hard network SG. The hard network SG acts as a stable skeleton to effectively suppress the volume expansion of the electrode structure. The highly elastic soft network LT acts as a buffer layer to relieve the stress generated by the volume expansion inside the electrode. The dual network structure binder has excellent mechanical properties, which can effectively suppress the SiO x The volume expansion of the negative electrode during the charge and discharge cycle ensures the cycle stability of the electrode. The double network structure binder not only provides stronger mechanical strength and elasticity, but also enhances the bonding force between silicon particles and current collectors, thereby significantly improving the cycle life and capacity retention of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a comparison chart of the cycle performance of button batteries of Application Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0025] The content of the present invention is further described below in conjunction with specific examples, but it should not be construed as limiting the present invention. If not specifically indicated, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0026] Example 1

[0027] 1. Dissolve 0.15 g of sericin protein with a molecular weight of 2000 in 4.85 g of water by magnetic stirring, then add 0.0334 g of 50 wt% glutaraldehyde aqueous solution and 50 μL of 12 mol / L hydrochloric acid, and stir and react for 1 h to obtain a 5 wt% SG solution;

[0028] 2. Add 9.62 mg of lipoic acid and 0.38 mg of tannic acid to 200 mL of 5 wt% SG solution, and carry out in-situ polymerization at 150 °C for 2 h. Tannic acid and lipoic acid form a network LT based on the network SG to obtain a binder with a double-network structure, abbreviated as SGLT.

[0029] Example 2

[0030] 1. Dissolve 0.25 g of sericin protein with a molecular weight of 2000 in 4.75 g of water by magnetic stirring, then add 0.05 g of 50% wt glutaraldehyde aqueous solution and 50 μL of 12 mol / L hydrochloric acid, and stir and react for 1 h to obtain a 5 wt% network SG solution;

[0031] 2. Add 9.62 mg of lipoic acid and 0.38 mg of tannic acid to 200 mL of 5 wt% SG solution, and carry out in-situ polymerization at 150 °C for 2 h. Tannic acid and lipoic acid form a network LT based on the network SG to obtain a binder with a double-network structure, abbreviated as SGLT.

[0032] Comparative Example 1

[0033] Add 0.15 g of sericin protein with a molecular weight of 2000 to 4.85 g of water, then add 0.05 g of 50 wt% glutaraldehyde aqueous solution and 50 μL of 12 mol / L hydrochloric acid, and stir and react for 1 h to obtain a 5 wt% SG binder.

[0034] Application Example 1

[0035] 1. Add 9.62 mg of lipoic acid and 0.38 mg of tannic acid in the preparation process of the binder SGLT in Example 1 to 200 mL of 5 wt% SG solution, and put it into a defoaming blender with the active substance SiO x (0 < x < 2) and the conductive agent Super P and stir to obtain a uniformly dispersed electrode paste;

[0036] 2. Coating the electrode paste on the copper foil and carrying out in-situ cross-linking reaction at 150 °C for 2 h to obtain a pole piece with a binder having a double-network structure.

[0037] 3. The dried electrode sheet of Example 1 was cut into a circular shape with a diameter of 12 mm as the negative electrode sheet, and transferred into a glove box filled with argon gas, with a lithium sheet as the counter electrode, and an electrolyte (10 wt% of fluoroethylene carbonate (FEC) and 1 wt% of vinylene carbonate (VC) as additives, 1 mmol / L of LiPF6 dissolved in ethylene carbonate (DEC) and diethyl carbonate (EC), wherein the volume ratio of DEC to EC was 1:1). Assemble into a CR2032 button cell, abbreviated as SGLT@SiO x (0 <x<2)。

[0038] Application Example 2

[0039] 1. Add 9.62 mg of lipoic acid and 0.38 mg of tannic acid in the preparation process of the binder SGLT in Example 2 to 200 mL of 5 wt% SG solution and mix with the active substance SiO x Put the conductive agent Super P into a deaerator and stir to obtain a uniformly dispersed electrode slurry;

[0040] 2. The electrode slurry was coated onto copper foil and subjected to in-situ cross-linking reaction at 150° C. for 2 h to obtain an electrode having a dual network structure binder (SGLT).

[0041] Application Comparative Example 1

[0042] 1. Mix the active material SiO in a mass ratio of 7:2:1 x , the conductive agent SupperP was mixed with 5wt% of the SG binder of Comparative Example 1, and 200μL of water was added and mixed and stirred for 6h to obtain a uniformly dispersed electrode slurry;

[0043] 2. The electrode slurry was coated onto copper foil, vacuum dried at 80°C for 12 h, and cut into circular electrodes with a diameter of 12 mm.

[0044] 3. The dried electrode was transferred into an argon-filled glove box, and a lithium sheet was used as the counter electrode, and an electrolyte (10 wt% of fluoroethylene carbonate (FEC) and 1 wt% of vinylene carbonate (VC) as additives, 1 mmol / L of LiPF6 was dissolved in ethylene carbonate (DEC) and diethyl carbonate (EC), where the volume ratio of DEC to EC was 1:1) was used to assemble a CR2032 button cell, abbreviated as SG@SiO x (0 <x<2)。

[0045] After the CR2032 button cells assembled in Application Example 1 and Comparative Example 1 were left to stand at 28°C for 10 hours, the electrochemical performance was tested by constant current in the Xinwei test system. The test conditions were: current density 400mA / g; voltage window 0.01-1.5V. Figure 1The figure is a comparison of the cycle performance of the CR2032 button-type battery assembled in Application Example 1 and Comparative Example 1. Figure 1 It can be seen that the button battery of comparative example 1 has a discharge capacity decay of 681 mAh / g after 100 cycles at a current density of 400 mA / g, the button battery of application example 1 has an initial discharge specific capacity of more than 2100 mAh / g, an initial coulombic efficiency of more than 60%, and a capacity of 1061 mAh / g after 100 cycles, which has a higher discharge capacity and better cycle stability. The results show that the dual network structure binder SGLT of the present invention can make SiO x The negative electrode exhibits good cycle stability. In addition, the dual network structure binder not only provides stronger mechanical strength and elasticity, but also enhances the bonding force between silicon particles and current collectors, thereby significantly improving the cycle life and capacity retention of the battery.

[0046] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A double network structure binder for a silicon-based negative electrode of a lithium-ion battery, characterized in that: The double network structure adhesive is abbreviated as SGLT. The sericin is first dissolved in water, glutaraldehyde and HCl solution are added to obtain SG solution, and then tannic acid and lipoic acid are added to perform in-situ polymerization at 120-180° C. Tannic acid and lipoic acid form network LT based on network SG.

2. The double network structure binder for lithium ion battery silicon-based negative electrode according to claim 1, characterized in that: The mass ratio of the sericin, glutaraldehyde, tannic acid and lipoic acid is 1:(0.062-0.125):(0.2-1):(0.01-0.04); the mass ratio of glutaraldehyde and HCl solution is (2-6):

1.

3. The double network structure binder for lithium ion battery silicon-based negative electrode according to claim 1, characterized in that: The mass ratio of the sericin to water is 1:(20-50); the molecular weight of the sericin is 2000-100000; and the concentration of the HCl solution is 10-16 mol / L.

4. The double network structure binder for lithium ion battery silicon-based negative electrode according to claim 1, characterized in that: The time of the in-situ polymerization is 2 to 4 hours.

5. The method for preparing a double network structure binder for a silicon-based negative electrode of a lithium-ion battery according to any one of claims 1 to 4, characterized in that: The steps include: S1. Add water to sericin and stir, then add glutaraldehyde and a group activator to cause a cross-linking reaction to obtain an SG solution; S2. Add tannic acid and thioctic acid to the SG solution, and carry out in-situ polymerization at 120-180° C. Tannic acid and thioctic acid form a network LT based on the network SG, and obtain a double network structure adhesive through hydrogen bond cross-linking reaction.

6. A negative electrode, characterized in that: The negative electrode is prepared by mixing the double-network structure binder, active substance SiO x , where 0 < x < 2, conductive agent and water, and then adding water and stirring to obtain a uniformly dispersed electrode paste. The electrode paste is coated on a copper foil and subjected to in-situ polymerization at 120-180 °C and dried.

7. The negative electrode according to claim 6, characterized in that: The conductive agent is conductive carbon black, carbon nanotubes or conductive graphite; the active material SiO x , the mass ratio of the conductive agent and the double network structure binder is (7-8):(1-2):1; the stirring time is 6-8 hours, the drying temperature is 60-80°C, and the drying time is 12-36 hours.

8. Use of the negative electrode according to claim 6 or 7 in a lithium ion battery.

Citation Information

Patent Citations

  • Water-based adhesive and application thereof in lithium ion battery

    CN111969206A

  • Vegetable protein-based formaldehyde-free adhesive

    CN112063364A

  • Composite binder for silicon-based negative electrode of lithium ion battery as well as preparation method and application of composite binder

    CN113363482A

  • Solvent-free binder, and preparation method and application thereof

    CN113621342A

  • Supramolecular composite binder for silicon-based negative electrode of lithium ion battery as well as preparation method and application of supramolecular composite binder

    CN116914146A

Cited By

  • Electrode binder for rechargeable lithium battery, electrode, and rechargeable lithium battery manufactured using same

    EP4749696A1