Waterproof and leakproof phase change heat storage material, preparation method of phase change heat storage thermal insulation wallboard and flexible sunlight greenhouse

By modifying polyethylene glycol-based phase change materials through ring-opening and cross-linking, and combining them with inorganic porous materials, a multi-layered waterproof and leak-proof phase change heat storage material is formed. This solves the problems of leakage, expansion, and moisture intrusion of phase change materials in flexible greenhouses, achieving efficient temperature control and long-term stability. It is suitable for planting high-value-added fruits and vegetables during high-temperature seasons.

CN118956353APending Publication Date: 2024-11-15BEIJING FAIRVIEW NEW TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411106806.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The phase change heat storage materials in existing flexible solar greenhouses suffer from leakage, thermal expansion, moisture intrusion, and long-term stability issues, leading to decreased heat storage performance and structural damage, which cannot meet the needs of planting high-value-added fruits and vegetables during the high-temperature season.

Method used

A multi-layered waterproof and leak-proof phase change heat storage material is formed by using polyethylene glycol-based phase change materials through ring-opening and cross-linking modification, combined with inorganic porous materials and binders. The stability and thermal performance of the material are improved through chemical modification and physical encapsulation.

Benefits of technology

It significantly improves the chemical stability, mechanical properties, and thermal conductivity of phase change materials, reduces the risk of leakage, and ensures the long-term stability and heat storage effect of phase change heat storage plates, making them suitable for efficient temperature control in flexible greenhouses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956353A_ABST
    Figure CN118956353A_ABST
Patent Text Reader

Abstract

The invention relates to a waterproof leakproof phase change heat storage material. A preparation method of the waterproof leakproof phase change heat storage material comprises the following steps: preparing a hydroxylated phase change heat storage material by using a polyethylene glycol phase change heat storage material; preparing a cross-linked modified phase change heat storage material; preparing a phase change porous material loaded with the cross-linked modified phase change heat storage material; the calcium carbonate powder containing stearic acid and the fly ash adsorbing fatty acid are mixed and heated, the phase change porous material is added, uniform stirring and granulation are performed, and cooling is performed to obtain the product. Chemical groups with specific functions are introduced into the molecular structure of the polyethylene glycol type phase change heat storage material, so that the physical and chemical properties of the polyethylene glycol type phase change heat storage material are improved; a three-dimensional network structure is formed through cross-linking modification of PCM, so that the volume change of the PCM in the phase change process is limited, and the problems of structural stress concentration and cracking when the PCM is prepared into the phase change heat storage plate are solved; the phase-change porous material is granulated and wrapped by calcium carbonate powder containing stearic acid and fly ash adsorbing fatty acid, so that the adverse effect on the performance stability of the phase-change material when water invades is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a phase-change heat storage material, a heat-insulating wallboard and a solar greenhouse, and specifically relates to a waterproof and leak-proof phase-change heat storage material, a preparation method of a phase-change heat-storage and heat-insulating wallboard having the same, and a flexible solar greenhouse. Background Art

[0002] Cultivated land does not allow for walls required for construction, so when building greenhouses on cultivated land, more and more flexible insulation wall solar greenhouse structures are used. This structure is basically the same as an ordinary brick wall greenhouse, with a span of 9-12 meters, a maximum span of 18 meters, a ridge height of 5-6 meters, and a general orientation of 5-8 degrees south or south-east. It can protect cultivated land while allowing greenhouse planting. The flexible insulation wall solar greenhouse structure uses galvanized steel frames + insulation cotton to replace brick walls or earth walls. It is a light wall, a non-masonry building wall, with a thickness of 0.2-0.3 meters. The skeleton is generally a truss or elliptical tube skeleton, equipped with quilts, greenhouse film and winding equipment, and an active heat storage and release system. Compared with brick wall or earth wall greenhouses, the advantages are simple construction, low cost, fast heating, high land utilization rate (50%-65%), and easy mechanized operation; the disadvantages are relatively weak insulation, fast cooling, and a service life of about 10 years. It is only suitable for spring and autumn fruit and vegetable crops, winter leafy vegetables, strawberry production or seasonal seedling cultivation. However, they cannot grow solanaceous crops with high economic added value, and they cannot grow fruits and vegetables with high temperature requirements in winter. In addition, they cannot solve the practical problem that they cannot grow vegetables due to high temperatures in summer. Facility agriculture mainly targets off-season fruits and vegetables. This type of solar greenhouse can only grow vegetables earlier in spring and later in autumn. The core problem of facility agriculture is the energy problem. If the problem of heat storage is not solved, only leafy vegetables with little economic value can be grown in winter, and farmers cannot achieve stable income. This flexible insulation wall solar greenhouse is not suitable for off-season fruit and vegetable production in the three northern regions and has little economic value.

[0003] How to set up a flexible wall structure to solve the problem of heat storage and realize the cultivation of fruits and vegetables with high economic added value and temperature requirements is an urgent problem to be solved. The existing flexible solar greenhouse quilt wall has a 10cm-15cm extruded board (insulation reinforcement layer) laid between the inner keels. The extruded board is also a non-absorption interface without heat storage function, and the heat storage coefficient is close to 0. In this way, how to set a 10cm-15cm phase change heat storage layer / board on the extruded board and ensure its performance stability. The technical difficulties are (1) phase change material leakage: the phase change material may leak during multiple phase changes, resulting in a decrease in heat storage performance and damage to the material structure. The leakage of the phase change material directly affects the temperature and durability of the solar greenhouse of the present invention. It is also a common problem of phase change heat storage materials currently existing. (2) Thermal expansion problem: The volume of the phase change material changes during the phase change process, which may cause stress concentration and cracking of the 10cm-15cm phase change thermal storage layer (plate) structure; at the same time, the phase change material (PCM) undergoes changes in physical state during the storage and release of thermal energy. Some problems with PCM, such as volume changes and chemical instability during the phase change process, may cause material leakage and performance degradation. (3) The impact of moisture intrusion on the 10cm-15cm phase change thermal storage layer (plate): The interior of the solar greenhouse is a high humidity environment, and moisture intrusion may have an adverse effect on the performance and stability of the phase change material, especially in terms of material leakage. (4) Long-term stability and durability issues: The cyclic stability, mechanics and mechanical properties of the flexible solar greenhouse phase change thermal storage material of the present invention are key factors affecting the long-term stability and durability of the flexible solar greenhouse. Summary of the invention

[0004] The present invention aims to solve the technical problem of performance stability of a 10cm-15cm phase change heat storage layer / plate used for a flexible greenhouse wall, and provides a waterproof and leak-proof phase change heat storage material.

[0005] The technical solution of the present invention to solve the above technical problems is as follows: a waterproof and leak-proof phase change thermal storage material, comprising the following steps:

[0006] Step (1), dissolving a polyethylene glycol phase change thermal storage material in deionized water to form a uniform solution; adding a ring-opening catalyst and stirring evenly, slowly introducing a ring-opening reaction gas, and after the reaction is completed, adjusting the system to neutrality, washing with ethanol to remove unreacted impurities, and vacuum drying the product to obtain a hydroxylated phase change thermal storage material;

[0007] Step (2), dissolving the hydroxylated phase change thermal storage material obtained in step (1) in a solvent to obtain a solution, adding a crosslinking catalyst to the solution, stirring evenly, slowly adding a crosslinking agent in a stirring state, stirring evenly, completing the reaction, removing the solvent, adding an antioxidant and a stabilizer, stirring evenly, and obtaining a crosslinked modified phase change thermal storage material;

[0008] Step (3), adding an interface modifier to the inorganic porous material and mixing them evenly, heating and melting the cross-linked modified phase change thermal storage material obtained in step (2) at a temperature of 50-70° C. to become a liquid, adding a thermal conductive nano material and mixing them evenly, adding a binder to the mixed mixture and stirring them evenly, slowly stirring and adsorbing in a vacuum, and then cooling and solidifying naturally, thereby obtaining a phase change porous material loaded with the cross-linked modified phase change thermal storage material;

[0009] Step (4), mixing the calcium carbonate powder containing stearic acid and the fly ash adsorbing fatty acids and heating to 130-160°C, adding the phase change porous material obtained in step (3), stirring evenly and introducing into a disc granulator for granulation, and cooling to obtain a waterproof and leakproof phase change thermal storage material.

[0010] The beneficial effects of the present invention are: introducing chemical groups with specific functions into the molecular structure of polyethylene glycol phase change thermal storage materials to improve their physical and chemical properties; that is, carboxyl groups or hydroxyl groups can be introduced into polyethylene glycol (PEG) (PEG) to enhance its compatibility with other materials and phase change thermal performance; the present invention cross-links and modifies PCM to form a three-dimensional network structure through chemical reaction to limit its volume change during the phase change process, thereby solving the structural stress concentration and cracking problems when the phase change material is prepared into a phase change thermal storage plate; at the same time, the phase change porous material is granulated and wrapped by calcium carbonate powder containing stearic acid and fly ash adsorbing fatty acids, thereby preventing moisture from invading the phase change thermal storage plate and having an adverse effect on the performance and stability of the phase change material.

[0011] Based on the above technical solution, the present invention can also be improved as follows.

[0012] Furthermore, the calcium carbonate powder containing stearic acid is specifically prepared by: heating the light calcium carbonate powder and stearic acid at a constant temperature of 65-75° C., preferably at a constant temperature of 70° C., and continuously stirring and mixing, and stopping when a uniform layer of stearic acid is formed on the surface of the light calcium carbonate powder particles;

[0013] Furthermore, the specific preparation of the fly ash adsorbing fatty acids is as follows: 1) adding a small amount of water to dry fly ash, stirring evenly, and then adding lime calcium powder, stirring to obtain a slurry so that the potential on the surface of the fly ash particles is positive; 2) adding fatty acids to water, and adding a surfactant to emulsify it so that the potential on the surface of the fatty acids is negative; 3) adding the fatty acid emulsion emulsified in step 2) to the slurry obtained in 1) at room temperature, stirring so that the fatty acids are fully adsorbed on the fly ash particles; 4) the fly ash fully adsorbed in step 3) is allowed to stand to remove the supernatant, and then heated and dried below the fatty acid phase transition temperature to obtain the fly ash adsorbing fatty acids.

[0014] Furthermore, the fatty acid is one or a combination of two of octanoic acid, decanoic acid, n-dodecanoic acid, n-tetradecanoic acid, and n-hexadecanoic acid; the surfactant is one of sodium dodecyl sulfate, sodium dodecyl ether sulfate, sodium dodecylbenzene sulfonate, sodium alkylbenzene sulfonate, sodium alkyl phosphate, sodium lauryl alcohol polyoxyethylene ether sulfate, and α-olefin sulfonate.

[0015] Furthermore, the polyethylene glycol phase change thermal storage material is one or two of PEG600, PEG1000, PEG2000, PEG4000, PEG6000, and PEG10000; the ring-opening catalyst is one of TiCl4, SnCl4, AlCl3, BF3, ZnCl2, and LiCl; and the ring-opening reaction gas is one of ethylene oxide, propylene oxide, butylene oxide, oxadiene, octane oxide, decane oxide, and propylene glycol methyl ether acetate.

[0016] Furthermore, the cross-linking catalyst is one of TEA, DBTDL, TSP, TETA, MEA, MDEA, and TEOA; and the cross-linking agent is one of isocyanate TDI, MDI, PAPI, HDI, IPDI, NDI, and HTDI.

[0017] The present invention adopts an organic base catalyst as a cross-linking catalyst, which has the following advantages: 1. Promote reaction speed: It can effectively promote the reaction between isocyanate and hydroxyl groups in polyethylene glycol or other polymers, and accelerate the speed of the cross-linking reaction. 2. Improve reaction efficiency: The catalyst can reduce the occurrence of side reactions and improve the selectivity of the cross-linking reaction, thereby improving the quality and consistency of the product. 3. Regulate reaction conditions: The catalyst can control the reaction process by adjusting the pH value of the system to ensure that the reaction is carried out under suitable conditions. 4. Excellent selectivity: The catalyst can selectively catalyze the reaction between isocyanate and hydroxyl groups, and has a good inhibitory effect on other possible side reactions, thereby ensuring the integrity and performance of the cross-linking network. 5. Heat resistance: The catalyst can still maintain good catalytic activity at higher temperatures, making it suitable for systems that require high-temperature treatment. At the same time, it is environmentally friendly, the catalyst has low toxicity, and is easier to handle and recycle, and is more environmentally friendly; it can catalyze the reaction under milder conditions, avoiding the degradation and damage that high temperature may cause to the polymer.

[0018] Furthermore, the antioxidant and stabilizer are any two combinations of BHT, antioxidant 264, 4,4-di-tert-octyl-diphenylamine, pentaerythritol tetramethylene β-propionate, carbodiimide, UV-327, UV-531, Chimassorb 944, and Tinuvin 765.

[0019] Furthermore, the interface modifier is one of silane coupling agents A-1100, A-174, A-186, A-187, A-151, and A-172; and the inorganic porous material is one of perlite, vermiculite, montmorillonite, diatomaceous earth, volcanic rock, zeolite, medical stone, and coral stone.

[0020] Silane coupling agent is a bifunctional compound. One end can react with the hydroxyl group on the surface of inorganic porous materials to form a strong chemical bond; the other end can interact with the functional group in the organic phase change material (PCM) to improve the interfacial compatibility between the two. Specifically, it is as follows: 1. Enhanced interfacial bonding strength: Chemical bonding: Silane coupling agent firmly combines perlite and PCM through chemical bonding to form a stable interface layer, which significantly improves the bonding strength and stability of the two. Improved interfacial compatibility: Through the bifunctional characteristics of silane coupling agent, the interfacial compatibility between perlite and PCM is improved, the defects and cracks at the interface are reduced, and the overall performance of the material is improved. 2. Improved material performance: Improved thermal conductivity: The modified perlite has a good interface with PCM, which can conduct heat more effectively and improve the thermal conductivity and heat storage efficiency of the phase change material. Enhanced mechanical strength: The introduction of modifiers can enhance the mechanical strength and durability of composite materials and reduce material fatigue and cracking caused by thermal cycles. 3. Multiple silane coupling agent options: According to different phase change materials and application requirements, different types of silane coupling agents can be selected to achieve customized interface modification effects. 4. Environmental protection and safety: Silane coupling agents have good environmental performance and low toxicity.

[0021] Furthermore, the thermally conductive nanomaterial is any two combinations of nano-SiO2, nano-TiO2, nano-Al2O3, nano-ZnO, nano-CuO, nano-Fe2O3, nano-graphene, and nano-carbon tubes.

[0022] Furthermore, the adhesive is one of polyvinyl alcohol, urea-formaldehyde resin, sodium silicate, potassium silicate, polyvinyl acetate, VAE glue powder, and acrylic glue powder.

[0023] Furthermore, before adding the interface modifier to the inorganic porous material and mixing them evenly, the inorganic porous material is washed and then dried at 105° C. to remove moisture.

[0024] According to the waterproof and leak-proof phase change heat storage material of the present invention, first, a multi-layer coating granulator can be used for granulation, and multiple layers of calcium carbonate powder containing stearic acid and fly ash adsorbing fatty acids are used for coating to form multi-layer structured microspheres, thereby reducing the leakage rate of the phase change material.

[0025] Secondly, this chemical modification method of introducing carboxyl or hydroxyl groups into polyethylene glycol (PEG) (PEG) can effectively improve the chemical stability, mechanical properties and thermal conductivity of phase change materials, thereby significantly reducing their volume change and leakage risks during the phase change process, and realizing their feasibility and reliability in the practical application of phase change thermal storage panels.

[0026] The present invention adopts a method for introducing hydroxyl groups into polyethylene glycol by ring-opening reaction. Epoxides (also called ethylene oxide or epoxy compounds) are a class of compounds with epoxy groups (-CCO-), in which an oxygen atom forms a three-membered ring with two carbon atoms. Epoxides are highly reactive, and the amount of ethylene oxide is usually calculated according to the number of moles required for the reaction. There are two hydroxyl groups on each PEG molecule, and each hydroxyl group reacts with one ethylene oxide molecule, so: the number of moles of ethylene oxide required = the number of moles of PEG × the number of hydroxyl groups. The ring-opening reaction is usually carried out under milder conditions, avoiding harsh conditions such as high temperature and high pressure, making the reaction process safer and easier to control. The ring-opening reaction can accurately control the site of the reaction and the progress of the reaction, ensure the introduction of hydroxyl groups at specific positions of polyethylene glycol, reduce the occurrence of side reactions, and the ring-opening reaction usually has a higher reaction rate and a higher product yield, and can efficiently introduce hydroxyl groups into polyethylene glycol. Through the ring-opening reaction, not only a single hydroxyl group can be introduced, but also other functional groups can be introduced through subsequent reactions to achieve multifunctional modification. The ring-opening reaction can be carried out in a solvent-free or aqueous medium, reducing the use of organic solvents and complying with the principles of green chemistry. Due to its high selectivity and few by-products, the modified polyethylene glycol product obtained by the ring-opening reaction has a high purity, reducing the complexity of subsequent purification steps. The reaction conditions and reaction time are easy to control, making the regulation of the product molecular weight and degree of functionalization more precise.

[0027] Third, cross-linking agent modification is introduced into PCM to solve the leakage and volume expansion of phase change materials.

[0028] A cross-linking agent is introduced into PCM to form a three-dimensional network structure through chemical reaction to limit its volume change during phase change. Specifically, isocyanate can be used as a cross-linking agent and combined with PEG to form a stable cross-linked network; when isocyanate reacts with PEG, the hydroxyl group in the PEG molecule forms a covalent bond with the isocyanate group to form a cross-linked structure. This process is called a cross-linking reaction. The cross-linking reaction will lead to the formation of a three-dimensional network structure between molecules, improving the volume stability, mechanical properties and thermal stability of the polymer material.

[0029] In order to precisely control the cross-linking density, the cross-linking density can be precisely controlled by selecting PEG with different molecular weights and different types of isocyanates, thereby adjusting the mechanical properties and functional characteristics of the material. Functional monomers or fillers can be introduced into the cross-linking network to give the material specific functions, such as thermal conductivity, increased heat storage density, and antibacterial properties. The use of non-toxic or low-toxic isocyanates and environmentally friendly solvents can reduce environmental pollution and health risks during the production process. This method has mild reaction conditions, simple operation, and is easy to achieve large-scale industrial production.

[0030] Third, inorganic porous materials are used to coat modified phase change thermal storage materials. Inorganic porous materials have high specific surface area and porosity. Porous materials can absorb a large amount of phase change materials, acting as carriers and coatings to prevent the phase change materials from flowing and leaking during the phase change process. Inorganic porous materials wrap the phase change materials in the pores through physical adsorption or chemical adsorption. Through adsorption, the volume and shape of the phase change materials are kept stable, avoiding fluidity problems during the phase change process, and enhancing the overall stability and service life of the materials. The following advantages are obtained:

[0031] Improve thermal conductivity: Inorganic porous materials generally have higher thermal conductivity, which can significantly improve the thermal conductivity of phase change materials, shorten the charging and discharging time, and improve energy utilization efficiency.

[0032] Stabilize phase change materials: Through the wrapping and adsorption of porous materials, the phase change materials can be effectively prevented from leakage and decomposition during use, thereby improving the stability and life of the phase change materials.

[0033] Increase the loading capacity of phase change materials: The high specific surface area and porosity of porous materials enable them to adsorb and encapsulate a large amount of phase change materials, increasing the loading capacity of phase change materials and thus improving the heat storage capacity per unit volume of materials.

[0034] Improve the controllability of phase change temperature: By adjusting the pore size and structure of inorganic porous materials, the phase change temperature of phase change materials can be regulated to meet the temperature requirements in different application scenarios.

[0035] Environmental protection: Using inorganic materials as porous adsorption media usually has good environmental friendliness and reduces pollution to the environment.

[0036] Multifunctional integration: In addition to serving as adsorption media, inorganic porous materials can also give composite materials other functions, such as compatibility with inorganic gelling materials. Coating phase change materials will reduce the impact of phase change materials on the mechanical strength and mechanical strength of gelling materials, etc., expanding the application scope of phase change thermal storage materials.

[0037] Fourthly, by adding binders, the structural strength and stability of the mixture can be significantly improved. They can form a network structure in the mixture, firmly combining the inorganic porous material particles and the phase change material, thereby improving the overall strength of the material. The uniform distribution of the binder can ensure that each component in the mixture can be effectively combined to avoid the problem of stratification or dispersion of the material during use. Through sufficient stirring, the binder can be evenly coated on the surface of the inorganic porous material and the phase change material to form a uniform and stable composite material. The use of binders can not only enhance the structural strength, but also improve the thermal properties of the material. The binder has a certain high temperature resistance and can improve the heat resistance of the material; while the binder has good film forming properties and thermal conductivity, which can optimize the thermal conductivity characteristics of the phase change material.

[0038] The present invention combines inorganic porous materials with phase change materials. The inorganic porous materials serve as the substrate, providing light weight and heat insulation properties; the phase change materials absorb or release heat through the phase change process to regulate the temperature. The addition of the binder not only enhances the structural strength, but also optimizes the overall performance of the composite material. By optimizing the stirring process, the uniform distribution of the binder in the mixture is ensured. The uniform distribution not only improves the structural strength of the material, but also ensures that the phase change material plays an effective role in the entire mixture, providing stable thermal management performance.

[0039] Fifth, the present invention mixes light calcium carbonate and stearic acid (phase change material), preferably heated at a constant temperature of 70°C, 70°C is a temperature near the melting point of stearic acid, which can melt stearic acid; continuous stirring is to ensure that stearic acid can be evenly dispersed and covered on the surface of calcium carbonate particles. When stearic acid melts, it will gradually form a uniform coating on the surface of calcium carbonate particles; after stopping stirring and cooling, stearic acid will solidify to form a stable coating. Stearic acid is coated on the surface of calcium carbonate particles, which can change the surface properties of calcium carbonate, improve its hydrophobicity or improve its compatibility with organic matrices; stearic acid, as a phase change material, can absorb or release a large amount of latent heat at a specific temperature, thereby being used for thermal energy storage and temperature regulation; through the surface coating process, the modified calcium carbonate not only has its original physical and chemical properties, but also can obtain the characteristics of stearic acid phase change material, thereby playing a variety of functions in composite materials.

[0040] In the preparation of fly ash adsorbing fatty acids, by adding lime calcium powder and stirring for 20 minutes, the potential on the surface of the fly ash particles becomes positively charged; the anionic surfactant and lauric acid molecules have carboxyl groups (-COOH), which can dissociate in water to form negatively charged carboxyl groups (-COO^-); due to the principle of opposite charges attracting each other, the negatively charged lauric acid molecules will be attracted by the positively charged surface of the fly ash particles, resulting in adsorption. The fatty acid (lauric acid) is emulsified by the anionic surfactant. This emulsification process allows the fatty acid (lauric acid) molecules to be stably dispersed in the water in the form of small droplets, increasing the surface area of ​​lauric acid and the chance of its contact with the surface of the fly ash particles, thereby promoting adsorption. The long-chain alkyl part in the lauric acid molecule can interact with the surface of fly ash particles through van der Waals force (physical adsorption); at the same time, the carboxyl group in the fatty acid (lauric acid) may undergo chemical adsorption with the calcium ions (Ca^2+) on the surface of the fly ash particles to form a stronger bond. The synergistic effect of these two adsorption mechanisms allows lauric acid to be fully adsorbed on the surface of fly ash particles; the fatty acid is emulsified by a surfactant to make its surface negatively charged, and then the emulsified fatty acid is added to the positively charged fly ash. The fatty acid is evenly distributed on the fly ash particles through electrostatic adsorption. This step enhances the phase change energy storage capacity of the fly ash.

[0041] By mixing calcium carbonate powder containing stearic acid with fly ash adsorbed with fatty acid (phase change material) and heating at 150°C, the physical and chemical combination between stearic acid, fatty acid (phase change material) and calcium carbonate and fly ash is promoted to form inorganic high-efficiency waterproof powder. Subsequently, the porous material composite phase change material is added, and the inorganic high-efficiency waterproof powder is evenly distributed and wrapped on the surface of the porous material (containing the phase change material) through stirring, heating and granulation by a granulator, thereby increasing the thermal conductivity and phase change effect of the porous material (containing the phase change material).

[0042] The materials are uniformly mixed and formed through heating and granulation processes, and finally the inorganic high-efficiency waterproof powder is used to wrap the porous material (containing phase change material), ensuring the performance stability and consistency of the final product. A multi-level coating method is adopted, which improves the phase change energy storage capacity, leakage prevention ability and waterproof performance of the porous material (containing phase change material).

[0043] The present invention also provides a method for preparing a waterproof and leakproof phase-change heat storage and thermal insulation wallboard. The method comprises the following steps: adding water at a water-to-material ratio of 1:1 to 500-700 parts of ordinary silicate cement, 15-25 parts of polystyrene particles, 300-350 parts of the above-mentioned waterproof and leakproof phase-change heat storage material, 2-5 parts of polypropylene anti-cracking fibers, 3-6 parts of VAE glue powder, and 3-6 parts of hydroxypropyl methylcellulose, and stirring evenly to obtain a phase-change heat storage slurry; placing a 10cm-15cm thick extruded insulation board at the bottom of a mold, applying a special interface agent for the extruded insulation board on the inner surface, laying an anti-cracking glass fiber mesh cloth, pouring the prepared phase-change heat storage slurry to a thickness of 10cm-15cm, pressing the anti-cracking glass fiber mesh cloth into the surface, and adopting vibration molding, curing and demoulding.

[0044] The present invention also provides a flexible solar greenhouse, comprising a rear wall and side walls, wherein the rear wall and / or side walls are constructed with a keel, and the phase change thermal storage insulation wall panel obtained by the preparation method of the waterproof and leakproof phase change thermal storage insulation wall panel is installed on the inner side of the keel, and a nano thermal conductive coating layer is coated on the side of the phase change thermal storage insulation wall panel away from the extruded insulation board; or a 10-15 cm extruded insulation board is inlaid on the inner side of the keel, a steel mesh is welded on the keel, and the phase change thermal storage mortar described in the preparation method of the 10-15 cm waterproof and leakproof phase change thermal storage insulation wall panel is applied, and after curing and demolding, a nano thermal conductive coating layer is sprayed. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a schematic diagram of the structure of the flexible solar greenhouse of the present invention;

[0046] In the accompanying drawings, the components represented by the reference numerals are listed as follows:

[0047] 1. Wall keel, 2. Phase change thermal insulation wall panel, 3. Roof frame, 4. Upwind vent starting position, 5. Upwind vent stop position, 6. Downwind vent starting position, 7. Upwind vent stop position, 8. Quilt, 9. Quilt limit rod, 10. Foundation pile, 11. XPS insulation board, 12. Longitudinal pipe. DETAILED DESCRIPTION

[0048] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention but not to limit the scope of the present invention.

[0049] Example 1

[0050] The method for preparing the waterproof and leakproof phase-change thermal storage material of the present invention comprises the following steps:

[0051] Step (1), dissolving 40 kg of PEG600 and 60 kg of PEG6000 in 200 L of deionized water to form a uniform solution, adding 0.5 kg of LiCl, stirring evenly, slowly introducing 8.10 kg of propylene glycol methyl ether acetate as a ring-opening reaction gas, and keeping the solution at 60° C. for 2 hours; after the reaction is completed, adding NaOH to adjust the pH to neutral, repeatedly washing the product with deionized water to neutral, and then washing with ethanol to remove unreacted impurities; the product is vacuum dried to obtain a hydroxylated phase change thermal storage material.

[0052] Step (2), dissolving 100 parts of the obtained hydroxylated phase change thermal storage material in 50 parts of xylene, stirring until completely dissolved to obtain a solution, adding 0.5 parts of TEOA to the solution, and continuing to stir evenly. Slowly add 10 parts of HTDI crosslinking agent to the solution, stir evenly, and react at room temperature to ensure that the crosslinking agent and the hydroxylated phase change thermal storage material fully react to form a three-dimensional network structure; during the reaction, keep stirring, and the reaction at 60°C needs to be carried out for 4 hours to ensure complete crosslinking; after the reaction is completed, remove the solvent by reduced pressure distillation or other methods, add 0.25 parts of BHT antioxidant and 0.25 parts of UV-327 stabilizer, stir evenly, and obtain HTDI crosslinked modified phase change thermal storage material.

[0053] Step (3), take 30 parts of coral stone, wash and dry at 105°C to remove moisture; add 2 parts of A-172 interface modifier and mix well; take 70 parts of HTDI cross-linked modified phase change thermal storage material, heat at 50°C to melt it into liquid, add 2.5 parts of nano Fe2O3 and 2.5 parts of graphene, add 5 parts of VAE rubber powder, and stir well; transfer the mixture to a vacuum adsorption device, set the vacuum degree to -0.1MPa, keep it for 30 minutes, and stir slowly under vacuum environment at a stirring speed of 30 rpm. Cool the mixture after vacuum adsorption to room temperature and solidify naturally to obtain coral stone coated cross-linked modified phase change thermal storage material.

[0054] Step (4), weigh 50 parts of light calcium carbonate and 2 parts of stearic acid, heat at 70°C, and stir and mix continuously until a uniform layer of stearic acid is formed on the surface of the calcium carbonate powder particles, to obtain calcium carbonate powder containing stearic acid. Add 125 parts of water to 50 parts of dry fly ash, stir evenly, and then add 15 parts of fly ash calcium powder, stir for 20 minutes, to obtain fly ash slurry;

[0055] Add 8 parts of decanoic acid to 25 ml of water, and add 0.1 parts of sodium alkylbenzene sulfonate to emulsify it; at room temperature, add the emulsified decanoic acid emulsion to the fly ash slurry and stir for 30 minutes to fully adsorb the decanoic acid on the fly ash particles to obtain decanoic acid emulsified slurry. Let the decanoic acid emulsified slurry stand for 1 hour, remove the supernatant, and then heat and dry at ≤32°C to obtain fly ash adsorbed with decanoic acid. Mix the calcium carbonate powder containing stearic acid and the fly ash treated with decanoic acid adsorption and heat to 150°C, add 125 parts of coral stone coated cross-linked modified phase change thermal storage material, stir evenly and introduce into the disc granulator for granulation, and after cooling, obtain the inorganic high-efficiency waterproof powder coated coral stone composite phase change material, that is, waterproof and leak-proof phase change thermal storage material.

[0056] Example 2

[0057] The method for preparing the waterproof and leakproof phase-change thermal storage material of the present invention comprises the following steps:

[0058] Step (1), dissolving 50 kg of PEG600 and 50 kg of PEG10000 in 200 L of deionized water to form a uniform solution; adding 0.5 kg of TiCl4, stirring evenly, slowly introducing 8.91 kg of ethylene oxide as a ring-opening reaction gas, and keeping the solution at 60° C. for 2 hours; after the reaction is completed, adding NaOH to adjust the pH to neutral; repeatedly washing the product with deionized water until it is neutral, and then washing with ethanol to remove unreacted impurities, and vacuum drying the product to obtain a hydroxylated phase change thermal storage material.

[0059] Step (2) dissolving 100 parts of the obtained hydroxylated phase change thermal storage material in 50 parts of xylene, stirring until completely dissolved to obtain a solution; adding 0.5 parts of DBTDL to the solution, continuing to stir evenly, slowly adding 10 parts of MDI cross-linking agent to the solution, and stirring evenly; reacting at room temperature to ensure that the MDI cross-linking agent and the hydroxylated phase change thermal storage material fully react to form a three-dimensional network structure; during the reaction, stirring is maintained, and the reaction at 60°C needs to be carried out for 4 hours to ensure complete cross-linking; after the reaction is completed, the solvent is removed by reduced pressure distillation or other methods, and 0.30 parts of carbodiimide and 0.20 parts of Chimassorb944 are added and stirred evenly to obtain an MDI cross-linked modified phase change thermal storage material.

[0060] Step (3) Take 28 parts of volcanic rock, wash and dry at 105°C to remove moisture; add 3 parts of A-1100 interface modifier and mix well; take 68 parts of MDI cross-linked modified phase change thermal storage material, heat at 50°C to melt it into liquid, add 2.0 parts of nano-TiO2 and 2.0 parts of graphene, add 10 parts of acrylic powder, and stir well; transfer the mixture to a vacuum adsorption device, set the vacuum degree to -0.1MPa, keep it for 30 minutes, and stir slowly under vacuum at a stirring speed of 30 rpm. Cool the mixture after vacuum adsorption to room temperature and solidify naturally; obtain the volcanic rock coated cross-linked modified phase change thermal storage material;

[0061] Step (4) Preparation of calcium carbonate powder containing stearic acid and fly ash slurry is the same as in Example 1;

[0062] Add 8 parts of n-dodecanoic acid to 25 ml of water, and add 0.1 parts of sodium dodecyl sulfate to emulsify it; at room temperature, add the emulsified n-dodecanoic acid emulsion to the fly ash slurry and stir for 30 minutes to fully adsorb the n-dodecanoic acid on the fly ash particles to obtain the n-dodecanoic acid emulsified slurry. Let the n-dodecanoic acid emulsified slurry stand for 1 hour, remove the supernatant, and then heat and dry at ≤32°C to obtain the fly ash adsorbing n-dodecanoic acid. Mix the above-mentioned calcium carbonate powder containing stearic acid and the fly ash adsorbing n-dodecanoic acid and heat to 150°C, add 125 parts of volcanic rock coated cross-linked modified phase change thermal storage material, stir evenly and introduce into the disc granulator for granulation, and after cooling, obtain the inorganic high-efficiency waterproof powder wrapped volcanic rock composite phase change material, waterproof and leak-proof phase change thermal storage material.

[0063] Example 3

[0064] The method for preparing the waterproof and leakproof phase-change thermal storage material of the present invention comprises the following steps:

[0065] Step (1), dissolving 100 kg of PEG2000 in 200 L of deionized water to form a uniform solution, adding 0.5 kg of SnCl4, and stirring evenly; slowly introducing 8.94 kg of propylene oxide as a ring-opening reaction gas, and keeping the solution at 60° C. for 2 hours; after the reaction is completed, adding NaOH to adjust the pH to neutral; repeatedly washing the product with deionized water until it is neutral, and then washing with ethanol to remove unreacted impurities; and vacuum drying the product to obtain a hydroxylated phase change thermal storage material.

[0066] Step (2), dissolving 100 parts of the obtained hydroxylated phase change thermal storage material in 50 parts of xylene, stirring until completely dissolved to obtain a solution; adding 0.5 parts of TEA to the solution, and continuing to stir evenly. Slowly add 10 parts of TDI crosslinking agent to the solution, stir evenly, and react at room temperature to ensure that the crosslinking agent and the hydroxylated phase change thermal storage material fully react to form a three-dimensional network structure. During the reaction, keep stirring, and the reaction at 60°C needs to be carried out for 4 hours to ensure complete crosslinking. After the reaction is completed, remove the solvent by vacuum distillation or other methods to obtain a crosslinked hydroxylated phase change thermal storage material. Add 0.20 parts of antioxidant 264 and 0.30 parts of UV-531 and stir evenly to obtain a TDI crosslinked modified phase change thermal storage material.

[0067] Step (3), take 20 parts of diatomite, wash it and dry it at 105°C to remove moisture; add 3 parts of A-186 interface modifier and mix them evenly; take 78 parts of TDI cross-linked modified phase change thermal storage material, heat it at 50°C to melt it into liquid, add 3.0 parts of nano-SiO2 and 1.0 parts of carbon nanotubes, add 10 parts of PVA glue powder, and stir evenly; transfer the mixture to a vacuum adsorption device, set the vacuum degree to -0.1MPa, keep it for 30 minutes, and stir it slowly under vacuum environment at a stirring speed of 30 rpm; cool the mixture after vacuum adsorption to room temperature and solidify it naturally. The diatomite-coated TDI cross-linked modified phase change thermal storage material is obtained.

[0068] Step (4) Preparation of calcium carbonate powder containing stearic acid and fly ash slurry is the same as in Example 1;

[0069] 8 parts of n-tetradecanoic acid are added to 25 ml of water, and 0.1 parts of sodium dodecylbenzene sulfonate is added to emulsify it; at room temperature, the emulsified n-tetradecanoic acid emulsion is added to the fly ash slurry, stirred for 30 minutes, so that the n-tetradecanoic acid is fully adsorbed on the fly ash particles to obtain the n-tetradecanoic acid emulsified slurry; the n-tetradecanoic acid emulsified slurry is allowed to stand for 1 hour, the supernatant is removed, and then heated and dried at ≤32°C to adsorb the fly ash with n-tetradecanoic acid; the stearic acid-containing calcium carbonate powder and the fly ash adsorbed with n-tetradecanoic acid are mixed and heated to 150°C, 125 parts of diatomaceous earth-coated TDI cross-linked modified phase change thermal storage material are added, stirred evenly, introduced into a disc granulator for granulation, and after cooling, an inorganic high-efficiency waterproof powder-coated diatomaceous earth composite phase change material is obtained.

[0070] Example 4

[0071] The method for preparing the waterproof and leakproof phase-change thermal storage material of the present invention comprises the following steps:

[0072] Step (1), dissolve 60kg of PEG2000 and 40kg of PEG4000 in 200L of deionized water to form a uniform solution, add 0.5kg of AlCl3, stir evenly, slowly introduce 9.23kg of butylene oxide as the ring-opening reaction gas, and keep the solution at 60°C for 2 hours. After the reaction is completed, add NaOH to adjust the pH to neutral, repeatedly wash the product with deionized water to neutral, and then wash with ethanol to remove unreacted impurities. Dry the product in a vacuum drying oven to obtain a hydroxylated phase change thermal storage material.

[0073] Step (2), dissolving 100 parts of the obtained hydroxylated phase change thermal storage material in 50 parts of xylene, stirring until completely dissolved to obtain a solution. Add 0.5 parts of TSP to the solution and continue to stir evenly. Slowly add 10 parts of HDI crosslinker to the solution and stir evenly; react at room temperature to ensure that the crosslinker and the hydroxylated phase change thermal storage material fully react to form a three-dimensional network structure. During the reaction, keep stirring, and the reaction at 60°C needs to be carried out for 4 hours to ensure complete crosslinking; after the reaction is completed, remove the solvent by vacuum distillation or other methods to obtain a cross-linked hydroxylated phase change thermal storage material; add 0.15 parts of 4,4-di-tert-octyl-diphenylamine and 0.15 parts of Tinuvin 765 and stir evenly to obtain an HDI cross-linked modified phase change thermal storage material;

[0074] Step (3), take 25 parts of montmorillonite, wash it and dry it at 105°C to remove moisture. Add 3 parts of A-174 interface modifier and mix well; take 70 parts of HDI cross-linked modified phase change thermal storage material, heat it at 50°C to melt it into a liquid, add 2.0 parts of nano ZnO and 2.0 parts of graphene, add 10 parts of urea-formaldehyde resin powder, and stir well. Transfer the mixture to a vacuum adsorption equipment, set the vacuum degree to -0.1MPa, keep it for 30 minutes, and stir slowly under vacuum environment at a stirring speed of 30 rpm. Cool the mixture after vacuum adsorption to room temperature and solidify naturally. Obtain montmorillonite-coated HDI cross-linked modified phase change thermal storage material;

[0075] Step (4), preparation of calcium carbonate powder containing stearic acid and fly ash slurry is the same as in Example 1;

[0076] 8 parts of n-hexadecanoic acid are added to 25 ml of water, and 0.1 parts of sodium alkyl phosphate are added to emulsify it; at room temperature, the emulsified n-hexadecanoic acid emulsion is added to the upper fly ash slurry, stirred for 30 minutes, so that the n-hexadecanoic acid is fully adsorbed on the fly ash particles to obtain n-hexadecanoic acid emulsified slurry; the n-hexadecanoic acid emulsified slurry is allowed to stand for 1 hour, the supernatant is removed, and then heated and dried at ≤32°C to adsorb the fly ash with n-hexadecanoic acid; the stearic acid-containing calcium carbonate powder and the fly ash adsorbed with n-hexadecanoic acid are mixed and heated to 150°C, 125 parts of montmorillonite-coated cross-linked modified phase change thermal storage material are added, stirred evenly, and introduced into a disc granulator for granulation, and after cooling, an inorganic high-efficiency waterproof powder-coated montmorillonite composite phase change material, i.e., a waterproof and leak-proof phase change thermal storage material, is obtained.

[0077] Example 5

[0078] The method for preparing the waterproof and leakproof phase-change thermal storage material of the present invention comprises the following steps:

[0079] Step (1), dissolving 50 kg of PEG1000 and 50 kg of PEG4000 in 200 L of deionized water to form a uniform solution, adding 0.5 kg of BF3, and stirring evenly; slowly introducing 16.0 kg of octane oxide as a ring-opening reaction gas, and keeping the solution at 60° C. for 2 hours; after the reaction is completed, adding NaOH to adjust the pH to neutral; repeatedly washing the product with deionized water until it is neutral, and then washing with ethanol to remove unreacted impurities, and vacuum drying the product to obtain a hydroxylated phase change thermal storage material.

[0080] Step (2), dissolving 100 parts of the obtained hydroxylated phase change thermal storage material in 50 parts of xylene, stirring until completely dissolved to obtain a solution. Add 0.5 parts of TETA to the solution and continue to stir evenly. Slowly add 10 parts of PAPI crosslinker to the solution and stir evenly; react at room temperature to ensure that PAPI and the hydroxylated phase change thermal storage material fully react to form a three-dimensional network structure; during the reaction, keep stirring, and the reaction at 60°C needs to be carried out for 4 hours to ensure complete crosslinking; after the reaction is completed, remove the solvent by reduced pressure distillation or other methods, add 0.30 parts of tetramethylene β-propionic acid pentaerythritol ester and 0.10 parts of UV328 and stir evenly to obtain PAPI crosslinked modified phase change thermal storage material.

[0081] Step (3), take 50 parts of zeolite, wash and dry at 105°C to remove moisture. Add 3 parts of A-187 interface modifier and mix well; take 50 parts of PAPI cross-linked modified phase change thermal storage material, heat at 50°C to melt it into liquid, add 1.0 parts of nano-CuO and 1.0 parts of graphene, add 10 parts of polyvinyl acetate powder, and stir well; transfer the mixture to a vacuum adsorption device, set the vacuum degree to -0.1MPa, keep it for 30 minutes, and stir slowly under vacuum environment at a stirring speed of 30 rpm; cool the mixture after vacuum adsorption to room temperature and solidify naturally. Obtain zeolite-coated PAPI cross-linked modified phase change thermal storage material.

[0082] Step (4), preparation of calcium carbonate powder containing stearic acid and fly ash slurry is the same as in Example 1;

[0083] 4 parts of n-dodecanoic acid and 4 parts of octanoic acid are added to 25 ml of water, and 0.1 parts of α-olefin sulfonate is added to emulsify them; at room temperature, the emulsified n-dodecanoic acid and octanoic acid emulsion is added to the slurry obtained in (2), and stirred for 30 minutes to allow the n-dodecanoic acid and octanoic acid to be fully adsorbed on the fly ash particles; the n-dodecanoic acid and octanoic acid emulsified slurry is allowed to stand for 1 hour, the supernatant is removed, and then heated and dried at ≤32°C to obtain fly ash adsorbing n-dodecanoic acid and octanoic acid; calcium carbonate powder containing stearic acid is mixed with fly ash adsorbing n-dodecanoic acid and octanoic acid, heated to 150°C, 125 parts of zeolite-coated PAPI cross-linked modified phase change thermal storage material are added, stirred evenly, and introduced into a disc granulator for granulation, and after cooling, an inorganic high-efficiency waterproof powder-coated zeolite composite phase change material is obtained.

[0084] Example 6

[0085] The method for preparing the waterproof and leakproof phase-change thermal storage material of the present invention comprises the following steps:

[0086] Step (1), dissolve 20kg of PEG2000 and 80kg of PEG6000 in 200L of deionized water to form a uniform solution; add 0.5kg of ZnCl2 to the phase change thermal storage material solution and stir evenly; slowly introduce 5.17kg of oxacyclohexane as the ring-opening reaction gas, and keep the solution at 60°C for 2 hours. After the reaction is completed, add NaOH to adjust the pH to neutral. Repeatedly wash the product with deionized water until it is neutral, and then wash with ethanol to remove unreacted impurities. Dry the product in a vacuum drying oven to obtain a hydroxylated phase change thermal storage material.

[0087] Step (2), dissolving 100 parts of the obtained hydroxylated phase change thermal storage material in 50 parts of xylene, stirring until completely dissolved to obtain a solution. Add 0.5 parts of MEA to the solution and continue to stir evenly. Slowly add 10 parts of NDI crosslinking agent to the solution and stir evenly. React at room temperature to ensure that NDI and the hydroxylated phase change thermal storage material fully react to form a three-dimensional network structure. During the reaction, keep stirring, and the reaction at 60°C needs to be carried out for 4 hours to ensure complete crosslinking. After the reaction is completed, remove the solvent by vacuum distillation or other methods to obtain a cross-linked hydroxylated phase change thermal storage material. Add 0.30 parts of BHT and 0.10 parts of UV531 and stir evenly to obtain an NDI cross-linked modified phase change thermal storage material.

[0088] Step (3), take 20 parts of vermiculite, wash it and dry it at 105°C to remove moisture. Add 3 parts of A-151 interface modifier and mix well; take 80 parts of NDI cross-linked modified phase change thermal storage material, heat it at 50°C to melt it into a liquid, add 4.0 parts of nano Fe2O3 and 1.0 parts of carbon nanotubes, add 10 parts of sodium silicate powder, and stir well. Transfer the mixture to a vacuum adsorption device, set the vacuum degree to -0.1MPa, keep it for 30 minutes, and stir slowly under a vacuum environment at a stirring speed of 30 rpm. Cool the mixture after vacuum adsorption to room temperature and solidify naturally. Obtain vermiculite-coated NDI cross-linked modified phase change thermal storage material.

[0089] Step (4) Preparation of calcium carbonate powder containing stearic acid and fly ash slurry is the same as in Example 1;

[0090] 5 parts of n-dodecanoic acid and 1 part of n-tetradecanoic acid are added to 25 ml of water, and 0.1 parts of sodium lauryl polyoxyethylene ether sulfate are added to emulsify them; at room temperature, the emulsified n-dodecanoic acid and n-tetradecanoic acid emulsions are added to fly ash slurry, stirred for 30 minutes, so that the n-dodecanoic acid and n-tetradecanoic acid are fully adsorbed on the fly ash particles to obtain n-dodecanoic acid and n-tetradecanoic acid emulsified slurry; the n-dodecanoic acid and n-tetradecanoic acid emulsified slurry is allowed to stand for 1 hour, the supernatant is removed, and then heated and dried at ≤32°C to obtain fly ash adsorbing n-dodecanoic acid and n-tetradecanoic acid; stearic acid-containing calcium carbonate powder and fly ash adsorbing n-dodecanoic acid and n-tetradecanoic acid are mixed and heated to 150°C, 125 parts of vermiculite-coated NDI cross-linked modified phase change thermal storage material are added, stirred evenly and introduced into a disc granulator for granulation, and after cooling, an inorganic high-efficiency waterproof powder-coated vermiculite composite phase change material is obtained.

[0091] Example 7

[0092] The method for preparing the waterproof and leakproof phase-change thermal storage material of the present invention comprises the following steps:

[0093] Step (1), dissolve 20kg of PEG2000 and 80kg of PEG4000 in 200L of deionized water to form a uniform solution. Add 0.5kg of TiCl4 to the phase change thermal storage material solution and stir evenly. Slowly introduce 30.2kg of decane oxide as the ring-opening reaction gas and keep the solution at 60°C for 2 hours. After the reaction is completed, add NaOH to adjust the pH to neutral. Repeatedly wash the product with deionized water until it is neutral, and then wash with ethanol to remove unreacted impurities. Dry the product in a vacuum drying oven to obtain a hydroxylated phase change thermal storage material.

[0094] Step (2), dissolving 100 parts of the obtained hydroxylated phase change thermal storage material in 50 parts of xylene, stirring until completely dissolved to obtain a solution; adding 0.5 parts of MDEA to the solution, and continuing to stir evenly. Slowly add 10 parts of IPDI crosslinking agent to the solution and stir evenly. React at room temperature to ensure that IPDI and the hydroxylated phase change thermal storage material fully react to form a three-dimensional network structure. During the reaction, keep stirring, and the reaction at 60°C needs to be carried out for 4 hours to ensure complete crosslinking. After the reaction is completed, remove the solvent by vacuum distillation or other methods to obtain a cross-linked hydroxylated phase change thermal storage material; add 0.40 parts of BHT and 0.10 parts of UV327 and stir evenly to obtain an IPDI cross-linked modified phase change thermal storage material.

[0095] Step (3) Take 20 parts of perlite, wash and dry at 105°C to remove moisture. Add 3 parts of A-186 interface modifier and mix well; Take 80 parts of IPDI cross-linked modified phase change thermal storage material, heat at 50°C to melt it into liquid, add 3.0 parts of nano AL2O3 and 2.0 parts of graphene, add 10 parts of potassium silicate powder, and stir well; Transfer the mixture to a vacuum adsorption device, set the vacuum degree to -0.1MPa, keep it for 30 minutes, and stir slowly under vacuum at a stirring speed of 30 rpm; Cool the mixture after vacuum adsorption to room temperature and solidify it naturally to obtain perlite-coated IPDI cross-linked modified phase change thermal storage material;

[0096] Step (4) Preparation of calcium carbonate powder containing stearic acid and fly ash slurry is the same as in Example 1;

[0097] 3.5 parts of n-dodecanoic acid and 1.5 parts of n-hexadecanoic acid are added to 25 ml of water, and 0.1 parts of sodium dodecyl ether sulfate is added to emulsify it; at room temperature, the emulsified n-dodecanoic acid and n-hexadecanoic acid emulsion are added to the fly ash slurry, stirred for 30 minutes, so that the n-dodecanoic acid and n-hexadecanoic acid are fully adsorbed on the fly ash particles, and the n-dodecanoic acid and n-hexadecanoic acid emulsified slurry are obtained, and the n-dodecanoic acid and n-hexadecanoic acid emulsified slurry is allowed to stand for 1 hour, the supernatant is removed, and then heated and dried at ≤32°C to adsorb the fly ash of n-dodecanoic acid and n-hexadecanoic acid. The calcium carbonate powder of stearic acid obtained in step (1) is mixed with the fly ash adsorbing n-dodecanoic acid and n-hexadecanoic acid, heated to 150°C, 125 parts of perlite-coated IPDI cross-linked modified phase change thermal storage material are added, stirred evenly, introduced into a disc granulator for granulation, and cooled to obtain an inorganic high-efficiency waterproof powder-coated perlite composite phase change material.

[0098] The performance index test results of the hydroxylated phase change thermal storage materials of Examples 1 to 7 are shown in Table 1.

[0099] Table 1. Properties of hydroxylated phase change thermal storage materials ((hydroxylated PEG))

[0100]

[0101]

[0102] Note: Compatibility with other materials mainly refers to the compatibility of the phase change thermal storage material with the inorganic nanomaterials and nanocarbon materials used in the present invention, and the gelling materials (ordinary Portland cement, polypropylene anti-cracking fiber, rubber powder and hydroxypropyl methylcellulose).

[0103] The performance index test results of the cross-linked modified phase change thermal storage materials of Examples 1 to 7 are shown in Table 2.

[0104] Table 2. Properties of cross-linked modified phase change thermal storage materials

[0105]

[0106] The performance index test results of the inorganic porous coated cross-linked modified phase change thermal storage materials of Examples 1 to 7 are shown in Table 3.

[0107] Table 3. Properties of cross-linked phase change materials wrapped by inorganic porous materials

[0108]

[0109] Note: In Table 3, “before encapsulation” refers to the performance of the phase change thermal storage material modified by cross-linking before being coated with inorganic porous materials, and “after encapsulation” refers to the performance of the phase change thermal storage material modified by cross-linking with inorganic porous materials.

[0110] The performance indicators of the inorganic high-efficiency waterproof powder-coated porous composite phase change materials of Examples 1 to 7 are shown in Tables 4-1 and 4-2.

[0111] Table 4-1. Performance of porous composite phase change materials wrapped with inorganic high-efficiency waterproof powder

[0112]

[0113] Note: In Table 4-1, before wrapping refers to the performance of phase change thermal storage materials modified by cross-linking of inorganic porous materials. After wrapping refers to porous composite phase change materials wrapped by inorganic high-efficiency waterproof powder.

[0114] Table 4-2. Performance of porous composite phase change materials wrapped with inorganic high-efficiency waterproof powder (waterproof performance)

[0115]

[0116]

[0117] Note: In Table 4-2, before wrapping refers to the performance of phase change thermal storage materials modified by cross-linking of inorganic porous materials. After wrapping refers to porous composite phase change materials wrapped by inorganic high-efficiency waterproof powder.

[0118] Example 8

[0119] The preparation method of the phase-change heat storage and thermal insulation wallboard of the present invention is as follows: 640 parts of ordinary silicate cement, 20 parts of polystyrene particles, 330 parts of the inorganic high-efficiency waterproof powder-wrapped coral stone composite phase change material of Example 1, 3 parts of polypropylene anti-cracking fiber, 4 parts of VAE glue powder, and 3 parts of hydroxypropyl methylcellulose are taken, and water is added at a water-to-material ratio of 50% and stirred evenly to obtain a phase-change heat storage mortar. A 12 cm thick extruded insulation board (XPS) is placed at the bottom of the mold, a special interface agent for the extruded insulation board is applied to the inner surface, and an anti-cracking glass fiber mesh cloth is laid. The prepared phase-change heat storage mortar is poured to a thickness of 12 cm, and an anti-cracking glass fiber mesh cloth is pressed into the surface, and vibration molding is adopted. Under the conditions of 20°C and relative humidity greater than 90%, it is cured until it has sufficient strength for demoulding, and a 500 um black nano-thermal conductive coating (thermal conductivity coefficient λ≥10w / mk) is sprayed on the surface to obtain a phase-change heat storage and thermal insulation wallboard.

[0120] Example 9

[0121] The preparation method of the phase-change heat storage and thermal insulation wallboard of the present invention is as follows: 640 parts of ordinary silicate cement, 20 parts of polystyrene particles, 330 kg of the inorganic high-efficiency waterproof powder wrapped volcanic stone composite phase change material of Example 2, 3 parts of polypropylene anti-cracking fiber, 4 parts of acrylic acid powder, and 3 parts of hydroxypropyl methylcellulose are taken, and water is added at a water-to-material ratio of 50% and stirred evenly to obtain a phase-change heat storage mortar. A 10 cm thick extruded insulation board (XPS) is placed at the bottom of the mold, a special interface agent for the extruded insulation board is applied to the inner surface, and an anti-cracking glass fiber mesh cloth is laid. The prepared phase-change heat storage mortar is poured to a thickness of 10 cm, and an anti-cracking glass fiber mesh cloth is pressed into the surface, and vibration molding is adopted. Under the conditions of 20°C and relative humidity greater than 90%, it is cured until it has sufficient strength for demoulding, and 500 um of black nano thermal conductive coating (thermal conductivity coefficient λ≥10w / mk) is sprayed on the surface to obtain a phase-change heat storage and thermal insulation wallboard.

[0122] Example 10

[0123] The preparation method of the phase-change heat storage and thermal insulation wallboard of the present invention is as follows: 640 parts of ordinary silicate cement, 20 parts of polystyrene particles, 330 parts of the inorganic high-efficiency waterproof powder wrapped diatomite composite phase change material of Example 3, 3 parts of polypropylene anti-cracking fiber, 4 parts of PVA glue powder, and 3 parts of hydroxypropyl methylcellulose are taken, and water is added at a water-to-material ratio of 50% and stirred evenly to obtain a phase-change heat storage mortar. A 15 cm thick extruded insulation board (XPS) is placed at the bottom of the mold, a special interface agent for the extruded insulation board is applied to the inner surface, and an anti-cracking glass fiber mesh cloth is laid. The prepared phase-change heat storage mortar is poured to a thickness of 15 cm, and an anti-cracking glass fiber mesh cloth is pressed into the surface, and vibration molding is adopted. Under the conditions of 20°C and relative humidity greater than 90%, it is cured until it has sufficient strength for demoulding, and a 500 um black nano thermal conductive coating (thermal conductivity coefficient λ≥10w / mk) is sprayed on the surface to obtain a phase-change heat storage and thermal insulation wallboard.

[0124] Embodiment 11

[0125] The preparation method of the phase-change heat storage and thermal insulation wallboard of the present invention is as follows: 640 parts of ordinary silicate cement, 20 parts of polystyrene particles, 330 parts of the inorganic high-efficiency waterproof powder-wrapped diatomite composite phase change material of Example 4, 3 parts of polypropylene anti-cracking fiber, 4 parts of PVA glue powder, and 3 parts of hydroxypropyl methylcellulose are taken, and water is added at a water-to-material ratio of 50% and stirred evenly to obtain a phase-change heat storage mortar. A 15 cm thick extruded insulation board (XPS) is placed at the bottom of the mold, a special interface agent for the extruded insulation board is applied to the inner surface, and an anti-cracking glass fiber mesh cloth is laid. The prepared phase-change heat storage mortar is poured to a thickness of 12 cm, and an anti-cracking glass fiber mesh cloth is pressed into the surface, and vibration molding is adopted. Under the conditions of 20°C and relative humidity greater than 90%, it is cured until it has sufficient strength for demoulding, and a 500 um black nano-thermal conductive coating (thermal conductivity coefficient λ≥10w / mk) is sprayed on the surface to obtain a phase-change heat storage and thermal insulation wallboard.

[0126] Example 12

[0127] The preparation method of the phase-change heat storage and thermal insulation wallboard of the present invention is as follows: 640 parts of ordinary silicate cement, 20 parts of polystyrene particles, 330 parts of inorganic high-efficiency waterproof powder-wrapped zeolite composite phase change material of Example 5, 3 parts of polypropylene anti-cracking fiber, 4 parts of polyvinyl acetate glue powder, and 3 parts of hydroxypropyl methylcellulose are taken, and water is added at a water-to-material ratio of 50% and stirred evenly to obtain a phase-change heat storage mortar. A 12 cm thick extruded insulation board (XPS) is placed at the bottom of the mold, a special interface agent for the extruded insulation board is applied to the inner surface, and an anti-cracking glass fiber mesh cloth is laid. The prepared phase-change heat storage mortar is poured to a thickness of 12 cm, and an anti-cracking glass fiber mesh cloth is pressed into the surface, and vibration molding is adopted. Under the conditions of 20°C and relative humidity greater than 90%, it is cured until it has sufficient strength for demolding, and a 500 um black nano thermal conductive coating (thermal conductivity coefficient λ≥10w / mk) is sprayed on the surface to obtain a phase-change heat storage and thermal insulation wallboard.

[0128] Embodiment 13

[0129] Take 640 parts of ordinary Portland cement, 20 parts of polystyrene particles, 330 parts of the inorganic high-efficiency waterproof powder wrapped vermiculite composite phase change material of Example 6, 3 parts of polypropylene anti-cracking fiber, 4 parts of sodium silicate glue powder, and 3 parts of hydroxypropyl methylcellulose, add water at a water-to-material ratio of 50% and stir evenly to obtain a phase change thermal storage mortar. Place a 15cm thick extruded insulation board (XPS) at the bottom of the mold, apply a special interface agent for the extruded insulation board on the inner surface, lay an anti-cracking glass fiber mesh cloth, pour the prepared phase change thermal storage mortar 15cm thick, press the anti-cracking glass fiber mesh cloth on the surface, and use vibration molding. Curing at 20°C and relative humidity greater than 90% until it has sufficient strength to demould, spray 500um of black nano thermal conductive coating (thermal conductivity λ≥10w / mk) on the surface to obtain a phase change thermal storage insulation wallboard.

[0130] Embodiment 14

[0131] Take 640 parts of ordinary Portland cement, 20 parts of polystyrene particles, 330 parts of Example 7 inorganic high-efficiency waterproof powder wrapped perlite composite phase change material, 3 parts of polypropylene anti-cracking fiber, 4 parts of potassium silicate powder, 3 parts of hydroxypropyl methylcellulose, add water at a water-to-material ratio of 50% and stir evenly to obtain phase change thermal storage mortar. Place a 15cm thick extruded insulation board (XPS) at the bottom of the mold, apply a special interface agent for extruded insulation board on the inner surface, lay anti-cracking glass fiber mesh cloth, pour the prepared phase change thermal storage mortar 15cm thick, press the anti-cracking glass fiber mesh cloth on the surface, and use vibration molding. Curing at 20°C and relative humidity greater than 90% until there is sufficient strength to demold, spray 500um black nano thermal conductive coating (thermal conductivity λ≥10w / mk) on the surface to obtain a phase change wallboard with extruded insulation board. The performance index parameters of the phase change wallboard with extruded insulation board prepared in Examples 8 to 14 are shown in Table 5.

[0132] Table 5. Phase change thermal insulation wallboard performance parameters

[0133]

[0134]

[0135] Examples 15 to 21

[0136] A flexible solar greenhouse comprises a rear wall and side walls, wherein the rear wall and / or side walls are constructed with keels, and the phase-change thermal storage insulation wall panels obtained by the preparation methods described in Examples 8 to 14 are installed on the inner side of the keels, and a nano-thermal conductive coating layer is coated on the side of the phase-change thermal storage insulation wall panels away from the insulation board. The performance indexes of the rear wall of the flexible solar greenhouse with phase-change thermal storage insulation wall panels are shown in Table 6, and the temperature indexes in the flexible solar greenhouse are shown in Table 7. The rear wall of the present invention can also be made of double-layered phase-change thermal storage insulation wall panels.

[0137] like Figure 1 The flexible solar greenhouse wall of the embodiment of the present invention is shown, the rear wall adopts a phase change heat storage insulation wallboard 2 installed on the rear wall keel 1, the roof frame 3 is connected and fixed to the rear wall keel 1 and is fixed with a longitudinal pipe 12, and a 150mm thick extruded polystyrene insulation board 11 is used to set a cold-proof wall in the front and back underground. The rear wall keel 1 and the roof frame 3 are constructed on the foundation pile 10; the latitude, temperature and winter solstice solar altitude angle of the solar greenhouse are positively correlated according to the statistics of a large number of applications. The equation is as follows: the latitude of Tongliao area is 45.5°, the front roof angle of the solar greenhouse is α=31°, the rear roof angle is β=40°, the span of L=14m is M is 2.4m, the horizontal projection length of the rear roof is L2=M×cosβ=1.84m, the mathematical equations of the span L, the rear wall height h, the rear roof panel projection length L2, and the total height H are: H=(L-L2)*tanα=7.3m, h=H-L2*tanβ=5.3m.

[0138] The insulation blanket is made of multi-layer composite material with three layers of 4cm thickness;

[0139] Phase-change thermal storage and insulation wall panels: (150 mm thick extruded polystyrene (XPS) insulation board + 120 mm phase-change thermal storage and insulation wall panels obtained by the preparation method described in Examples 8 to 14 + 500 um nano thermal conductive coating); the solar greenhouse consists of an indoor floor, a 150 mm thick extruded polystyrene insulation board cold-proof wall to the local freezing line, a low wall on the sunny side and a roof panel.

[0140] 500um nano thermal conductive coating, take λ h =10w / mk; 150mm phase change thermal storage plateλ h =2.5w / mk;

[0141] External wall insulation XPS thickness = 150mm, λxps = 0.028w / mk;

[0142] Thermal insulation quilt thickness δw = 4cm + 4cm + 4cm, w = 0.035w / mk;

[0143] ∑R λ =(0.5*10 -3 / 10+0.12 / 2.5+0.15 / 0.028+0.12 / 0.035)=8.83,

[0144] K0=1 / (R i+∑Rλ+Re),

[0145] K0=1 / (0.115+8.83+0.0443)=1 / 8.99=0.11w / (m 2 .K)≤1.0w / (m 2 .K).

[0146] Table 6. Phase change thermal insulation wallboard flexible solar greenhouse wall performance indicators

[0147]

[0148] It can be seen from Table 6 that the wall heat transfer coefficient is significantly less than ≤1.0w / (m 2 .K).

[0149] Table 7. Temperature index of the wall of the flexible solar greenhouse with phase change thermal insulation wall panels

[0150]

[0151]

[0152] It can be seen from Table 7 that the flexible solar greenhouse can significantly increase the temperature inside the greenhouse and ensure that when the outdoor minimum temperature is -35°C, the average indoor night temperature reaches 17.9°C through the phase change heat storage and insulation wall panels of the present invention, which ensures the planting of crops while significantly improving the utilization rate of solar energy and saving energy.

[0153] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a waterproof and leakproof phase change thermal storage material, characterized in that: The following steps are involved: Step (1), dissolving a polyethylene glycol phase change thermal storage material in deionized water to form a uniform solution; adding a ring-opening catalyst and stirring evenly, slowly introducing a ring-opening reaction gas, and after the reaction is completed, adjusting the system to neutrality, washing with ethanol to remove unreacted impurities, and vacuum drying the product to obtain a hydroxylated phase change thermal storage material; Step (2), dissolving the hydroxylated phase change thermal storage material obtained in step (1) in a solvent to obtain a solution, adding a crosslinking catalyst to the solution, stirring evenly, slowly adding a crosslinking agent in a stirring state, stirring evenly, completing the reaction, removing the solvent, adding an antioxidant and a stabilizer, stirring evenly, and obtaining a crosslinked modified phase change thermal storage material; Step (3), adding an interface modifier to the inorganic porous material and mixing them evenly, heating and melting the cross-linked modified phase change thermal storage material obtained in step (2) at a temperature of 50-70° C. to become a liquid, adding a thermal conductive nano material and mixing them evenly, adding a binder to the mixed mixture and stirring them evenly, slowly stirring and adsorbing in a vacuum, and then cooling and solidifying naturally, thereby obtaining a phase change porous material loaded with the cross-linked modified phase change thermal storage material; Step (4), mixing the calcium carbonate powder containing stearic acid and the fly ash adsorbing fatty acids and heating to 130-160°C, adding the phase change porous material obtained in step (3), stirring evenly and introducing into a disc granulator for granulation, and cooling to obtain a waterproof and leakproof phase change thermal storage material.

2. The method for preparing a waterproof and leakproof phase change thermal storage material according to claim 1, characterized in that: The specific preparation of the calcium carbonate powder containing stearic acid is as follows: light calcium carbonate powder and stearic acid are heated at a constant temperature of 65-75° C., and are continuously stirred and mixed, and the mixture is obtained when a uniform layer of stearic acid is formed on the surface of the light calcium carbonate powder particles; The specific preparation of the fly ash adsorbing fatty acids is as follows: 1) adding a small amount of water to dry fly ash, stirring evenly, and then adding lime calcium powder, stirring to obtain a slurry so that the potential on the surface of the fly ash particles is positive; 2) adding fatty acids to water, and adding a surfactant to emulsify it so that the potential on the surface of the fatty acids is negative; 3) adding the fatty acid emulsion emulsified in step 2) to the slurry obtained in 1) at room temperature, stirring to allow the fatty acids to be fully adsorbed on the fly ash particles; 4) the fly ash that is fully adsorbed in step 3) is allowed to stand to remove the supernatant, and then heated and dried below the fatty acid phase transition temperature to obtain the fly ash adsorbing fatty acids.

3. The method for preparing a waterproof and leakproof phase change thermal storage material according to claim 2, characterized in that: The fatty acid is one or a combination of two of octanoic acid, decanoic acid, n-dodecanoic acid, n-tetradecanoic acid, and n-hexadecanoic acid; the surfactant is one of sodium dodecyl sulfate, sodium dodecyl ether sulfate, sodium dodecylbenzene sulfonate, sodium alkylbenzene sulfonate, sodium alkyl phosphate, sodium lauryl alcohol polyoxyethylene ether sulfate, and α-olefin sulfonate.

4. The method for preparing a waterproof and leakproof phase change thermal storage material according to claim 1, characterized in that: The polyethylene glycol phase change thermal storage material is one or two of PEG600, PEG1000, PEG2000, PEG4000, PEG6000, and PEG10000; the ring-opening catalyst is one of TiCl4, SnCl4, AlCl3, BF3, ZnCl2, and LiCl; the ring-opening reaction gas is one of ethylene oxide, propylene oxide, butylene oxide, oxadiene, octane oxide, decane oxide, and propylene glycol methyl ether acetate.

5. The method for preparing a waterproof and leakproof phase change thermal storage material according to claim 1, characterized in that: The cross-linking catalyst is one of TEA, DBTDL, TSP, TETA, MEA, MDEA, and TEOA; the cross-linking agent is one of isocyanate TDI, MDI, PAPI, HDI, IPDI, NDI, and HTDI.

6. The method for preparing a waterproof and leakproof phase change thermal storage material according to claim 1, characterized in that: The antioxidant and stabilizer are any two combinations of BHT, antioxidant 264, 4,4-di-tert-octyl-diphenylamine, tetramethylene β-pentaerythritol propionate, carbodiimide, UV-327, UV-531, Chimassorb944, and Tinuvin 765.

7. The method for preparing a waterproof and leakproof phase change thermal storage material according to claim 1, characterized in that: The interface modifier is one of silane coupling agents A-1100, A-174, A-186, A-187, A-151, and A-172; the inorganic porous material is one of perlite, vermiculite, montmorillonite, diatomaceous earth, volcanic rock, zeolite, medical stone, and coral stone.

8. The method for preparing a waterproof and leakproof phase-change thermal storage material according to claim 1, characterized in that: The thermally conductive nanomaterial is any combination of two of nano-SiO2, nano-TiO2, nano-Al2O3, nano-ZnO, nano-CuO, nano-Fe2O3, nano-graphene, and nano-carbon tubes; The adhesive is one of polyvinyl alcohol, urea-formaldehyde resin, sodium silicate, potassium silicate, polyvinyl acetate, VAE glue powder and acrylic glue powder.

9. A method for preparing a phase-change thermal storage and insulation wallboard, comprising: adding 500-700 parts of ordinary silicate cement, 15-25 parts of polystyrene particles, 300-350 parts of the waterproof and leak-proof phase-change thermal storage material according to any one of claims 1 to 9, 2-5 parts of polypropylene anti-cracking fibers, 3-6 parts of VAE glue powder, and 3-6 parts of hydroxypropyl methylcellulose, and mixing them uniformly at a water-to-material ratio of 1:1 to obtain a phase-change thermal storage slurry; placing a 10cm-15cm extruded insulation board at the bottom of a mold, applying a special interface agent for extruded insulation boards on the inner surface, laying anti-cracking glass fiber mesh cloth, pouring a 10cm-15cm thick phase change layer of the prepared phase-change thermal storage slurry, pressing the anti-cracking glass fiber mesh cloth into the surface, and adopting vibration molding and curing demolding.

10. A flexible solar greenhouse, characterized in that: The greenhouse includes a rear wall and side walls, and the rear wall and / or side wall are constructed with a keel. The phase change thermal storage insulation wall panel obtained by the preparation method according to claim 9 is installed on the inner side of the keel, and a nano thermal conductive coating layer is coated on the side of the phase change thermal storage insulation wall panel away from the extruded insulation board; or a 10-15 cm extruded insulation board is embedded on the inner side of the keel, a steel mesh is welded on the keel, and 10 cm-15 cm of the phase change thermal storage slurry according to claim 9 is applied. After curing and demolding, 200-500 um nano thermal conductive coating is sprayed.