Production method of low-alloy steel ultra-pure electroslag ingot
Through inverted packing operation and vacuum casting technology, the problems of high phosphorus slag fallback and secondary oxidation in electroslag ingot production are solved, and the production of electroslag ingot with ultra-low gas content is achieved, and the purity and performance of the product are improved.
Patent Information
- Application Number
- CN202411164277.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing electroslag ingot production process, the residual high phosphorus slag enters the ladle when the arc furnace is out of steel, resulting in the phosphorus component in LF refining exceeding the standard, and the atmospheric betting of the self-consumed electrodes leads to secondary oxidation of the molten steel, increasing oxygen, nitrogen and hydrogen. Gas elements affect product quality.
The inverted bag operation is used to transfer the arc furnace water into the LF furnace to prevent high phosphorus slag from entering the LF furnace. Then, the self-consumable electrode is poured in the vacuum casting system to ensure that the steel is poured in the vacuum state, avoid air contact, and control oxygen, nitrogen, The hydrogen content is at very low levels.
The production of electroslag ingots with ultra-low phosphorus, ultra-low oxygen, ultra-low nitrogen and ultra-low hydrogen has been achieved, ensuring the uniformity and purity of the product composition, improving the plasticity, fatigue strength and welding properties of the product, and reducing the risk of hydrogen embrittlement.
Smart Images

Figure CN118957283A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electroslag ingot production, and in particular to a method for producing an ultra-pure electroslag ingot of low alloy steel. Background Art
[0002] The current electroslag ingot preparation process is shown in Figure 1 The specific production process is as follows: (1) Before smelting in the electric arc furnace, high-quality scrap steel and alloys are carefully selected to control the content of the five harmful elements in the charge to avoid the five harmful elements affecting the performance of the final product; during smelting in the electric arc furnace, a reasonable slag making and power supply system is used to control the phosphorus content of the steel to be within 0.003%. After the phosphorus sampled in the furnace meets the requirements, the slag flow operation is carried out. After the temperature meets the requirements, the steel is tapped. During the tapping process, deoxidizers, alloys, slag, etc. are added with the steel flow, and deoxidation and alloying are performed after the furnace; (2) After the LF receives the steel, auxiliary materials are added to make slag. During the power supply process, powdered deoxidizer is used for diffusion deoxidation. After the slag turns completely white, VD operation is carried out. After VD, it returns to the LF furnace station for heating, and the composition and temperature are determined. After the pouring requirements are met, the ladle is used for pouring; (3) The atmospheric pouring method is used to produce consumable electrodes for electroslag remelting to produce electroslag ingots. The molten steel enters the ingot mold from the bottom through the center pouring pipe and the bottom plate, and multiple consumable electrodes can be poured at the same time; this method is to produce consumable electrodes in the atmosphere. After contact with the air, it will inevitably cause secondary oxidation of the molten steel; (4) After the consumable electrodes are polished and tested, they are used for electroslag remelting to produce electroslag ingots. Electroslag remelting is a method of smelting that uses the resistance heat generated when electric current passes through the molten slag as a heat source. The steel remelted by electroslag has the characteristics of low sulfur content, less non-metallic inclusions, smooth ingot surface, uniform and dense crystallization, and uniform metallographic structure and chemical composition.
[0003] The existing technology mainly has the following problems: 1. When the electric arc furnace is tapping steel, residual high-phosphorus slag enters the ladle, and phosphorus regeneration during the LF operation causes the composition to exceed the standard; 2. When the consumable electrodes are produced by atmospheric pouring, the molten steel is secondary oxidized in contact with the air, resulting in an increase in inclusions in the molten steel. The secondary oxidation causes an increase in oxygen, nitrogen and hydrogen gas elements in the molten steel. The atmospheric pouring method for producing consumable electrodes can cause the nitrogen in the molten steel to increase by 20-30ppm, the hydrogen to increase by 1-2ppm, and the oxygen in the steel to increase by 10-20ppm, which has a very serious impact on product quality.
[0004] Therefore, providing a method for producing electroslag ingots to solve the above problems is of great significance to the industry. Summary of the invention
[0005] In view of this, the present invention provides a method for producing ultra-pure electroslag ingots of low alloy steel. The technical solution of the present invention is as follows: a method for producing ultra-pure electroslag ingots of low alloy steel, the main process of which is: After smelting in the electric arc furnace, the steel is tapped normally, and no deoxidation or alloying operations are performed after the furnace. The molten steel from the electric arc furnace is injected into ladle B through the water inlet at the bottom of ladle A and then enters the LF furnace for refining. By pouring the molten steel, the high-phosphorus slag after dephosphorization in the electric arc furnace is left in ladle A to avoid excessive phosphorus content during sampling, testing and analysis due to phosphorus regeneration during LF refining. The ladle B after LF refining is directly poured into the vacuum pouring system to pour the consumable electrode; pouring under vacuum can avoid the problem of secondary oxidation caused by the contact between molten steel and air during the pouring process, so that the electroslag ingot has the advantages of ultra-low oxygen, ultra-low nitrogen and ultra-low hydrogen, among which the oxygen content is less than 20PPm, the nitrogen content is less than 30ppm, and the hydrogen content is less than 1ppm; the ultra-low oxygen, ultra-low nitrogen and ultra-low hydrogen consumable electrodes produced by this method are electroslag remelted in an argon atmosphere to produce electroslag ingots, which avoids secondary oxidation by air and removes non-metallic inclusions in the product to achieve the final ultra-purity requirements of the product.
[0006] The above-mentioned production method of ultra-pure electroslag ingot of low alloy steel also includes batching, controlling the mass percentage of five harmful elements in scrap steel and pig iron, among which As≤0.015%, Sn≤0.015%, Sb≤0.010%, Pb≤0.010%, Bi≤0.010%, and the total of the five harmful elements As+Sn+Sb+Pb+Bi≤0.035%.
[0007] Preferably, before charging the electric arc furnace, lime is added into the electric arc furnace, and the mass ratio of lime to scrap steel and pig iron is 3-5:100.
[0008] Preferably, when the temperature in the electric arc furnace is greater than 1530°C and the amount of slag in the furnace to the amount of molten steel is between 1 and 1.5:10, sampling is performed to detect the phosphorus content; when P≤0.002%, the next step is continued; when P≥0.0021%, slag is supplemented according to the weight ratio of lime to scrap steel and pig iron of 1 to 2:100 to perform dephosphorization operation.
[0009] Preferably, before the molten steel in the electric arc furnace is discharged, the mass percentages of the elements in the molten steel are as follows: C≤0.07%, Si≤0.01%, Mn≤0.20%, P≤0.002%, Cr≤0.30%, Ni=3.80%-4.80%, and Mo≤0.50%.
[0010] Preferably, in the LF refining furnace, aluminum ingots and ferrosilicon are added to the molten steel, the weight ratio of the aluminum ingot to the molten steel is 2.5:1000, and the weight ratio of the ferrosilicon to the molten steel is 3:1000.
[0011] Preferably, in the LF refining furnace, slag containing lime and fluorite is added to control the slag, the weight ratio of the slag to the molten steel is 25-40:1000, and the weight ratio of the lime to the fluorite is 4:1.
[0012] Preferably, the vacuum pouring system comprises a vacuum tank, which comprises a tank body and a tank cover detachably connected to the tank body, wherein the tank cover and the tank body form a closed space; a vacuum pump is provided on the tank body, and air is pumped out by the vacuum pump to maintain a vacuum state in the vacuum tank; A flow guide pipe is arranged on the tank body, a chassis is arranged inside the tank body, a consumable electrode mold is fixed on the chassis, and a liquid injection pipe on the consumable electrode mold corresponds to the outlet position of the flow guide pipe; When in use, the water inlet of ladle B is connected to the guide tube, and molten steel is injected into the consumable electrode mold; since the outlet of the guide tube is located in the tank body, and the consumable electrode mold is located in the tank body, the consumable electrode mold casting process is carried out in a vacuum state, thereby effectively avoiding the secondary oxidation of the molten steel by air and achieving the purpose of low oxygen, low nitrogen and low hydrogen.
[0013] Preferably, a movable handle is provided on the tank cover to facilitate operation of the tank cover to separate it from the tank body; and an observation hole is provided on the tank body.
[0014] Compared with the prior art, the beneficial effects of the present invention are: 1. In the present invention, the density of slag is less than that of molten steel and slag floats on the molten steel. The molten steel after tapping from the electric arc furnace passes through the water inlet at the bottom of ladle A and is poured into ladle B. The water inlet is closed after the molten steel flows out, so that the high-phosphorus slag of the electric arc furnace can be prevented from entering the ladle B to the greatest extent. After the electric arc furnace taps, the ladle is poured to avoid phosphorus return during LF refining, so as to achieve the purpose of ultra-low phosphorus production.
[0015] 2. The vacuum casting system is used to replace the atmospheric casting to produce consumable electrodes, avoiding the secondary oxidation of molten steel by air, so that the product can achieve the goals of ultra-low oxygen, ultra-low nitrogen and ultra-low hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0017] Figure 1 This is the production flow chart of conventional electroslag ingots.
[0018] Figure 2 This is a production flow chart of the ultra-pure electroslag ingot of the present invention.
[0019] Figure 3 Schematic diagram of molten steel pouring.
[0020] Figure 4 This is a schematic diagram of the production of consumable electrodes used in the production of ultra-pure electroslag ingots according to the present invention.
[0021] In the figure, 1- ladle A, 2- ladle B, 3- slag, 4- molten steel in electric arc furnace, 5- tank body, 6- tank cover, 7- vacuum pump, 8- flow guide pipe, 9- chassis, 10- consumable electrode mold, 11- moving handle, 12- observation hole, 13- molten steel in LF refining furnace, 14- center injection pipe. DETAILED DESCRIPTION
[0022] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0023] Example 1 Combination Figure 2-Figure 4 , a method for producing ultra-pure electroslag ingots of low alloy steel, the process is as follows: (1) Batching operation: 37,000 kg of scrap steel, 12,000 kg of pig iron and 2,200 kg of electrolytic nickel were selected for the production of electric arc furnaces. The five harmful elements in the scrap steel were analyzed as follows: As = 0.002%, Sn = 0.003%, Sb = 0.003%, Pb = 0.001%, Bi = 0.002%; the five harmful elements in the pig iron were analyzed as follows: As = 0.0035%, Sn = 0.0004%, Sb = 0.001%, Pb = 0.0001%, Bi = 0.0001%; through the selection of raw materials, the five harmful elements in the molten steel were As ≤ 0.015%, Sn ≤ 0.015%, Sb ≤ 0.010%, Pb ≤ 0.010%, Bi ≤ 0.010%, and the sum of the five harmful elements As + Sn + Sb + Pb + Bi ≤ 0.035%; (2) Electric arc furnace operation: Before charging the electric arc furnace, according to the quality of the total charge (scrap steel + pig iron + nickel plate), 2560kg of lime is added to the furnace bottom for slag making and dephosphorization. After adding the selected total charge, high voltage electricity is sent to start melting. Oxygen is blown in the early stage to assist melting of the charge. When the temperature in the furnace is 1550℃, the steel liquid P is sampled and analyzed to be 0.0019%. If it passes the inspection, oxygen is blown to decarburize and heat up. Sampling analysis before steel tapping shows that the weight ratios of the elements in the molten steel are as follows: C = 0.070%, Si = 0.0036%, Mn = 0.142%, P = 0.0015%, Cr = 0.134%, Ni = 3.97%, Mo = 0.020%; the steel tapping temperature is 1670°C, and the ladle operation is adopted; (3) Reverse packaging operation: In order to maximize the low phosphorus requirements of the product, the molten steel enters the ladle A after the electric arc furnace is tapped. Deoxidation operation is not allowed in the ladle A. The ladle inversion mode is adopted. Figure 3 , the molten steel flows from the bottom water inlet of ladle A1 to ladle B2. When slag is seen flowing out of the bottom water inlet of ladle A1, the water inlet is immediately closed to keep the high-phosphorus slag in the electric arc furnace in the inverted ladle A1; (4) LF refining operation: Through the ladle pouring operation, the molten steel from the electric arc furnace is added to the ladle B2 through the ladle A1, and 120kg aluminum ingots, 144kg ferrosilicon, 300kg electrolytic nickel, 317kg ferromolybdenum, 670kg micro-carbon ferrochrome, and 175kg metallic manganese are added to the ladle B2. The weight ratio of the aluminum ingot to the molten steel is 2.5:1000, the weight ratio of ferrosilicon to the molten steel is 3:1000, the weight of the added electrolytic nickel is controlled according to the product Ni component target value of 4.60%, the weight of the added ferromolybdenum is controlled according to the product Mo component target value of 0.45%, the weight of the added micro-carbon ferrochrome is controlled according to the product Cr component target value of 1.00%, and the weight of the added metallic manganese is controlled according to the product Mn component target value of 0.50%; After ladle A is poured into ladle B, the slag is controlled and 1440kg of lime and 360kg of fluorite are added to ladle B; In order to control the gas content in the molten steel, the electrolytic nickel, ferromolybdenum, low carbon ferrochrome, ferrovanadium, metal manganese and other alloy materials and slag materials such as lime and fluorite added to ladle B must be baked; the baking temperature is in accordance with the following principles: the baking temperature of electrolytic nickel, ferromolybdenum, low carbon ferrochrome, ferrovanadium, metal manganese and other alloy materials is 500℃, and the baking time is 24h; the baking temperature of slag materials such as lime and fluorite is 200℃, and the baking time is 4h; The LF furnace was adjusted to the maximum level 1 and the current was adjusted to 25000A before power was supplied to increase the temperature. 80kg of ferrosilicon powder was added for diffusion deoxidation. The composition was adjusted after the slag turned white and the temperature was ≥1600℃. When the temperature was greater than 1660℃, VD was performed to reduce the content of gas elements in the molten steel. After VD, the gas contents were sampled and analyzed as follows: oxygen = 19.3PPM, hydrogen = 0.9PPM, nitrogen = 32PPM. The temperature reached 1638℃ before steel pouring. Diffusion deoxidation is a deoxidation method in the refining furnace, which aims to reduce the oxygen content of molten steel; (5) Consumable electrode casting operation: Combination Figure 4 The vacuum casting system includes a vacuum tank, which includes a tank body 5 and a tank cover 6 detachably connected to the tank body 5, wherein the tank cover 6 and the tank body 5 form a closed space; a vacuum pump 7 is provided on the tank body 5, and air is pumped by the vacuum pump 7 to maintain a vacuum state in the vacuum tank; A flow guide tube 8 is provided on the tank body 5, a chassis 9 is provided inside the tank body 5, a consumable electrode mold 10 is fixed on the chassis 9, and a liquid injection tube on the consumable electrode mold 10 corresponds to the outlet position of the flow guide tube 8; When in use, the water inlet of the ladle B2 is connected to the guide pipe 8, and the LF refining furnace molten steel 13 is injected into the consumable electrode mold 10; since the outlet of the guide pipe 8 is located in the tank body 5, and the consumable electrode mold 10 is located in the tank body 5, the pouring process of the consumable electrode mold 10 is carried out in a vacuum state, thereby effectively avoiding the secondary oxidation of the molten steel by air, and achieving the purpose of low oxygen, low nitrogen, and low hydrogen; A movable handle 11 is provided on the tank cover to facilitate the operation of the tank cover 6 to separate it from the tank body; an observation hole 12 is provided on the tank body 5; After the chassis 9, the consumable electrode mold 10, and the middle pouring pipe 14 are assembled, they are baked and dried, and the pouring guide pipe is baked to 900°C; in order to avoid excessive gas content caused by molten steel contacting the air during the pouring process, ladle B2 is used as the intermediate ladle for vacuum pouring during the consumable electrode pouring. Ladle B2 is directly placed on the vacuum tank for pouring to avoid the increase of oxygen, nitrogen and hydrogen content caused by the contact of molten steel with the air during the pouring process. After the ladle B2 water outlet is drained, the ladle is hoisted to the pouring position and vacuum is started. When the vacuum in the vacuum tank is When the temperature of the molten steel reaches 133Pa, it is 1592℃. The ladle water inlet is opened to start pouring the consumable electrode. After cooling and demoulding, the sample composition of the consumable electrode body is as follows: C=0.114%, Si=0.391%, Mn=0.505%, P=0.0021%, S=0.0003%, Cr=1.05%, Mo=0.45%, Ni=4.8%, Al=0.0154%, O=18.3PPm, N=27PPM, H=0.4PPM; (6) Electroslag remelting operation: After the consumable electrode is demoulded, the riser is cut off, and the surface is polished and inspected, it is electroslag remelted. When the consumable electrode is electroslag remelted, the electroslag furnace uses argon gas for protection to avoid secondary oxidation of the product by air. Under the protection of argon atmosphere, an electroslag ingot with high purity, few non-metallic inclusions, uniform metallographic structure and chemical composition is obtained; the chemical composition of the final electroslag ingot is: C=0.109%, Si=0.385%, Mn=0.51%, P=0.0022%, S=0.0003%, Cr=1.03%, Mo=0.48%, Ni=4.89%, Al=0.019%, O=16.5PPm, N=28PPM, H=0.6PPM; the grade of non-metallic inclusions in the final electroslag ingot is shown in Table 1 below; Table 1 Non-metallic inclusion grade of electroslag ingot in Example 1 category Type A sulfide inclusions Type B alumina inclusions Type C silicate inclusions Type D spherical oxide inclusions DS type single particle spherical inclusion Fine series (level) Level 0 Level 0.5 Level 0 Level 0 Level 0 Coarse series (grade) Level 0 Level 0 Level 0 Level 0 Level 0 Example 2 Combination Figure 2-Figure 4, a method for producing ultra-pure electroslag ingots of low alloy steel, the process is as follows: (1) Batching operation: 10,000kg of selected scrap steel, 12,000kg of pig iron, 27,000kg of low-alloy steel return scrap steel, and 900kg of electrolytic nickel are used in the production of electric arc furnaces. The low-alloy steel return scrap steel is the residual material after product processing. Its composition is the same as the smelting material. The five harmful elements are: As=0.004%, Sn=0.0024%, Sb=0.0004%, Pb=0.00035%, Bi=0.0002%; the five harmful elements in scrap steel The five harmful elements in scrap steel are analyzed as follows: As=0.002%, Sn=0.003%, Sb=0. 0.003%, Pb=0.001%, Bi=0.002%; the chemical analysis values of the five harmful elements in pig iron are: As=0.0035%, Sn=0.0004%, Sb=0.001%, Pb=0.0001%, Bi=0.0001%; by selecting raw materials and combining some low-alloy returned scrap steel, the five harmful elements in molten steel are As≤0.015%, Sn≤0.015%, Sb≤0.010%, Pb≤0.010%, Bi≤0.010%, and the sum of the five harmful elements As+Sn+Sb+Pb+Bi≤0.035%; (2) Electric arc furnace operation: Before charging the electric arc furnace, according to the mass of the total charge (scrap steel + pig iron + nickel plate), 2500 kg of lime is added to the furnace bottom for slagging and dephosphorization. After adding the selected raw materials in step (1), high voltage electricity is sent to start melting. Oxygen is blown in the early stage to assist in melting the charge. When the temperature in the furnace is 1555°C, the molten steel P is sampled and analyzed to be 0.0019%, and the test is qualified. Oxygen is blown to decarburize and heat up. Sampling analysis before steel tapping shows that the weight ratios of the elements in the molten steel are as follows: C=0.055%, Si=0.0029%, Mn=0.185%, P=0.0019%, Cr=0.234%, Ni=4.11%, Mo=0.201%. After steel tapping, the ladle is inverted, and deoxidation is not allowed in the ladle. The tapping temperature is 1678℃. (3) Reverse packaging operation: In order to maximize the low phosphorus requirements of the product, the molten steel enters the ladle A after the electric arc furnace is tapped. Deoxidation operation is not allowed in the ladle A. The ladle inversion mode is adopted. Figure 3 , the molten steel flows from the bottom water inlet of ladle A1 to ladle B2. When slag is seen flowing out of the bottom water inlet of ladle A1, the water inlet is immediately closed to keep the high-phosphorus slag in the electric arc furnace in the inverted ladle A1; (4) LF refining operation: Through the ladle pouring operation, the molten steel from the electric arc furnace is added to the ladle B through the ladle A. 118kg of aluminum ingots, 140kg of ferrosilicon, 230kg of electrolytic nickel, 325kg of ferromolybdenum, 600kg of micro-carbon ferrochrome and 151kg of metallic manganese are added to the ladle B. The weight ratio of aluminum ingots to molten steel is 2.5:1000, the weight ratio of ferrosilicon to molten steel is 3:1000, the weight of electrolytic nickel added is controlled according to the product Ni component target value of 4.60%, the weight of ferromolybdenum added is controlled according to the product Mo component target value of 0.45%, the weight of micro-carbon ferrochrome added is controlled according to the product Cr component target value of 1.00%, and the weight of metallic manganese added is controlled according to the product Mn component target value of 0.50%.
[0024] After pouring the ladle, control the slag and add 1440kg of lime and 360kg of fluorite slag into ladle B; In order to control the gas content in the molten steel, the electrolytic nickel, ferromolybdenum, low carbon ferrochrome, ferrovanadium, metal manganese and other alloy materials and lime, fluorite and other slag materials entering the furnace must be baked; the baking temperature follows the following principles: the baking temperature of electrolytic nickel, ferromolybdenum, low carbon ferrochrome, ferrovanadium, metal manganese and other alloy materials = 500℃, baking time = 24h, the baking temperature of lime and fluorite and other slag materials is 200℃, baking time = 4h; The LF furnace was adjusted to the maximum gear 1 and the current was adjusted to 25000A, and then the power was supplied to increase the temperature. 80kg of ferrosilicon powder was added for diffusion deoxidation. The composition was adjusted after the slag turned white and the temperature was ≥1600℃. When the temperature was greater than 1660℃, VD was performed to reduce the content of gas elements in the molten steel. After VD, the gas contents were sampled and analyzed, respectively: oxygen = 15.3PPM, hydrogen = 0.8PPM, nitrogen = 33PPM. After the temperature reached 1635℃, the steel was poured. (5) Consumable electrode casting operation: Combination Figure 4 The vacuum casting system includes a vacuum tank, which includes a tank body 5 and a tank cover 6 detachably connected to the tank body 5, wherein the tank cover 6 and the tank body 5 form a closed space; a vacuum pump 7 is provided on the tank body 5, and air is pumped by the vacuum pump 7 to maintain a vacuum state in the vacuum tank; A flow guide tube 8 is provided on the tank body 5, a chassis 9 is provided inside the tank body 5, a consumable electrode mold 10 is fixed on the chassis 9, and a liquid injection tube on the consumable electrode mold 10 corresponds to the outlet position of the flow guide tube 8; When in use, the water inlet of the ladle B2 is connected to the guide pipe 8, and the LF refining furnace molten steel 13 is injected into the consumable electrode mold 10; since the outlet of the guide pipe 8 is located in the tank body 5, and the consumable electrode mold 10 is located in the tank body 5, the pouring process of the consumable electrode mold 10 is carried out in a vacuum state, thereby effectively avoiding the secondary oxidation of the molten steel by air, and achieving the purpose of low oxygen, low nitrogen, and low hydrogen; A movable handle 11 is provided on the tank cover to facilitate the operation of the tank cover 6 to separate it from the tank body; an observation hole 12 is provided on the tank body 5; After the chassis 9, the consumable electrode mold 10, and the middle pouring pipe 14 are assembled, they are baked and dried, and the pouring guide pipe is baked to 900°C; in order to avoid excessive gas content caused by molten steel contacting the air during the pouring process, ladle B2 is used as the intermediate ladle for vacuum pouring during the consumable electrode pouring. Ladle B2 is directly placed on the vacuum tank for pouring to avoid the increase of oxygen, nitrogen and hydrogen content caused by the contact of molten steel with the air during the pouring process. After the ladle B2 water outlet is drained, the ladle is hoisted to the pouring position and vacuum is started. When the vacuum degree in the vacuum tank is When the temperature of the molten steel reaches 133Pa, it is 1590℃. The ladle water inlet is opened to start pouring the consumable electrode. After cooling and demoulding, the sample composition of the consumable electrode body is as follows: C=0.102%, Si=0.294%, Mn=0.611%, P=0.0025%, S=0.0004%, Cr=0.621%, Mo=0.613%, Ni=5.15%, Al=0.0133%, O=13.3PPm, N=27PPM, H=0.5PPM; (6) Electroslag remelting operation: After the consumable electrode is demoulded, the riser is cut off, and the surface is polished and inspected, it is electroslag remelted. When the consumable electrode is electroslag remelted, the electroslag furnace uses argon gas for protection to avoid secondary oxidation of the product by air. Under the protection of argon atmosphere, an electroslag ingot with high purity, few non-metallic inclusions, uniform metallographic structure and chemical composition is obtained; the chemical composition of the final electroslag ingot is: C=0.101%, Si=0.286%, Mn=0.599%, P=0.0026%, S=0.0003%, Cr=0.625%, Mo=0.615%, Ni=5.18%, Al=0.016%, O=12.2PPm, N=29PPM, H=0.6PPM; the grade of non-metallic inclusions in the final electroslag ingot is shown in Table 2, as follows: Table 2 Non-metallic inclusion grades of electroslag ingots in Example 2 category Type A sulfide inclusions Type B alumina inclusions Type C silicate inclusions Type D spherical oxide inclusions DS type single particle spherical inclusion Fine series (level) Level 0 Level 0.5 Level 0 Level 0.5 Level 0 Coarse series (grade) Level 0 Level 0 Level 0 Level 0 Level 0 Compared with conventional processes, the method of the present invention can significantly reduce the contents of oxygen, nitrogen and hydrogen in the product; among them, the reduction of oxygen content can improve the plasticity of the product, which has an important influence on improving the fatigue strength and impact toughness of the product; the reduction of nitrogen content can significantly reduce the strength of steel, significantly improve the plasticity, especially toughness, improve the weldability and cold brittleness of the material, and improve the cold bending performance of the material; the reduction of hydrogen content can significantly improve the "hydrogen embrittlement" of the product material.
[0025] It can be seen that the present invention provides a technology for smelting, pouring and producing ultra-pure molten steel and electroslag ingots; the crude molten steel smelted in the electric arc furnace enters the LF refining furnace for smelting after the ladle inversion operation, and the high-phosphorus slag of the electric arc furnace is retained in the ladle A by the ladle inversion, so as to avoid the molten steel from returning to phosphorus during the LF refining process, resulting in excessive phosphorus during sampling and analysis. The LF furnace adopts a full-process white slag making operation to control the total oxygen in the steel within 20PPm, and after complete deoxidation, a vacuum pouring system is adopted to reduce the vacuum tank pressure to below 133Pa. The pure molten steel smelted in the LF furnace is poured into a consumable electrode under vacuum, and while avoiding the secondary oxidation of the molten steel by air during atmospheric pouring, the tasks of deoxidation / nitrogenation / dehydrogenation can be achieved, and the requirements for producing ultra-pure consumable electrodes can be met; the consumable electrode is used for electroslag remelting to produce electroslag ingots after being polished and inspected, so as to realize the production of ultra-pure electroslag ingots; due to the above advantages, the consumable electrode is now widely used in the production of electroslag ingots for large forgings required in the fields of power, shipbuilding, metallurgy, petrochemical, heavy machinery, and national defense.
[0026] Although the present invention has been described in detail by reference to the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.
Claims
1. A method for producing ultra-pure electroslag ingots of low alloy steel, It is characterized in that The main process is: After smelting in the electric arc furnace, the steel is tapped normally, and no deoxidation or alloying operation is performed after the furnace. The molten steel from the electric arc furnace is injected into ladle B through the water inlet at the bottom of ladle A and then enters the LF furnace for refining. By pouring the molten steel, the high-phosphorus slag after dephosphorization in the electric arc furnace is left in ladle A. After LF refining, ladle B is directly poured into the vacuum pouring system to pour the consumable electrode; pouring under vacuum makes the oxygen content of the electroslag ingot less than 20PPm, the nitrogen content less than 30ppm, and the hydrogen content less than 1ppm; the ultra-low oxygen, ultra-low nitrogen, and ultra-low hydrogen consumable electrodes produced by this method are electroslag remelted in an argon atmosphere to produce electroslag ingots to achieve the final ultra-purity requirements of the product.
2. The method for producing ultra-pure electroslag ingot of low alloy steel according to claim 1, It is characterized in that The production method of ultra-pure electroslag ingots of low-alloy steel also includes batching and controlling the mass percentage of five harmful elements in scrap steel and pig iron, wherein As≤0.015%, Sn≤0.015%, Sb≤0.010%, Pb≤0.010%, Bi≤0.010%, and the total of the five harmful elements As+Sn+Sb+Pb+Bi≤0.035%.
3. The method for producing ultra-pure electroslag ingot of low alloy steel as claimed in claim 2, It is characterized in that After batching and before charging the electric arc furnace, lime is added into the electric arc furnace. The mass ratio of lime to scrap steel and pig iron is 3~5:
100.
4. The method for producing ultra-pure electroslag ingot of low alloy steel as claimed in claim 3, It is characterized in that When the temperature in the electric arc furnace is greater than 1530℃ and the amount of slag to molten steel in the furnace is between 1~1.5:10, take samples to detect the phosphorus content; when P≤0.002%, proceed to the next step; when P≥0.0021%, add slag according to the weight ratio of lime to scrap steel and pig iron of 1~2:100 to carry out dephosphorization operation.
5. The method for producing ultra-pure electroslag ingot of low alloy steel as claimed in claim 4, It is characterized in that Before the molten steel comes out of the electric arc furnace, the mass percentage of each element in the molten steel is as follows: C≤0.07%, Si≤0.01%, Mn≤0.20%, P≤0.002%, Cr≤0.30%, Ni=3.80%-4.80%, Mo≤0.50%.
6. The method for producing ultra-pure electroslag ingot of low alloy steel according to claim 5, It is characterized in that In the LF refining furnace, aluminum ingots and ferrosilicon are added to the molten steel. The weight ratio of aluminum ingots to molten steel is 2.5:1000, and the weight ratio of ferrosilicon to molten steel is 3:1000.
7. The method for producing ultra-pure electroslag ingot of low alloy steel according to claim 6, It is characterized in that In the LF refining furnace, slag is controlled by adding lime and fluorite. The weight ratio of slag to molten steel is 25~40:1000, and the weight ratio of lime to fluorite is 4:
1.
8. The method for producing ultra-pure electroslag ingot of low alloy steel according to claim 1, It is characterized in that The vacuum pouring system comprises a vacuum tank, which comprises a tank body and a tank cover detachably connected to the tank body, wherein the tank cover and the tank body form a closed space; a vacuum pump is provided on the tank body; A flow guide pipe is arranged on the tank body, a chassis is arranged inside the tank body, a consumable electrode mold is fixed on the chassis, and a liquid injection pipe on the consumable electrode mold corresponds to the outlet position of the flow guide pipe.
9. The method for producing ultra-pure electroslag ingot of low alloy steel as claimed in claim 8, It is characterized in that The tank cover is provided with a moving handle; and the tank body is provided with an observation hole.