Copper strip for tab material and preparation method of copper strip

By optimizing the casting and processing technology of copper materials, the problems of poor surface consistency and smoothness of copper materials for the middle ear materials of new energy vehicles are solved, and the preparation of high-quality copper tape is realized to meet the high surface quality needs of new energy vehicles.

CN118957352APending Publication Date: 2024-11-15CHINALCO DAYE COPPER PLATE & STRIP CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411062453.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The production of copper materials for the middle ear materials of new energy vehicles has immature casting blank stability control, colorless rolling, brushless texture annealing and cleaning and damage-free shearing technology, resulting in poor surface consistency and smoothness of the product, and there is a situation after electroplating. Surface defects such as chromatic aberration and color spots and low adhesion.

Method used

By optimizing raw material control, deoxygenation and degassing of melting furnace, purification and decomposition of insulation furnace, reasonable matching of casting temperature and casting speed, vertical electromagnetic continuous casting technology is used, combining hot rolling treatment, rough rolling treatment, annealing treatment, finishing treatment and After multiple post-treatment, a copper tape for high-quality electrode material was prepared to control surface roughness, conductivity and tensile strength to ensure zero defects after nickel plating.

Benefits of technology

It achieves uniform and consistent surface quality and zero defects of copper tape, meets the demand for copper for high-surface quality electrode materials in new energy vehicles, improves the mechanical properties and conductivity of the product, reduces the formation of copper oxide skin, and solves the problem of Surface oxide layer residue problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957352A_ABST
    Figure CN118957352A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of copper material processing, in particular to a copper strip for a tab material and a preparation method thereof.The copper strip for the tab material comprises, by mass, more than 99.95% of Cu, less than 0.001% of O, less than 0.004% of Fe and the balance inevitable impurities, by optimizing rolling parameters such as the roller roughness, the rolling pass and the rolling medium and cooperatively controlling the annealing process and the cleaning and oil removing process, a color difference-free rolling control technology is formed, the surface of the strip is free of macroscopic surface lines, the shearing technology is optimized and controlled, and the lossless shearing effect is achieved. The method has the advantages of being high in market competitiveness, remarkable in economic benefit and high in product yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of copper material processing, and in particular to a copper strip for tab material and a preparation method thereof. Background Art

[0002] With the rise of a new round of scientific and technological revolution and industrial transformation, the new energy vehicle industry has entered a stage of accelerated development. After years of continuous efforts, my country's new energy vehicle industry has significantly improved its technical level, improved its industrial system, and greatly enhanced its corporate competitiveness, presenting a good situation of "double improvement" in market scale and development quality. Especially under the goal of achieving "dual carbon" globally, the development of new energy has received more attention because it helps reduce greenhouse gas emissions, respond to climate change challenges, and improve the global ecological environment. Copper is a key material in core components of new energy vehicles such as power batteries, motors, wiring harnesses and connections, electronic controls and terminals. With the rapid development of the domestic new energy vehicle industry, higher requirements are placed on the performance and surface quality of copper materials used in new energy vehicles.

[0003] The copper used in the tab materials of new energy vehicles has good electrical conductivity, thermal conductivity and bending performance. The current technical bottlenecks in the production of domestic tab materials are mainly the immature technology of ingot stability control, color difference-free rolling, brushless annealing and cleaning, and damage-free shearing, which makes the surface consistency and finish of the product poor, resulting in surface defects such as color difference and color spots after electroplating, as well as low adhesion. As a result, it is impossible to produce copper materials for tabs that meet the market's requirements for O content ≤10PPM, P content <3PPM, 180-degree repeated bending performance ≥7 times, clean and bright surface without black silk, uniform color without color difference, and no surface damage, especially the needs of downstream customers for high surface quality copper for tab materials. Summary of the invention

[0004] In view of this, the present invention provides a copper strip for tab material and a preparation method thereof, so as to achieve the requirements of uniform surface quality of the entire roll of copper material, consistent surface after nickel plating, zero defects, etc., thereby meeting the development needs of copper strip for tab material with high surface quality for new energy vehicles.

[0005] To solve the above problems, the present invention provides a copper strip for tab material on one hand. The copper strip for tab material comprises the following components in mass percentage: Cu content>99.95%, O content<0.001%, Fe content<0.004%, and the remainder is unavoidable impurities.

[0006] The surface roughness of the copper strip for the tab material of the present invention is 0.12-0.15 μm, the number of 360° bending times of the copper strip for the tab material is ≥8, the conductivity of the copper strip for the tab material is 100.1-102.4% IACS, the surface of the copper strip for the tab material is zero-defect after the whole roll of nickel plating is treated, the tensile strength of the copper strip for the tab material is 220-250 MPa, and the elongation is 30-40%.

[0007] A second aspect of the present invention provides a method for preparing a copper strip for a tab material, the method specifically comprising the following steps:

[0008] S1. Raw materials for preparing copper strips for tab materials;

[0009] S2, sequentially performing baking treatment and smelting treatment on the raw materials prepared in step S1 to obtain an intermediate melt;

[0010] S3, subjecting the intermediate melt obtained in step S2 to heat preservation treatment, and then subjecting the intermediate melt to vertical full-continuous casting to obtain a copper ingot;

[0011] S4, sequentially subjecting the copper ingot obtained in step S3 to heating treatment and hot rolling treatment to obtain a hot-rolled billet;

[0012] S5, subjecting the hot-rolled billet obtained in step S4 to milling treatment, rough rolling treatment and annealing treatment in sequence, and then performing a post-treatment to obtain a rough-rolled billet;

[0013] S6, subjecting the rough rolled billet obtained in step S5 to finish rolling, secondary post-processing and annealing in sequence, and then performing three post-processing to obtain a finished rolled strip;

[0014] S7, shearing the finished rolled strip obtained in step S6 to obtain a copper strip for tab material.

[0015] In some embodiments, in step S2, the Cu in the raw material is high-purity electrolytic copper with a purity of >99.99%, and the parameters of the baking treatment are as follows: temperature is 180-220° C., and time is 10-15 min.

[0016] In some embodiments, in step S2, dry charcoal is added as a cover during the smelting process and high-purity argon is blown at the bottom, wherein the cover thickness of the dry charcoal is 150-200 mm, and the smelting temperature is 1180-1250°C.

[0017] In some embodiments, in step S3, the insulation treatment is performed in an insulation furnace and covered with spherical graphite particles, and the temperature of the insulation treatment is 1180-1200°C.

[0018] In some embodiments, in step S3, the vertical full continuous casting process is assisted by an electromagnetic stirring device, and the parameters of the vertical full continuous casting are as follows: temperature is 1160-1180°C, speed is 75-95mm / min, vibration frequency is 35-45 times / min, cooling water pressure is 0.5-0.6MPa; the frequency of the electromagnetic stirring device is 20Hz, and the current is 20-24A.

[0019] In some embodiments, in step S4, the heating treatment is performed in a walking beam furnace, the air-fuel ratio of the walking beam furnace is 8-9, and the oxide scale is sucked out before leaving the furnace.

[0020] In some embodiments, in step S4, the parameters of the hot rolling process are as follows: a total of 9 passes, and the deformation amount of the 7th pass is 42-48%.

[0021] In some embodiments, in step S5, the rough rolling process is performed for 8 passes, and the roll roughness of the first pass is 0.6 μm and the pass reduction is 15-20%, and the roll roughness of the eighth pass is 0.3 μm and the pass reduction is 35-40%.

[0022] In some embodiments, in step S5, the annealing treatment is performed in a bell furnace, and the parameters of the annealing treatment are as follows: temperature is 400-450° C., and time is 4-6 hours.

[0023] In some embodiments, in step S5, the post-treatment includes sequentially performing surface degreasing, pickling and grinding, and the abrasive mesh size of the grinding treatment is 2000-3000 mesh.

[0024] In some embodiments, in step S6, the finishing rolling process is performed for a total of 5 passes, and the viscosity of the rolling oil during the finishing rolling process is 6-8 mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 15-20%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 30-35%.

[0025] In some embodiments, in step S6, the secondary post-treatment includes sequentially performing surface degreasing, cleaning and drying.

[0026] In some embodiments, in step S6, the annealing treatment is performed in an air cushion furnace, and the parameters of the annealing treatment are as follows: a temperature of 500-550° C. and a passing speed of 50-60 m / min.

[0027] In some embodiments, in step S6, the three post-treatments include pickling, cleaning and passivation in sequence.

[0028] In some embodiments, in step S7, the shear tension is 20-40 Kgf, the tension accuracy is 3-5%, and the pressing force is 0.1-0.3 Kgf.

[0029] Compared with the prior art, the present invention has the following advantages:

[0030] The present invention optimizes raw material control, deoxidation and degassing of smelting furnace, purification and impurity removal of holding furnace, reasonable matching of casting temperature and casting speed, and utilizes vertical electromagnetic continuous casting technology to prepare high-quality copper ingots for tab materials, improve cracks, cold shuts, pores and other defects generated during the smelting and casting process, and effectively solve the problems of peeling, holes, inclusions and other defects on the surface of copper strips in the subsequent production process. The heating atmosphere and furnace pressure of the copper ingots for tab materials in the heating furnace are clarified, the formation of copper oxide scale is reduced, and the problem of residual oxide layer on the surface of copper strips is solved. In addition, hot rolling treatment, rough rolling treatment, annealing treatment, primary post-treatment, finishing rolling treatment, secondary post-treatment, annealing treatment and tertiary post-treatment can not only accurately control the final thickness and achieve the required dimensional accuracy, but also maintain good plate shape and surface quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a cross-sectional macroscopic structure diagram of the ingot of Example 1 of the present invention;

[0032] Figure 2 This is a microstructure diagram of the finished strip of Example 1 of the present invention;

[0033] Figure 3 This is the cross-sectional macroscopic structure diagram of the ingot of comparative example 1 of the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the embodiments of the present invention belong. If the definitions set forth in this section are contrary to or otherwise inconsistent with the definitions set forth in the patents, patent applications, published patent applications, and other publications incorporated herein by reference, the definitions listed in this section take precedence over the definitions incorporated herein by reference.

[0037] Unless otherwise specified, the methods used in the following examples are all conventional methods. Unless otherwise specified, the materials, reagents and instruments used are all conventional materials, reagents and instruments in the art, and can be obtained by those skilled in the art through commercial channels.

[0038] When an amount, concentration or other value or parameter is expressed as a range, a preferred range or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range. In the present specification and claims, range definitions can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.

[0039] In the prior art, the ingot has problems such as stability control, color-free rolling, brushless annealing and cleaning, and immature non-damage shearing technology, which results in poor surface consistency and finish of the product, and surface defects such as color difference and color spots after electroplating, as well as low adhesion. In order to solve the above technical problems, one aspect of the present invention provides a copper strip for tab material. The copper strip for tab material includes the following components in mass percentage: Cu content>99.95%, O content<0.001%, Fe content<0.004%, and the remainder is unavoidable impurities. In the actual application field, it is difficult to achieve 100% Cu element content in the composition of the copper strip. The present invention can ensure that the obtained copper strip is not affected by impurities O and Fe by limiting the content of impurities O and Fe. Among them, the two metals Cu and Fe have very different properties, have high positive enthalpy values, and belong to metastable immiscible alloys. It can be seen from the copper-iron alloy phase diagram that Cu and Fe phases basically do not undergo solid solution at room temperature, and there is a liquid phase immiscible gap at high temperature. Therefore, the present invention controls the content of Fe element to ensure that the obtained copper strip is not affected by Fe element; a small amount of oxygen in the copper strip will react with harmful impurities that affect the performance of the copper strip, reduce or eliminate the harmful effects of certain trace impurities, and play the role of a scavenger, but excessive oxygen will form excessive Cu with copper. 2 O forms an uneven distribution in the copper matrix, which will lead to the expansion of cracks. It is easy to cause work hardening and local cracks during deep processing of the copper strip. Therefore, the O content is controlled within the range of less than 0.001% in this application.

[0040] The surface roughness of the copper strip for tab material obtained by the element composition and preparation method of the present invention is 0.12-0.15 μm, the number of 360° bending times of the copper strip for tab material is ≥8, the conductivity of the copper strip for tab material is 100.1-102.4% IACS, the surface of the copper strip for tab material is zero defect after the whole roll is nickel-plated, the tensile strength of the copper strip for tab material is 220-250 MPa, and the elongation is 30-40%.

[0041] Another aspect of the present invention provides a method for preparing the copper strip for the tab material, which specifically comprises the following steps:

[0042] S1. Raw materials for preparing copper strips for tab materials;

[0043] S2, sequentially performing baking treatment and smelting treatment on the raw materials prepared in step S1 to obtain an intermediate melt;

[0044] S3, subjecting the intermediate melt obtained in step S2 to heat preservation treatment, and then subjecting the intermediate melt to vertical full-continuous casting to obtain a copper ingot;

[0045] S4, sequentially subjecting the copper ingot obtained in step S3 to heating treatment and hot rolling treatment to obtain a hot-rolled billet;

[0046] S5, subjecting the hot-rolled billet obtained in step S4 to milling treatment, rough rolling treatment and annealing treatment in sequence, and then performing a post-treatment to obtain a rough-rolled billet;

[0047] S6, subjecting the rough rolled billet obtained in step S5 to finish rolling, secondary post-processing and annealing in sequence, and then performing three post-processing to obtain a finished rolled strip;

[0048] S7, shearing the finished rolled strip obtained in step S6 to obtain a copper strip for tab material.

[0049] The present invention limits the elemental composition and combines the step-by-step preparation steps, that is, firstly, the raw materials are subjected to baking and smelting treatments to obtain an intermediate melt, and then the copper ingot is subjected to insulation and vertical full-continuous casting to obtain a copper ingot blank, and then the copper ingot blank is heated and hot-rolled to obtain a hot-rolled blank, and then the hot-rolled skin is subjected to finish rolling treatment, secondary post-treatment, annealing treatment and tertiary post-treatment in sequence to obtain a finished rolled strip, and finally shearing is performed to obtain a copper strip for tab materials. In the above preparation process, the inventors fully considered multiple factors, and after many practices, the final copper strip for tab materials can meet market requirements.

[0050] Furthermore, in step S2, in order to further improve the quality of the copper strip finally obtained, the Cu used in the raw material is high-purity electrolytic copper with a purity of >99.99%.

[0051] Furthermore, in step S2, the parameters of the baking treatment are as follows: the temperature is 180-220°C, and the time is 10-15 minutes. The present invention bakes the raw materials before smelting, the purpose of which is to remove the moisture in the electrolytic copper and the mixing of chemical substances such as acid remaining in the electrolytic copper, ensure the purity of the copper melt added to the melting furnace, and reduce the introduction of impurity elements.

[0052] Further, in step S2, dry charcoal is added to cover during the smelting process and high-purity argon is blown at the bottom, wherein the covering thickness of the dry charcoal is 150-200mm, and the temperature of the smelting process is 1180-1250°C. The purpose of adding dry charcoal during the smelting process of the present invention is that the charcoal can consume the oxygen in the furnace at high temperature, forming a reducing atmosphere, effectively preventing the copper liquid from being oxidized at high temperature, thereby maintaining the purity of the copper raw material and improving the surface quality of the casting. In addition, the present invention further limits the covering thickness of the dry charcoal, and within the above thickness range, it can ensure that the impurity oxygen content in the raw material is within the required range. The present invention further blows high-purity argon into the bottom during the smelting process, and its purpose is that argon is an inert gas, and hydrogen and other harmful gases in the copper liquid can be effectively removed by blowing argon at the bottom, achieving a good degassing effect, which is crucial to the mechanical processing performance and the physical and mechanical properties of the final product.

[0053] Further, in step S3, the insulation treatment is carried out in an insulation furnace, and spherical granular graphite is used for covering, and the temperature of the insulation treatment is 1180-1200°C. The present invention uses spherical granular graphite for covering during the insulation process, and its purpose is: the spherical granular graphite covers the surface of the copper alloy melt, which helps to form a relatively closed environment, reduces heat loss, and makes the temperature of the copper alloy more uniform and stable during the entire insulation process, which is very important for controlling the microstructure of the alloy; secondly, graphite has good antioxidant properties, can isolate oxygen in the air, and reduce the oxidation of copper liquid at high temperature, thereby ensuring the purity of the copper melt and avoiding the formation of oxidized inclusions, which is very important for improving the quality of the ingot. The present invention adopts an insulation treatment temperature of 1180-1200°C, and its purpose is: within the above temperature range, the elements in the raw materials can be fully dissolved and diffused to achieve the required homogenization, while avoiding excessively high temperatures that cause melt inhalation and affect the melt quality; too low temperatures affect the subsequent surface quality of the ingot.

[0054] Furthermore, in step S3, an electromagnetic stirring device is used in the vertical full continuous casting process, and the parameters of the vertical full continuous casting are as follows: temperature is 1160-1180°C, speed is 75-95mm / min, vibration frequency is 35-45 times / min, cooling water pressure is 0.5-0.6MPa; the frequency of the electromagnetic stirring device is 20Hz, and the current is 20-24A. The present invention is assisted by an electromagnetic stirring device in the vertical full continuous casting process, and its purpose is: through stirring, the elements in the copper melt can be more evenly distributed, avoiding component segregation, ensuring the performance consistency of the casting along the length direction, and electromagnetic stirring can affect the solidification process of the melt, promote the formation of crystallization cores, thereby refining the grains to a certain extent, and the fine grain structure can improve the mechanical properties of the material, such as strength and toughness.

[0055] Further, in step S4, the heating treatment is carried out in a walking furnace, the air-fuel ratio of the walking furnace heating is 8-9, and the oxide scale is sucked before the furnace is discharged. The heating treatment of the present invention is carried out in a walking furnace, and the air-fuel ratio of the heating in the walking furnace is further limited, and its purpose is: during the combustion process, the ratio of fuel to air is strictly controlled within this range to ensure efficient and economical combustion, while reducing pollutant emissions, and a reasonable air-fuel ratio is crucial to maintaining the temperature uniformity in the furnace, optimizing the combustion efficiency and controlling the atmosphere in the furnace. The purpose of the present invention further sucking the oxide scale before the furnace is discharged is that copper is easily formed during the heating process, especially when there are impurities on the surface or when heated in an oxidizing atmosphere. This layer of oxide scale not only affects the surface quality of the copper material, but may also cause pollution or defects in the subsequent processing process. Therefore, using a suction device to remove the oxide scale before the copper material is discharged can ensure that the surface of the copper material is clean, provide a good starting point for subsequent processing such as cold working, forging or the molding of the final product, and also improve the utilization rate of the material and the quality of the finished product.

[0056] Furthermore, in step S4, the parameters of the hot rolling process are as follows: a total of 9 passes are performed, and the deformation amount of the 7th pass is 42-48%.

[0057] Furthermore, in step S5, the rough rolling process is performed for 8 passes, and the roll roughness of the first pass is 0.6 μm, the pass reduction is 15-20%, and the roll roughness of the eighth pass is 0.3 μm, and the pass reduction is 35-40%.

[0058] The present invention adopts the above-mentioned hot rolling and rough rolling process, and further limits the roller roughness and pass reduction while limiting the above-mentioned number of passes, mainly because: the key deformation passes are controlled, and the purpose is to promote grain refinement and improve the comprehensive performance of the material, including surface quality. Too large a pass deformation may cause uneven stress and strain inside the material, thereby forming defects such as cracks and wrinkles on the surface. Too small a deformation requires more rolling passes to complete the required shape and size changes, which will increase production time and cost and reduce production efficiency. The risk of surface scratches, roller marks and other defects in the copper strip is increased, affecting the surface quality of the final product. Appropriate deformation helps to maintain the integrity of the material and reduce surface defects. Excessive deformation may increase the surface roughness, while appropriate deformation helps to maintain or improve the surface finish. The control of surface roughness is mainly because the roughness of the roller affects the friction condition during the rolling process of the copper material. Higher roughness can increase the friction between the roller and the material, which helps to deform the material. However, too high roughness may cause excessive friction, resulting in energy loss and roller surface wear. A lower roughness will reduce the friction between the copper material and the copper material, which may increase the material sliding during the rolling process, affecting the rolling stability and the forming quality. In addition, the roughness of the roller will affect the surface quality of the product. If the roller surface is too rough, the surface of the material after rolling may be uneven, affecting the appearance and quality of the product. If it is too low, the desired effect will not be achieved. Therefore, the present invention adopts the above-mentioned pass reduction to obtain a higher quality hot-rolled billet.

[0059] Further, in step S5, annealing is carried out in a bell furnace, and the parameters of the annealing are as follows: temperature is 400-450°C, and time is 4-6h. The annealing process of the present invention is carried out in a bell furnace, and its purpose is that the bell furnace can effectively prevent the copper material from oxidizing at high temperatures by evacuating or filling with protective gas in a closed environment, and maintain its surface finish and intrinsic quality; and the purpose of the present invention using the above annealing temperature is that: within this temperature range, the grains of the material can be rearranged under the action of thermal energy, eliminating deformation hardening and internal stress caused by cold working (such as rolling, drawing, etc.), while not causing excessive growth of the grains, maintaining good mechanical properties and processability; the present invention is combined with the above annealing temperature, and sets the annealing time to 4-6h, and its purpose is to ensure that the material has enough time to complete the recrystallization process, so that the microstructure of the material reaches a relatively stable state.

[0060] Further, in step S5, the post-treatment includes sequentially performing surface degreasing, pickling and grinding, and the abrasive mesh number of the grinding is 2000-3000 mesh. The degreasing is used to remove organic pollutants such as grease, oil, dust, etc. on the copper surface, the pickling is to remove the oxide scale, rust and slight unevenness on the copper surface, and any residual grease, and the grinding is to further refine the surface texture of the copper material and improve the surface finish.

[0061] Furthermore, in step S6, the finishing rolling process is performed for a total of 5 passes, and the viscosity of the rolling oil during the finishing rolling process is 6-8 mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 15-20%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 30-35%.

[0062] Compared with the prior art, the present invention adopts the above-mentioned parameters of the finishing rolling treatment, wherein the rolling oil plays a vital role in the finishing rolling process, and the viscosity described in the present invention can not only effectively reduce the friction and heat generation between the roller and the copper strip, protect the roller and the material from damage, but also ensure a good lubrication effect, help heat dissipation, and prevent the material from overheating during high-speed rolling; the roughness of the roller in the first pass is further limited because: the roller with lower roughness helps to form a uniform contact surface in the initial stage of finishing rolling, reduces scratches on the surface of the material, provides a good processing starting point for subsequent passes, and is also conducive to controlling the thickness deviation on the inlet and outlet sides of the material. difference, ensuring thickness uniformity; in addition, in the early stage of finishing rolling, a larger reduction (15-20%) helps to quickly thin the material, but at the same time it should be controlled to a level that does not cause excessive deformation or damage to the material, ensuring the continuity and uniformity of the material; compared with the first pass, the fifth pass uses a lower roll roughness (0.15μm), the purpose of which is to further refine the surface when approaching the final thickness, reduce surface defects, and improve the surface finish of the final product; as the material gradually becomes thinner, the reduction in the last pass will increase (30-35%) to accurately control the final thickness and achieve the required dimensional accuracy while maintaining good plate shape and surface quality.

[0063] Furthermore, in step S6, the secondary post-processing includes sequentially performing surface degreasing, cleaning and drying.

[0064] Further, in step S6, annealing treatment is carried out in an air cushion furnace, and the parameters of the annealing treatment are as follows: temperature is 500-550°C, and the passing speed is 50-60m / min. The present invention adopts the above-mentioned annealing temperature, which is optimized for the copper material of the present invention, and is used to alleviate the work hardening phenomenon and restore the plasticity of the material. In this temperature range, the lattice structure inside the copper is reorganized, the stress generated during the processing is eliminated, and the material becomes soft, which is convenient for subsequent processing or forming operations. The selection of temperature requires precise control. Too high a temperature may cause the material structure to be coarse and affect its performance; too low a temperature may not be fully annealed. The passing speed is set to 50-60m / min mainly to ensure that the material has enough residence time in the furnace to achieve a uniform temperature distribution and complete the necessary microstructural changes while maintaining production efficiency.

[0065] Further, in step S6, the three post-treatments include pickling, cleaning and passivation in sequence.

[0066] Further, in step S7, the shear tension is 20-40Kgf, the tension accuracy is 3-5%, and the pressing force is 0.1-0.3Kgf. The reason why the present invention adopts the above parameters is that the shear tension setting helps to improve the quality and efficiency of shearing, and high tension accuracy is crucial to ensure the consistency of the processing process and product quality, especially in the continuous production of high-precision copper products, and the pressing force range of 0.1-0.3Kgf can ensure accurate material positioning and avoid material deformation caused by excessive pressing force.

[0067] The technical effects of the present invention are described below in conjunction with specific embodiments.

[0068] Example 1

[0069] The present embodiment provides a copper strip for a tab material, which is composed of the following components by mass percentage: Cu content 99.992%, O content 0.0005%, Fe content 0.0001%, and the remainder is unavoidable impurities. The copper strip for a tab material in the present embodiment is prepared by the following method:

[0070] S1. Raw materials for preparing copper strips for tab materials;

[0071] S2, the raw material prepared in step S1 is subjected to baking treatment and smelting treatment in sequence to obtain an intermediate melt, wherein the Cu in the raw material is high-purity electrolytic copper with a purity of 99.995%, and the parameters of the baking treatment are as follows: the temperature is 180° C., the time is 15 min, and during the smelting treatment, dry charcoal is added for covering and high-purity argon is blown at the bottom, wherein the covering thickness of the dry charcoal is 200 mm, and the temperature of the smelting treatment is 1250° C.;

[0072] S3, subjecting the intermediate melt obtained in step S2 to insulation treatment, and then subjecting it to vertical full continuous casting to obtain a copper ingot, wherein the insulation treatment is carried out in a heat-insulating furnace, and is covered with spherical granular graphite, the temperature of the insulation treatment is 1200° C., and an electromagnetic stirring device is used in the vertical full continuous casting process, and the parameters of the vertical full continuous casting are as follows: temperature is 1180° C., speed is 75 mm / min, vibration frequency is 45 times / min, cooling water pressure is 0.5 MPa; the frequency of the electromagnetic stirring device is 20 Hz, and the current is 24 A;

[0073] S4, the copper ingot obtained in step S3 is subjected to heating treatment and hot rolling treatment in sequence to obtain a hot-rolled billet, wherein the heating treatment is carried out in a walking furnace, the air-fuel ratio of the walking furnace is 9, and the oxide scale is sucked out before being taken out of the furnace, and the parameters of the hot rolling treatment are as follows: a total of 9 passes, and the deformation amount of the 7th pass is 48%;

[0074] S5, subjecting the hot rolled billet obtained in step S4 to milling treatment, rough rolling treatment and annealing treatment in sequence, and then performing a post-treatment to obtain a rough rolled billet, wherein the rough rolling treatment is performed for a total of 8 passes, and the roll roughness of the first pass is 0.6 μm, the pass reduction is 20%, the roll roughness of the eighth pass is 0.3 μm, and the pass reduction is 40%, the annealing treatment is performed in a bell furnace, and the annealing treatment parameters are as follows: temperature is 400° C., time is 6 hours; the post-treatment includes sequentially performing surface degreasing, pickling and grinding treatment, and the abrasive mesh number of the grinding treatment is 2400 mesh;

[0075] S6, subjecting the rough rolled billet obtained in step S5 to finishing rolling, secondary post-treatment and annealing treatment in sequence, and then to three post-treatments to obtain a finished rolled strip; wherein the finishing rolling is performed for a total of 5 passes, and the viscosity of the rolling oil during the finishing rolling process is 7mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 16%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 32%; the secondary post-treatment includes surface degreasing, cleaning and drying in sequence; the annealing treatment is carried out in an air cushion furnace, and the annealing treatment parameters are as follows: the temperature is 520℃, and the passing speed is 57m / min; the tertiary post-treatment includes pickling, cleaning and passivation in sequence.

[0076] S7. Shear the finished rolled strip obtained in step S6 to obtain a copper strip for tab material, with a shearing tension of 20 Kgf, a tension accuracy of 3%, and a pressing force of 0.15 Kgf.

[0077] Example 2

[0078] The present embodiment provides a copper strip for a tab material, which is composed of the following components by mass percentage: 99.993% Cu, 0.0009% O, 0.0005% Fe, and the remainder is unavoidable impurities. The copper strip for a tab material in the present embodiment is prepared by the following method:

[0079] S1. Raw materials for preparing copper strips for tab materials;

[0080] S2, the raw material prepared in step S1 is subjected to baking treatment and smelting treatment in sequence to obtain an intermediate melt, wherein the Cu in the raw material is high-purity electrolytic copper with a purity of 99.996%, and the parameters of the baking treatment are as follows: the temperature is 200° C., the time is 13 min, and during the smelting treatment, dry charcoal is added for covering and high-purity argon is blown at the bottom, wherein the covering thickness of the dry charcoal is 180 mm, and the temperature of the smelting treatment is 1200° C.;

[0081] S3, subjecting the intermediate melt obtained in step S2 to insulation treatment, and then subjecting it to vertical full continuous casting to obtain a copper ingot, wherein the insulation treatment is carried out in a heat-insulating furnace, and is covered with spherical granular graphite, the temperature of the insulation treatment is 1190° C., and an electromagnetic stirring device is used in the vertical full continuous casting process, and the parameters of the vertical full continuous casting are as follows: temperature is 1165° C., speed is 88 mm / min, vibration frequency is 38 times / min, cooling water pressure is 0.6 MPa; the frequency of the electromagnetic stirring device is 20 Hz, and the current is 20 A;

[0082] S4, the copper ingot obtained in step S3 is subjected to heating treatment and hot rolling treatment in sequence to obtain a hot-rolled billet, wherein the heating treatment is carried out in a walking furnace, the air-fuel ratio of the walking furnace is 8.3, and the oxide scale is sucked out before being taken out of the furnace, and the parameters of the hot rolling treatment are as follows: a total of 9 passes, and the deformation amount of the 7th pass is 44%;

[0083] S5, subjecting the hot rolled billet obtained in step S4 to milling treatment, rough rolling treatment and annealing treatment in sequence, and then performing a post-treatment to obtain a rough rolled billet, wherein the rough rolling treatment is performed for a total of 8 passes, and the roller roughness of the first pass is 0.6 μm, the pass reduction is 16%, the roller roughness of the eighth pass is 0.3 μm, and the pass reduction is 38%, the annealing treatment is performed in a bell furnace, and the annealing treatment parameters are as follows: temperature is 450° C., time is 4 h; the post-treatment includes sequentially performing surface degreasing, pickling and grinding treatment, and the abrasive mesh number of the grinding treatment is 2000 mesh;

[0084] S6, subjecting the rough rolled billet obtained in step S5 to finishing rolling, secondary post-treatment and annealing treatment in sequence, and then to three post-treatments to obtain a finished rolled strip; wherein the finishing rolling is performed for a total of 5 passes, and the viscosity of the rolling oil during the finishing rolling process is 6mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 18%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 30%; the secondary post-treatment includes surface degreasing, cleaning and drying in sequence; the annealing treatment is carried out in an air cushion furnace, and the annealing treatment parameters are as follows: the temperature is 500℃, and the passing speed is 60m / min; the tertiary post-treatment includes pickling, cleaning and passivation in sequence.

[0085] S7. Shear the finished rolled strip obtained in step S6 to obtain a copper strip for tab material, with a shearing tension of 28 Kgf, a tension accuracy of 4%, and a pressing force of 0.24 Kgf.

[0086] Example 3

[0087] The present embodiment provides a copper strip for a tab material, which is composed of the following components by mass percentage: Cu content 99.99%, O content 0.0008%, Fe content 0.002%, and the remainder is unavoidable impurities. The copper strip for a tab material in the present embodiment is prepared by the following method:

[0088] S1. Raw materials for preparing copper strips for tab materials;

[0089] S2, the raw materials prepared in step S1 are sequentially subjected to baking treatment and smelting treatment to obtain an intermediate melt, wherein the Cu in the raw materials is high-purity electrolytic copper with a purity of 99.993%, and the parameters of the baking treatment are as follows: the temperature is 210° C., the time is 12 min, and during the smelting treatment, dry charcoal is added for covering and high-purity argon is blown at the bottom, wherein the covering thickness of the dry charcoal is 170 mm, and the temperature of the smelting treatment is 1220° C.;

[0090] S3, subjecting the intermediate melt obtained in step S2 to insulation treatment, and then subjecting it to vertical full continuous casting to obtain a copper ingot, wherein the insulation treatment is carried out in a heat preservation furnace, and is covered with spherical granular graphite, the temperature of the insulation treatment is 1195° C., and an electromagnetic stirring device is used in the vertical full continuous casting process, and the parameters of the vertical full continuous casting are as follows: temperature is 1170° C., speed is 82 mm / min, vibration frequency is 42 times / min, cooling water pressure is 0.57 MPa; the frequency of the electromagnetic stirring device is 20 Hz, and the current is 21 A;

[0091] S4, the copper ingot obtained in step S3 is subjected to heating treatment and hot rolling treatment in sequence to obtain a hot-rolled billet, wherein the heating treatment is carried out in a walking furnace, the air-fuel ratio of the walking furnace is 8.6, and the oxide scale is sucked out before being taken out of the furnace, and the parameters of the hot rolling treatment are as follows: a total of 9 passes, and the deformation amount of the 7th pass is 46%;

[0092] S5, subjecting the hot rolled billet obtained in step S4 to milling treatment, rough rolling treatment and annealing treatment in sequence, and then performing a post-treatment to obtain a rough rolled billet, wherein the rough rolling treatment is performed for a total of 8 passes, and the roll roughness of the first pass is 0.6 μm, the pass reduction is 18%, the roll roughness of the eighth pass is 0.3 μm, and the pass reduction is 35%, the annealing treatment is performed in a bell furnace, and the annealing treatment parameters are as follows: temperature is 420° C., time is 5 h; the post-treatment includes sequentially performing surface degreasing, pickling and grinding treatment, and the abrasive mesh number of the grinding treatment is 2600 mesh;

[0093] S6, subjecting the rough rolled billet obtained in step S5 to finishing rolling, secondary post-treatment and annealing treatment in sequence, and then to three post-treatments to obtain a finished rolled strip; wherein the finishing rolling is performed for a total of 5 passes, and the viscosity of the rolling oil during the finishing rolling process is 8mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 15%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 34%; the secondary post-treatment includes surface degreasing, cleaning and drying in sequence; the annealing treatment is carried out in an air cushion furnace, and the annealing treatment parameters are as follows: the temperature is 530℃, and the passing speed is 53m / min; the tertiary post-treatment includes pickling, cleaning and passivation in sequence.

[0094] S7. Shear the finished rolled strip obtained in step S6 to obtain a copper strip for tab material, with a shearing tension of 40 Kgf, a tension accuracy of 3%, and a pressing force of 0.1 Kgf.

[0095] Example 4

[0096] The present embodiment provides a copper strip for a tab material, which is composed of the following components by mass percentage: 99.98% Cu, 0.0004% O, 0.001% Fe, and the remainder is unavoidable impurities. The copper strip for a tab material in the present embodiment is prepared by the following method:

[0097] S1. Raw materials for preparing copper strips for tab materials;

[0098] S2, the raw materials prepared in step S1 are sequentially subjected to baking treatment and smelting treatment to obtain an intermediate melt, wherein the Cu in the raw materials is high-purity electrolytic copper with a purity of 99.995%, and the parameters of the baking treatment are as follows: the temperature is 220° C., the time is 10 min, and during the smelting treatment, dry charcoal is added for covering and high-purity argon is blown at the bottom, wherein the covering thickness of the dry charcoal is 150 mm, and the temperature of the smelting treatment is 1180° C.;

[0099] S3, subjecting the intermediate melt obtained in step S2 to insulation treatment, and then subjecting it to vertical full continuous casting to obtain a copper ingot, wherein the insulation treatment is carried out in a heat-insulating furnace, and is covered with spherical granular graphite, the temperature of the insulation treatment is 1180° C., and an electromagnetic stirring device is used in the vertical full continuous casting process, and the parameters of the vertical full continuous casting are as follows: temperature is 1160° C., speed is 95 mm / min, vibration frequency is 35 times / min, cooling water pressure is 0.58 MPa; the frequency of the electromagnetic stirring device is 20 Hz, and the current is 22 A;

[0100] S4, the copper ingot obtained in step S3 is subjected to heating treatment and hot rolling treatment in sequence to obtain a hot-rolled billet, wherein the heating treatment is carried out in a walking furnace, the air-fuel ratio of the walking furnace is 8, and the oxide scale is sucked out before being taken out of the furnace, and the parameters of the hot rolling treatment are as follows: a total of 9 passes, and the deformation amount of the 7th pass is 42%;

[0101] S5, subjecting the hot rolled blank obtained in step S4 to milling treatment, rough rolling treatment and annealing treatment in sequence, and then performing a post-treatment to obtain a rough rolled blank, wherein the rough rolling treatment is performed for a total of 8 passes, and the roll roughness of the first pass is 0.6 μm, the pass reduction is 15%, the roll roughness of the eighth pass is 0.3 μm, and the pass reduction is 36%, the annealing treatment is performed in a bell furnace, and the annealing treatment parameters are as follows: temperature is 440° C., time is 4.5 h; the post-treatment includes sequentially performing surface degreasing, pickling and grinding treatment, and the abrasive mesh number of the grinding treatment is 3000 mesh;

[0102] S6, subjecting the rough rolled billet obtained in step S5 to finishing rolling, secondary post-treatment and annealing treatment in sequence, and then to three post-treatments to obtain a finished rolled strip; wherein the finishing rolling is performed for a total of 5 passes, and the viscosity of the rolling oil during the finishing rolling process is 6mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 20%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 35%; the secondary post-treatment includes surface degreasing, cleaning and drying in sequence; the annealing treatment is carried out in an air cushion furnace, and the annealing treatment parameters are as follows: the temperature is 550℃, and the passing speed is 50m / min; the tertiary post-treatment includes pickling, cleaning and passivation in sequence.

[0103] S7. Shear the finished rolled strip obtained in step S6 to obtain a copper strip for tab material, with a shearing tension of 35 Kgf, a tension accuracy of 5%, and a pressing force of 0.3 Kgf.

[0104] Comparative Example 1

[0105] This comparative example provides a copper strip for a tab material, which is different from Example 1 only in that, in this comparative example, the copper strip for the tab material is composed of the following components, calculated by mass percentage: Cu content 99.9%, O content 0.0005%, Fe content 0.0001%, and the remainder being unavoidable impurities; the preparation method is the same as that in Example 1, which will not be repeated here.

[0106] Comparative Example 2

[0107] This comparative example provides a copper strip for a tab material, which is different from Example 1 only in that, in this comparative example, the copper strip for the tab material is composed of the following components, calculated by mass percentage: Cu content 99.992%, O content 0.002%, Fe content 0.0001%, and the remainder being unavoidable impurities; the preparation method is the same as that in Example 1, which will not be repeated here.

[0108] Comparative Example 3

[0109] This comparative example provides a copper strip for a tab material, which is different from Example 1 only in that, in this comparative example, the copper strip for the tab material is composed of the following components, calculated by mass percentage: Cu content 99.992%, O content 0.0005%, Fe content 0.005%, and the remainder being unavoidable impurities; the preparation method is the same as that in Example 1, which will not be repeated here.

[0110] Comparative Example 4

[0111] This comparative example provides a copper strip for tab material, which is different from Example 1 only in that, in the preparation process of this comparative example, step S3 is: subjecting the intermediate melt obtained in step S2 to insulation treatment, the insulation treatment is carried out in an insulation furnace, and spherical granular graphite is used for covering, the insulation treatment temperature is 1200°C, and then cooled under a cooling water pressure of 0.5MPa to obtain a copper ingot blank; the other steps are the same as Example 1 and will not be repeated here.

[0112] Comparative Example 5

[0113] This comparative example provides a copper strip for a tab material, which is different from Example 1 only in that, during the preparation process of this comparative example, the deformation amount of the 7th pass in step S4 is 40%, and the rest is the same as Example 1, which will not be repeated here.

[0114] Comparative Example 6

[0115] This comparative example provides a copper strip for a tab material, which is different from Example 1 only in that, during the preparation process of this comparative example, the deformation amount of the 7th pass in step S4 is 50%, and the rest is the same as Example 1, which will not be repeated here.

[0116] Comparative Example 7

[0117] This comparative example provides a copper strip for tab material, which is different from Example 1 only in that, during the preparation process of this comparative example, in step S5, the rough rolling treatment is performed for a total of 8 passes, and the roller roughness of the first pass is 0.6 μm, and the pass reduction is 12%, and the roller roughness of the eighth pass is 0.3 μm, and the pass reduction is 40%.

[0118] Comparative Example 8

[0119] This comparative example provides a copper strip for a tab material, which differs from Example 1 only in that, in the preparation process of this comparative example, in step S5, the rough rolling treatment is performed for a total of 8 passes, and the roller roughness of the first pass is 0.6 μm, and the pass reduction is 22%, and the roller roughness of the eighth pass is 0.3 μm, and the pass reduction is 40%.

[0120] Comparative Example 9

[0121] This comparative example provides a copper strip for tab material, which is different from Example 1 only in that, in the preparation process of this comparative example, in step S5, the rough rolling treatment is performed for a total of 8 passes, and the roller roughness of the first pass is 0.6 μm, the pass reduction is 20%, and the roller roughness of the eighth pass is 0.3 μm, and the pass reduction is 30%.

[0122] Comparative Example 10

[0123] This comparative example provides a copper strip for tab material, which is different from Example 1 only in that, during the preparation process of this comparative example, in step S5, the rough rolling treatment is performed for a total of 8 passes, and the roller roughness of the first pass is 0.6 μm, the pass reduction is 20%, and the roller roughness of the eighth pass is 0.3 μm, and the pass reduction is 45%.

[0124] Comparative Example 11

[0125] This comparative example provides a copper strip for tab material, which is different from Example 1 only in that, in the preparation process of this comparative example, in step S6, the finishing rolling process is performed for a total of 5 passes, and the rolling oil viscosity during the finishing rolling process is 7 mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 13%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 32%.

[0126] Comparative Example 12

[0127] This comparative example provides a copper strip for tab material, which is different from Example 1 only in that, in the preparation process of this comparative example, in step S6, the finishing rolling process is performed for a total of 5 passes, and the rolling oil viscosity during the finishing rolling process is 7 mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 22%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 32%.

[0128] Comparative Example 13

[0129] This comparative example provides a copper strip for tab material, which is different from Example 1 only in that, in the preparation process of this comparative example, in step S6, the finishing rolling process is performed for a total of 5 passes, and the rolling oil viscosity during the finishing rolling process is 7 mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 16%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 28%.

[0130] Comparative Example 14

[0131] This comparative example provides a copper strip for tab material, which is different from Example 1 only in that, in the preparation process of this comparative example, in step S6, the finishing rolling process is performed for a total of 5 passes, and the rolling oil viscosity during the finishing rolling process is 7 mm 2 / s, the roll roughness of the first pass is 0.2μm, the pass reduction is 16%, the roll roughness of the fifth pass is 0.15μm, and the pass reduction is 38%.

[0132] The finished copper strips obtained in Examples 1-4 and Comparative Examples 1-13 were tested for performance. The test results are shown in Table 1. Figure 1 , Figure 2 and Figure 3 As shown, Figure 1 This is a cross-sectional macroscopic structure diagram of the ingot of Example 1 of the present invention; Figure 2 This is a microstructure diagram of the finished strip of Example 1 of the present invention; Figure 3 This is the cross-sectional macroscopic structure diagram of the ingot of comparative example 1 of the present invention.

[0133] Table 1: Performance test results of finished copper strips obtained in Examples 1-4 and Comparative Examples 1-13

[0134]

[0135]

[0136] It can be seen from the performance test results of Comparative Examples 1, 2, 3 and Example 1 that the present invention can control the content of copper, oxygen and iron elements and reduce the content of impurity elements in the copper strip, so that the copper strip can have better mechanical properties and conductivity, thereby meeting market demand. And the comparison between Comparative Examples 1-3 and Example 1 can further prove that even if the deviation of these elements is very small, it may lead to significant changes in alloy properties, including mechanical properties, conductivity, corrosion resistance and processing properties, etc. Therefore, using the element range disclosed in the present invention is conducive to obtaining copper strips with qualified performance. It can be seen from the performance test results of Comparative Example 4 and Example 1 that the present invention further improves the mechanical properties of the material, such as strength and toughness, by refining the grains by assisting electromagnetic stirring in the vertical full-continuous casting process; and it can be seen from the performance test results of Comparative Examples 5 to Comparative Examples 14 that in the present invention, controlling the deformation amount in the rolling step plays an important role. Specifically, the present invention promotes the refinement of the metal crystal structure by controlling the deformation amount of the key passes in the hot rolling process, and obtains a more uniform and fine grain structure, thereby improving the mechanical properties of the material; and the use of the deformation amount within the scope of the present invention for the key passes in the rough rolling process can improve production efficiency and reduce the number of subsequent finishing passes, but excessive deformation causes cracks or excessive hardening of the material, so too low or too high deformation has an impact on the final performance of the material; the deformation amount of the key passes in the finishing rolling process plays an important role in adjusting the residual stress distribution inside the material, avoiding warping and deformation, and ensuring the flatness and stability of the material. It can be seen from the results that the mechanical and physical properties of the material obtained by the present invention using the above-mentioned deformation amount of the finishing pass are within the required range.

[0137] In summary, the present invention optimizes and controls the material composition and reasonably coordinates the key processes to form a preparation control technology for a copper strip with high surface quality without color difference, brush marks and damage, and prepares a copper strip for tab material with excellent comprehensive performance and surface quality. The method has the characteristics of strong market competitiveness, significant economic benefits and high product yield.

[0138] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the protection scope of the claims.

Claims

1. A copper strip for tab material, characterized in that: According to the mass percentage, the copper strip for the tab material includes the following components in mass percentage: Cu content> 99.95%, O content< 0.001%, Fe content <0.004%, and the balance are inevitable impurities.

2. The copper strip for tab material according to claim 1, characterized in that: The surface roughness of the copper strip for the tab material is 0.12-0.15 μm, the number of 360° bending times of the copper strip for the tab material is ≥8, the electrical conductivity of the copper strip for the tab material is 100.1-102.4% IACS, the surface of the copper strip for the tab material is zero-defect after the entire roll is nickel-plated, the tensile strength of the copper strip for the tab material is 220-250 MPa, and the elongation is 30-40%.

3. A method for preparing a copper strip for tab material according to claim 1 or 2, characterized in that: The preparation method specifically comprises the following steps: S1. Raw materials for preparing copper strips for tab materials; S2, sequentially performing baking treatment and smelting treatment on the raw materials prepared in step S1 to obtain an intermediate melt; S3, subjecting the intermediate melt obtained in step S2 to heat preservation treatment, and then subjecting the intermediate melt to vertical full-continuous casting to obtain a copper ingot; S4, sequentially subjecting the copper ingot obtained in step S3 to heating treatment and hot rolling treatment to obtain a hot-rolled billet; S5, subjecting the hot-rolled billet obtained in step S4 to milling treatment, rough rolling treatment and annealing treatment in sequence, and then performing a post-treatment to obtain a rough-rolled billet; S6, subjecting the rough rolled billet obtained in step S5 to finish rolling, secondary post-processing and annealing in sequence, and then performing three post-processing to obtain a finished rolled strip; S7, shearing the finished rolled strip obtained in step S6 to obtain a copper strip for tab material.

4. The method for preparing the copper strip for tab material according to claim 3, characterized in that: In step S2, the Cu in the raw material is high-purity electrolytic copper with a purity of more than 99.99%, and the parameters of the baking treatment are as follows: temperature of 180-220° C., time of 10-15 min; and / or, During the smelting process, dry charcoal is added as a cover and high-purity argon is blown at the bottom, wherein the cover thickness of the dry charcoal is 150-200 mm, and the smelting temperature is 1180-1250° C.

5. The method for preparing the copper strip for tab material according to claim 3, characterized in that: In step S3, the heat preservation treatment is carried out in a heat preservation furnace and covered with spherical graphite particles. The temperature of the heat preservation treatment is 1180-1200°C.

6. The method for preparing the copper strip for tab material according to claim 3, characterized in that: In the step S3, an electromagnetic stirring device is used in the vertical full continuous casting process, and the parameters of the vertical full continuous casting are as follows: temperature is 1160-1180°C, speed is 75-95mm / min, vibration frequency is 35-45 times / min, cooling water pressure is 0.5-0.6MPa; the frequency of the electromagnetic stirring device is 20Hz, and the current is 20-24A.

7. The method for preparing the copper strip for tab material according to claim 3, characterized in that: In step S4, the heating treatment is carried out in a walking beam furnace, the air-fuel ratio of the walking beam furnace is 8-9, and the oxide skin is sucked out before leaving the furnace; and / or, The parameters of the hot rolling process are as follows: 9 passes in total, and the deformation amount of the 7th pass is 42-48%.

8. The method for preparing a copper strip for tab material according to claim 3, characterized in that: In step S5, the rough rolling process is performed for 8 passes, and the roll roughness of the first pass is 0.6 μm, the pass reduction is 15-20%, and the roll roughness of the eighth pass is 0.3 μm, and the pass reduction is 35-40%; and / or, The annealing treatment is carried out in a bell furnace, and the parameters of the annealing treatment are as follows: temperature of 400-450° C., time of 4-6 h; and / or, The primary post-treatment includes sequentially performing surface degreasing, pickling and grinding treatment, and the abrasive mesh number of the grinding treatment is 2000-3000 meshes.

9. The method for preparing a copper strip for tab material according to claim 3, characterized in that: In step S6, the finishing rolling process is performed for 5 times, and the viscosity of the rolling oil during the finishing rolling process is 6-8 mm 2 / s, the first pass has a roll roughness of 0.2 μm and a pass reduction of 15-20%, the fifth pass has a roll roughness of 0.15 μm and a pass reduction of 30-35%; and / or, Secondary post-treatment includes sequential surface degreasing, cleaning and drying; and / or, The annealing treatment is carried out in an air cushion furnace, and the parameters of the annealing treatment are as follows: temperature of 500-550° C., passing speed of 50-60 m / min; and / or, The tertiary post-treatment includes pickling, cleaning and passivation in sequence.

10. The method for preparing a copper strip for tab material according to claim 3, characterized in that: In step S7, the shearing tension is 20-40 Kgf, the tension accuracy is 3-5%, and the pressing force is 0.1-0.3 Kgf.

Citation Information

Cited By

  • Advanced copper plate strip continuous rolling process

    CN119456669A

  • Oxygen-free copper strip for ceramic copper-clad plate with grain texture cooperative control and preparation method of oxygen-free copper strip

    CN120866685A

  • Preparation method of high-precision automobile connector red copper belt

    CN121222858A