Preparation method and application of nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy

By prefabricating nitrogen-containing raw materials and plasma nitriding treatment, combined with rapid quenching technology, the problem of uneven distribution of nitrogen elements in iron-based amorphous alloys is solved, the magnetic performance and doping efficiency are improved, and new non-metallic element doping is provided Miscellaneous ways.

CN118957455AActive Publication Date: 2024-11-15GUANGDONG UNIV OF TECH

Patent Information

Application Number
CN202411080388.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing nitriding methods are difficult to effectively control the distribution of nitrogen elements in iron-based amorphous alloys, resulting in the inability to stably dopate nitrogen elements, affecting the magnetic properties of the alloy.

Method used

The prefabricated nitrogen-containing raw materials are prepared by plasma nitriding, and the nitrogen-containing iron sheet is melted with the amorphous element ingredients. The nitrogen-containing iron-based soft magnetic amorphous/nano-crystal alloy is prepared in combination with rapid quenching technology to ensure uniform distribution of nitrogen elements. .

Benefits of technology

The stable doping of nitrogen elements is achieved, the magnetic properties of amorphous alloys are improved, the coercive force is reduced, and new doping ideas are provided, widening the doping method of non-metallic elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957455A_ABST
    Figure CN118957455A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of alloy smelting and amorphous alloys, and particularly relates to a preparation method and application of a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy. According to the preparation method, a new preparation thought is adopted for carrying out chemical nitriding treatment on high-purity iron metal to obtain a secondary raw material with stable nitrogen content, then the secondary raw material is matched with amorphous forming elements and then smelted into a nitrogen-containing alloy ingot, and then a rapid quenching technology is adopted for preparing the completely amorphous state Fe Si B < c > CdNe iron-based soft magnetic amorphous alloy. And finally, carrying out heat treatment on the completely amorphous nitrogen-containing iron-based soft magnetic amorphous alloy to crystallize the completely amorphous nitrogen-containing iron-based soft magnetic amorphous alloy into an amorphous / nanocrystalline alloy. According to the method, the subsequent nitriding step is omitted in the preparation process of the amorphous alloy, the problems that in the past, nitrogen doping of the iron-based amorphous alloy is difficult, and nitrogen only exists on the surface of a strip are solved to a certain extent, the method has the advantages of being simple, efficient, low in cost and the like, and new reference and guidance are provided for the nitrogen doping approach of the amorphous alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy smelting and amorphous alloys, and in particular relates to a preparation method and application of a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy. Background Art

[0002] Amorphous alloy, also known as metallic glass, refers to a solid alloy with disordered atomic arrangement formed under rapid cooling conditions when the atoms inside the alloy do not have time to form an ordered arrangement structure by diffusion. Compared with crystalline alloys, the atomic spatial arrangement of amorphous alloys has the characteristics of long-range disorder and short-range order. Due to this unique disordered structure, amorphous alloys do not have common defects in traditional alloy structures such as dislocations and grain boundaries. Macroscopically, the structure of amorphous alloys is uniform and exhibits isotropic properties. From a thermodynamic point of view, amorphous alloys are metastable and have higher free energy than crystalline alloys. This also gives amorphous alloys unique physical properties, such as exciting phenomena in magnetic properties.

[0003] In recent years, it is a common method to regulate the magnetic properties of iron-based amorphous alloys by doping with trace elements. Among them, the doping of metal elements is easier to operate than that of non-metal elements. Soft magnetic properties mainly refer to the optimization of saturation magnetic induction intensity (Bs) and coercive force (Hc). For the Bs of iron-based amorphous alloys, Bs is positively correlated with the mass proportion of iron within a certain range. Therefore, metal element doping generally reduces the Bs of iron-based amorphous, resulting in a decrease in soft magnetic properties. Although the Co element can effectively improve the Bs of iron-based amorphous alloys, the high price of Co element limits the large-scale commercial application of such alloys. Non-metallic elements are another key factor for iron-based amorphous alloys to maintain high saturation magnetic induction intensity. The addition of non-metallic elements can keep the mass ratio of iron elements at a high level, so that the alloy has a higher Bs value. Existing research on non-metallic element doping mainly focuses on the addition and replacement of four elements: Si, B, P, and C. In addition to Si and B as necessary elements for iron-based amorphous alloys, the effects of P and C elements on the soft magnetic properties of iron-based amorphous alloys have also been widely studied. However, the effect of N doping on the soft magnetic properties of iron-based amorphous alloys has been less studied. One of the main reasons is that the alloy ingot cannot be effectively doped with N. For example, Chinese invention patent CN 109440058 A discloses a nitrogen-containing iron-based amorphous nanocrystalline soft magnetic alloy and a preparation method thereof, wherein the iron-based amorphous alloy is subjected to low-temperature and low-pressure or low-temperature and normal-pressure nitriding by plasma nitriding, and the nitriding temperature is required to be 100-400°C and the nitriding time is 10-60min. However, plasma nitriding belongs to a surface treatment process. By using this method, the surface of the iron-based amorphous alloy is directly nitrided, and the distribution of nitrogen is mainly concentrated on the surface of the alloy, and the distribution is uneven. Patent CN 109440023 B also discloses a high magnetic induction coupling iron-based amorphous nanocrystalline alloy and a preparation method thereof, wherein the method uses nitride as a smelting raw material for alloying to prepare a nitrogen-containing iron-based amorphous nanocrystalline alloy. However, nitrides have a high melting point and low density. After other raw materials melt during the arc melting process, nitrides tend to float on the surface of the melt due to their low density, resulting in the inability to effectively control the nitrogen element that is actually integrated into the alloy ingot.

[0004] For amorphous alloys, negative mixing enthalpy is beneficial to improve the ability to form amorphous. Since the mixing enthalpy of N element and other metal elements is negative and low, only a small amount of N element needs to be added to change the amorphous forming ability of iron-based amorphous alloys. However, the existing nitriding methods have their own defects and cannot effectively control the stable doping of N element. The nitrogen used for nitriding treatment of finished amorphous strips only exists on the surface of the strip, and nitride smelting is not an ideal nitriding method due to the low density and high melting point of nitrides. Therefore, more in-depth research is needed in the field of smelting to prepare nitrogen-containing amorphous alloys.

[0005] In summary, it is necessary to develop new nitrogen doping methods to change the various nitriding defects caused by traditional nitriding methods, such as improving the problem that the nitrogen content cannot be controlled. Summary of the invention

[0006] In order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a method for preparing nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloys, and adopts prefabricated nitrogen-containing raw materials to prepare nitrogen-containing iron-based soft magnetic amorphous alloys, which overcomes the problems of difficulty in nitrogen doping of iron-based amorphous alloys and nitrogen only existing on the surface of the strip. It provides a new doping idea for nitrogen doping of iron-based amorphous alloys and greatly broadens the way of doping non-metallic elements in iron-based amorphous alloys.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] The present invention provides a method for preparing a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy. The general formula of the nitrogen-containing iron-based soft magnetic amorphous alloy is: Fe a Si b B c C d N e , the atomic ratio of each component in the general formula is: a = 75%-85%, b = 0%-10%, c = 5%-15%, d = 0-2%, e = 0.05-0.5%; where a + b + c + d + e = 100%;

[0009] The method for preparing the nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy comprises the following steps:

[0010] S1. Plasma nitriding treatment is performed on high-purity iron metal to obtain nitrogen-containing iron sheet as secondary raw material, and then the nitrogen-containing iron sheet is smelted into alloy ingots with amorphous forming elements according to the alloy chemical formula, wherein the amorphous forming elements are selected from at least one of B, Si and C;

[0011] S2, crushing the alloy ingot in step S1 and spinning it with a strip spinning device, and adopting a rapid cooling technology to prepare an amorphous alloy strip;

[0012] S3. Heat-treating the amorphous alloy strip in step S2 under vacuum or protective atmosphere to obtain a nitrogen-containing iron-based amorphous nanocrystalline soft magnetic alloy.

[0013] The plasma nitriding method adopted by the present invention is a process in which nitrogen ions obtain electrons on the surface of the metal material, are reduced to nitrogen atoms and penetrate into the surface of the steel part and gradually diffuse inward to form a nitriding layer, i.e., nitriding treatment. At the same time, during this process of ion bombardment, the surface will also be sputtered and cleaned, and the oxide layer and oxidation products covering the surface of the material can be automatically removed, and the nitrogen element will exist in the material in the form of atoms. After this treatment, the nitrogen element exists in the raw material in the form of nitrogen atoms. This method of preparing nitrogen-containing iron-based soft magnetic amorphous alloys with prefabricated nitrogen-containing raw materials can overcome the problems of difficulty in nitrogen doping of iron-based amorphous alloys in the past and nitrogen only existing on the surface of the strip, provides a new doping idea for nitrogen doping of iron-based amorphous / nanocrystalline alloys, and greatly broadens the way of doping non-metallic elements in iron-based amorphous / nanocrystalline alloys.

[0014] Preferably, the high-purity iron metal is in the form of high-purity iron flakes or high-purity iron powder, with a purity of 99.9% or more.

[0015] Preferably, the smelting is vacuum arc melting or induction melting, and an inert gas or nitrogen is filled as a protective gas during the smelting process.

[0016] Preferably, the belt-spinning equipment is a single-roller rapid cooling belt-spinning machine, and the linear speed of the belt-spinning copper roller is 45-60 m / s.

[0017] Preferably, the heat treatment is stress relief annealing, and the annealing temperature is selected according to the DSC thermal analysis results. Stress relief annealing is generally selected between 100°C below the first crystallization temperature (i.e., the temperature at which α-Fe begins to precipitate) and the first crystallization temperature, and the time is 10min-1h. The stress relief annealing is performed before the temperature at which α-Fe nanoparticles are not precipitated, and the alloy after annealing is still an amorphous structure.

[0018] More preferably, the annealing temperature is 300-510° C., and the annealing time is 10 min-1 h.

[0019] Preferably, B is derived from boron or ferroboron.

[0020] The present invention also provides a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy prepared by the above-mentioned preparation method.

[0021] The nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy prepared by the method of the present invention not only maintains a relatively high Bs, but also the doping of an appropriate amount of nitrogen element can further reduce the coercive force of the amorphous alloy, and has excellent industrial application prospects.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention discloses a method for preparing a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy. A new preparation method is adopted to obtain a secondary raw material with a stable nitrogen content by chemical nitriding of high-purity iron metal, and then the secondary raw material is mixed with an amorphous forming element (at least one of B, Si, and C) and smelted into a nitrogen-containing alloy ingot. Then, a rapid cooling technology is adopted to prepare a completely amorphous Fe a Si b B c C d N e Iron-based soft magnetic amorphous alloy; in the amorphous alloy, the atomic ratio of each component is: a=75%-85%, b=0%-10%, c=5%-15%, d=0-2%, e=0.05-0.5%; wherein a+b+c+d+e=100%. Finally, the completely amorphous iron-based soft magnetic amorphous alloy containing nitrogen elements is heat-treated to crystallize it into an amorphous / nanocrystalline alloy. The present invention adopts prefabricated nitrogen-containing raw materials to prepare nitrogen-containing iron-based soft magnetic amorphous alloys. The appropriate amount of N content can not only improve the amorphous forming ability of the iron-based amorphous nanocrystalline alloy, but also has a certain effect on the coercivity of the amorphous alloy, and can effectively reduce the coercivity of the amorphous alloy. At the same time, the subsequent nitriding step is omitted in the preparation process of the amorphous alloy, which overcomes the problem of the difficulty of nitrogen doping in the previous iron-based amorphous alloy and the existence of nitrogen only on the surface of the strip to a certain extent. It has the advantages of simplicity, high efficiency, low cost, etc., and provides new reference and guidance for the nitrogen doping of amorphous alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the XRD pattern of the surface of the thin iron sheet after nitriding chemical surface treatment;

[0025] Figure 2 is the X-ray diffraction pattern of quenched Fe-based amorphous ribbon;

[0026] Figure 3 X-ray diffraction patterns of Example 1(a), Example 2(b) and Comparative Example 1(c) after annealing;

[0027] Figure 4 is the hysteresis curve of the quenched Fe-based amorphous alloy;

[0028] Figure 5 This is the curve showing the change of coercivity of Fe-based amorphous nanocrystalline alloy with heat treatment temperature. DETAILED DESCRIPTION

[0029] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0030] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0031] The present invention provides a nitrogen-containing iron-based amorphous / nanocrystalline soft magnetic alloy, the general formula of which is: Fe a Si b B c C d N e , the atomic ratio of each component in the general formula: a = 75%-85%, b = 0%-10%, c = 5%-15%, d = 0-2%, e = 0.05-0.5%; where a + b + c + d + e = 100%;

[0032] The method for preparing the nitrogen-containing iron-based amorphous alloy comprises the following steps:

[0033] (1) Nitriding high-purity metallic iron (in the form of flakes, powder, etc.) to obtain a nitrogen-containing secondary raw material. Then, the nitrogen-containing secondary raw material and amorphous forming elements (B, Si, C) are smelted to obtain an alloy ingot; the B source includes boron or ferroboron, and the C source comes from graphite.

[0034] (2) The alloy ingot obtained by the above smelting is crushed and then spun using a single-roller strip spinning machine to prepare an amorphous alloy strip.

[0035] (3) Heat treating the amorphous strip obtained above in vacuum or protective atmosphere to obtain nitrogen-containing iron-based amorphous nanocrystalline soft magnetic alloy.

[0036] All raw materials of the present invention have no special requirements and restrictions on their sources, and can be purchased from the market or prepared according to conventional methods well known to those skilled in the art of smelting.

[0037] All the pure metal raw materials of the present invention can adopt the conventional purity in the field, and the purity can be above 99.9%.

[0038] The preparation of the nitrogen-containing secondary raw material required by the present invention has no special requirements on the nitriding technology, and the specific nitrogen content is prepared according to the actual nitriding time and other requirements.

[0039] The present invention has no particular limitation on the smelting conditions, and smelting conditions familiar to those skilled in the art may be used. Those skilled in the art may adjust the smelting conditions according to actual production conditions, product requirements and quality requirements.

[0040] The present invention has no particular limitation on the belt-spinning method. The belt-spinning method for preparing amorphous alloys that is well known to those skilled in the art can be used. Those skilled in the art can select and adjust the method according to actual production conditions, product requirements and quality requirements. The belt-spinning method of the present invention is preferably a single-roller rapid cooling belt-spinning method. The belt-spinning device of the present invention is preferably a single-roller rapid cooling belt-spinning machine.

[0041] Finally, the present invention heat treats the amorphous alloy strip obtained in the above steps under vacuum or protective atmosphere to obtain an iron-based amorphous nanocrystalline soft magnetic alloy.

[0042] The present invention has no particular limitation on the concept of the heat treatment. The heat treatment of amorphous alloys familiar to those skilled in the art may be used. Those skilled in the art may select and adjust according to actual production conditions, product requirements and quality requirements. The heat treatment described in the present invention is preferably stress relief annealing.

[0043] The present invention has no particular limitation on the heat treatment temperature. The heat treatment temperature of amorphous alloys familiar to those skilled in the art may be used. Those skilled in the art may select and adjust the temperature according to actual production conditions, product requirements and quality requirements. The heat treatment temperature range of the present invention is preferably 300-510°C.

[0044] In order to further clearly present the nitrogen-containing iron-based amorphous / nanocrystalline alloy and the preparation method thereof of the present invention, a detailed description is given below in the form of embodiments and comparative examples.

[0045] Example 1: Preparation of Fe 82.45 SiC 15 C 0.5 N 0.05 Amorphous alloy strip

[0046] (1) Preparation of nitrogen-containing secondary raw materials (nitrogen-containing iron sheets): Cut high-purity thin iron sheets (>99.9wt%) into 100mm×100mm square sheets, and then perform plasma nitriding treatment on the front and back of the iron sheets to obtain nitrogen-containing iron sheets as secondary raw materials. The plasma nitriding treatment is specifically as follows: first, place the prepared iron sheet into a nitriding furnace, pass cooling water, turn on the vacuum pump to evacuate the furnace, and make the air pressure in the furnace body lower than 5Pa. Then, introduce 99.99% high-purity ammonia into the furnace body, adjust the rectifier output voltage, start the ignition, and raise the temperature to 200°C. At the same time, adjust the flowmeter and vacuum valve so that the flow rate of ammonia is 0.4m 3 / h, the gas pressure is maintained at about 500Pa, and the temperature is kept at 200℃ for 0.5h. Then the other side of the pure iron sheet is subjected to the same nitriding operation. The nitrogen content of the prepared nitrogen-containing iron sheet is measured by an oxygen-nitrogen analyzer and is found to be 0.34wt%. Figure 1The XRD result of the secondary raw material surface of the obtained nitrogen-containing iron sheet shows that it mainly exists in the form of FexN (x=2 or 3).

[0047] (2) According to the alloy chemical formula Fe 82.45 SiC 15 C 0.5 N 0.05 Weigh the ingredients and put the prepared raw materials (nitrogen-containing iron sheet, Si, Fe-B alloy, C) into the vacuum arc melting furnace, and evacuate the furnace to 5×10 -3 Then, fill in argon or nitrogen as protective gas, and when the pressure in the furnace is lower than the atmospheric pressure by 0.01Mpa, close the gas filling valve. At the same time, make the arc melting temperature reach 3000℃ or above, heat and melt the raw materials, and continue to melt for 2 minutes after the raw materials are completely melted, and then cool them to solidification, quickly turn them over and repeat the melting for 3 times to obtain an alloy ingot with uniform composition.

[0048] (3) The alloy ingot obtained by smelting is broken into small pieces of alloy, which are then cleaned and placed in a quartz tube with an open lower end, and then placed in the induction coil of a belt-spinning device (single-roller rapid cooling belt-spinning machine). After evacuation, high-purity argon gas with a purity of 99.99% is filled in as a protective gas, and the current is adjusted to melt the alloy. The molten alloy is then sprayed onto the surface of a copper roller with a rotation speed of 55 m / s and a cooling system using the pressure difference. The cooling rate reaches 10 5 ~10 6 K / s, and an amorphous ribbon with a width of about 1 mm and a thickness of about 21 μm was obtained. The structure of the alloy ribbon was detected by X-ray diffractometer, and the X-ray diffraction analysis results of the obtained amorphous ribbon are as follows Figure 2 As shown. Figure 2 It can be seen that the completely amorphous ribbon has a broadened and diffuse diffraction peak at about 45°, but no obvious sharp crystallization peak in other ranges, indicating that the quenched structure of the sample obtained in Example 2 is amorphous.

[0049] (4) The prepared amorphous alloy strip sample was tested with an oxygen and nitrogen analyzer, and the results showed that the nitrogen content of the strip was 0.0175wt%, and the theoretical nitrogen content was 0.0145wt%.

[0050] (5) The amorphous alloy ribbon is placed in a heat treatment furnace for annealing. Argon gas is filled for protection during the heat treatment process. The temperature is raised to 300°C and kept for 30 minutes. The temperature is then raised to 350°C, 380°C, 410°C, and 430°C, respectively, and kept for 10 minutes. The heating rate is 5°C / min. The ribbon is then cooled to room temperature and taken out to obtain an iron-based amorphous nanocrystalline alloy. The XRD results corresponding to each temperature treatment are shown in Figure 2. Figure 3As shown in (a), an obvious crystallization peak appears after 410 °C, indicating that above 410 °C, nanocrystals gradually precipitate to form an amorphous / nanocrystalline dual-phase structure.

[0051] The saturation magnetic induction intensity (Bs) and coercive force (Hc) performance tests of the annealed thin ribbon were carried out using magnetic detection equipment (vibrating sample magnetometer VSM and soft magnetic DC tester).

[0052] Figure 4 is the hysteresis loop diagram of Fe-based amorphous alloy. Figure 5 The coercivity of Fe-based amorphous nanocrystalline alloy varies with heat treatment temperature. 82.45 SiC 15 C 0.5 N 0.05 The Bs value of the amorphous state is 1.71T, and the Hc value is 7.9A / m. At the same time, as the heat treatment temperature increases, the coercive force reaches the lowest at 380°C, which is 2.1A / m.

[0053] Example 2: Preparation of Fe 82.4 SiC 15 C 0.5 N 0.1 Amorphous alloy strip

[0054] (1) Preparation of nitrogen-containing secondary raw material (nitrogen-containing iron sheet): High-purity thin iron sheet (>99.9wt%) was cut into square sheets of 100mm×100mm, and then the front and back sides of the iron sheet were subjected to plasma nitriding treatment (the specific treatment was the same as in Example 1) to obtain nitrogen-containing iron sheet as secondary raw material. The nitrogen content of the prepared nitrogen-containing iron sheet was measured by an oxygen-nitrogen analyzer, and the nitrogen content was 0.34wt%. Figure 1 From the XRD results of the surface of the secondary raw material of the obtained nitrogen-containing iron sheet, it can be found that it mainly exists in the form of FexN (x=2 or 3).

[0055] (2) According to the alloy chemical formula Fe 82.4 SiC 15 C 0.5 N 0.1 Weigh the ingredients and put the prepared raw materials (nitrogen-containing iron sheet, Si, Fe-B alloy, C) into the vacuum arc melting furnace, and evacuate the furnace to 5×10 -3 Then, fill in argon or nitrogen as protective gas, and when the pressure in the furnace is lower than the atmospheric pressure by 0.01Mpa, close the gas filling valve. At the same time, make the arc melting temperature reach 3000℃ or above, heat and melt the raw materials, and continue to melt for 3 minutes after the raw materials are completely melted, and then cool them to solidification, quickly turn them over and repeat the melting 3 times to obtain an alloy ingot with uniform composition.

[0056] (3) The alloy ingot obtained by smelting is broken into small pieces of alloy, which are then cleaned and placed in a quartz tube with an opening at the bottom, and then placed in the induction coil of a belt-spinning device (single-roller rapid cooling belt-spinning machine). After evacuation, high-purity argon gas with a purity of 99.99% is filled in as a protective gas, and the current is adjusted to melt the alloy. The alloy in a molten state is then sprayed onto the surface of a copper roller with a rotation speed of 55 m / s and a cooling system using a pressure difference. The cooling rate reaches 105-106 K / s, and an amorphous ribbon with a width of about 1 mm and a thickness of about 14 μm is obtained. The alloy strip is structurally tested using an X-ray diffractometer. The X-ray diffraction analysis results of the obtained amorphous ribbon are as follows: Figure 2 As shown by Figure 2 It can be seen that the completely amorphous ribbon has a broadened and diffuse diffraction peak at about 45°, but no obvious sharp crystallization peak in other ranges, indicating that the quenched structure of the sample obtained in Example 3 is amorphous.

[0057] (4) The prepared amorphous alloy strip was tested with an oxygen and nitrogen analyzer. The results showed that the nitrogen content of the strip was 0.0256wt%, and the theoretical nitrogen content was 0.029wt%.

[0058] (5) The amorphous alloy ribbon is placed in a heat treatment furnace for annealing. Argon gas is filled for protection during the heat treatment process. The temperature is raised to 300°C and kept for 30 minutes. The temperature is then raised to 350°C, 380°C, 410°C, and 430°C, respectively, and kept for 10 minutes. The heating rate is 5°C / min. The ribbon is then cooled to room temperature and taken out to obtain an iron-based amorphous nanocrystalline alloy. The XRD results corresponding to each temperature treatment are shown in Figure 2. Figure 3 As shown in (b), an obvious crystallization peak appears after 410°C, indicating that above 410°C, nanocrystals gradually precipitate to form an amorphous / nanocrystalline dual-phase structure.

[0059] The saturation magnetic induction intensity (Bs) and coercive force (Hc) performance tests of the annealed thin ribbon were carried out using magnetic detection equipment (vibrating sample magnetometer VSM and soft magnetic DC tester).

[0060] Figure 4 is the hysteresis loop diagram of Fe-based amorphous alloy. Figure 5 The coercivity of Fe-based amorphous nanocrystalline alloy varies with heat treatment temperature. 82.4 SiC 15 C 0.5 N 0.1 The Bs value of the amorphous state is 1.70T, and the Hc value is 11.7A / m. At the same time, as the heat treatment temperature increases, the coercive force reaches the lowest at 380℃, which is 2.7A / m.

[0061] Comparative Example 1: Preparation of Fe 82.5 SiC15 C 0.5 Amorphous alloy strip

[0062] (1) According to the alloy chemical formula Fe 82.5 SiC 15 C 0.5 Weigh the ingredients and put the prepared raw materials (Fe, Si, Fe-B alloy, C) into the vacuum arc melting furnace. Evacuate the furnace to 5×10 -3 Then fill in argon or nitrogen as protective gas, and when the pressure in the furnace is 0.01Mpa lower than the atmospheric pressure, close the gas filling valve. At the same time, make the arc melting temperature reach 3000℃ or above, heat and melt the raw materials, and continue to melt for 3 minutes after the raw materials are completely melted, and then cool to solidification, quickly turn it over and repeat the melting 3 times to obtain an alloy ingot with uniform composition.

[0063] (2) The alloy ingot obtained by smelting is broken into small pieces of alloy, which are then cleaned and placed in a quartz tube with an opening at the bottom, and then placed in the induction coil of a belt-spinning device (single-roller rapid cooling belt-spinning machine). After evacuation, high-purity argon gas with a purity of 99.99% is filled in as a protective gas, and the current is adjusted to melt the alloy. The alloy in a molten state is then sprayed onto the surface of a copper roller with a rotation speed of 55 m / s and a cooling system using a pressure difference. The cooling rate reaches 105-106 K / s, and an amorphous ribbon with a width of about 1 mm and a thickness of about 13 μm is obtained. The alloy strip is structurally tested using an X-ray diffractometer. The X-ray diffraction analysis results of the obtained amorphous ribbon are as follows: Figure 2 As shown. Figure 2 It can be seen that the completely amorphous ribbon has a broadened and diffuse diffraction peak at about 45°, but no obvious sharp crystallization peak in other ranges, indicating that the quenched structure of the sample obtained in Example 1 is amorphous.

[0064] (3) The prepared amorphous alloy strip sample was tested with an oxygen and nitrogen analyzer, and the results showed that the nitrogen content of the strip was 0.0098wt%, and the theoretical nitrogen content was 0wt%.

[0065] (4) The amorphous alloy ribbon is placed in a heat treatment furnace for annealing. Argon gas is filled for protection during the heat treatment process. The temperature is raised to 300°C and kept for 30 minutes. The temperature is then raised to 350°C, 380°C, 410°C, and 430°C, respectively, and kept for 10 minutes. The heating rate is 5°C / min. The ribbon is then cooled to room temperature and taken out to obtain an iron-based amorphous nanocrystalline alloy. The XRD results corresponding to each temperature treatment are shown in Figure 2. Figure 3 As shown in (c), an obvious crystallization peak appears after 410°C, indicating that above 410°C, nanocrystals gradually precipitate to form an amorphous / nanocrystalline dual-phase structure.

[0066] The saturation magnetic induction intensity (Bs) and coercive force (Hc) performance tests of the annealed thin ribbon were carried out using magnetic detection equipment (vibrating sample magnetometer VSM and soft magnetic DC tester).

[0067] Figure 4 is the hysteresis loop diagram of Fe-based amorphous alloy. Figure 5 The coercivity of Fe-based amorphous nanocrystalline alloy varies with heat treatment temperature. 82.5 SiC 15 C 0.5 The Bs value of the amorphous state is 1.72T, and the Hc value is 13.3A / m. At the same time, with the increase of heat treatment, the coercivity reaches the lowest at 380℃, which is 3.3A / m.

[0068] In summary, the preparation technology of nitrogen-doped iron-based amorphous / nanocrystalline alloy provided by the present invention is feasible, and the quenched Bs value of the products is higher than 1.65T, which not only maintains a relatively high Bs (Chen Guojun, Niu Yongji, Peng Weifeng, et al. Research Progress of High Saturation Flux Density Fe-based Amorphous Soft Magnetic Alloys [J]. Magnetic Materials and Devices, 2011, 42(5): 6. DOI: 10.3969 / j.issn.1001-3830.2011.05.002.), but also the doping of nitrogen can further reduce the coercivity of the amorphous alloy, which has excellent industrial application prospects.

[0069] The above is a detailed introduction to the preparation method and application of a nitrogen-containing iron-based soft magnetic amorphous nanocrystalline soft magnetic alloy provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method and its core idea of ​​the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including the manufacture and use of any device or system, and the implementation of any combined method. It should be pointed out that for those skilled in the art, without departing from the principles and spirit of the present invention, various changes, modifications, substitutions and variations of these implementations still fall within the scope of protection of the present invention.

Claims

1. A method for preparing a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy, characterized in that: The general formula of the nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy is: Fe a Si b B c C d N e , the atomic ratio of each component in the general formula is: a = 75%-85%, b = 0%-10%, c = 5%-15%, d = 0-2%, e = 0.05-0.5%; where a + b + c + d + e = 100%; The method for preparing the nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy comprises the following steps: S1. Plasma nitriding treatment is performed on high-purity iron metal to obtain nitrogen-containing iron sheet as secondary raw material, and then the nitrogen-containing iron sheet is smelted into alloy ingots with amorphous forming elements according to the alloy chemical formula, wherein the amorphous forming elements are selected from at least one of B, Si and C; S2, crushing the alloy ingot in step S1 and spinning it with a strip spinning device, and adopting a rapid cooling technology to prepare an amorphous alloy strip; S3. Heat-treating the amorphous alloy strip in step S2 under vacuum or protective atmosphere to obtain a nitrogen-containing iron-based amorphous nanocrystalline soft magnetic alloy.

2. The method for preparing a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy according to claim 1, characterized in that: The high-purity iron metal is in the form of high-purity iron flakes or high-purity iron powder, and the purity is above 99.9%.

3. The method for preparing a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy according to claim 1, characterized in that: The smelting is vacuum arc melting or induction melting, and inert gas or nitrogen is filled as protective gas during the smelting process.

4. The method for preparing a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy according to claim 1, characterized in that: The belt-spinning equipment is a single-roller rapid cooling belt-spinning machine, and the linear speed of the belt-spinning copper roller is 45-60m / s.

5. The method for preparing a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy according to claim 1, characterized in that: The heat treatment is a stress relief annealing treatment, the annealing temperature is between 100° C. below the first crystallization temperature and the first crystallization temperature, and the time is 10 min-1 h.

6. The method for preparing a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy according to claim 5, characterized in that: First raise the temperature to 300℃ and keep it for 30min, then raise the temperature to 350-600℃ and keep it for 10min-1h.

7. The method for preparing a nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy according to claim 5, characterized in that: B is derived from boron or ferroboron.

8. Nitrogen-containing iron-based soft magnetic amorphous / nanocrystalline alloy prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • High magnetic induction nitrogen-coupled iron-based amorphous nanocrystalline alloy and preparation method thereof

    CN109440023A

  • Nitrogen-containing iron-based amorphous nanocrystalline soft magnetic alloy and preparation method thereof

    CN109440058A

  • Method for producing metallic glass alloy, and the metallic glass alloy

    JP2012206140A

  • Soft magnetic amorphous alloy having nitrogen and preparing method thereof

    KR101783553B1

Cited By

  • Nano-catalyst as well as preparation method and application thereof

    CN120485815A

  • A nano-catalyst, a preparation method and application thereof

    CN120485815B