Transition metal chalcogenide nanotube one-step growth and structure controllable method
Through the chemical vapor deposition method assisted by gold nanoparticle catalyst, the problem of growth and chiral regulation of transition metal chalcogenide nanotubes is solved, and the uniform growth and structural controllability of nanotubes are achieved, which promotes its use in device applications. develop.
Patent Information
- Application Number
- CN202411027514.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to achieve simple and effective growth and chiral regulation of transition metal chalcogenide nanotubes, resulting in the stagnation of its development in device applications and research.
Using a chemical vapor deposition method assisted by gold nanoparticle catalyst, the evaporation of transition metal oxides and sulfur (selenium) is controlled separately through a dual-temperature zone high-temperature furnace, and a magnetron sputtering and annealing process is used to prepare a highly reactive gold nanoparticle catalyst to achieve the transition The growth and controllable structure of metal chalcogenide nanotubes are one-step.
It realizes the uniform growth, diameter and number of layers of transition metal chalcogenide nanotubes, meets the requirements of high crystal quality, high yield and chiral controllability, and promotes its application in basic research and high-performance devices. .
Smart Images

Figure CN118957761A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing transition metal chalcogenide nanotubes, which realizes one-step growth and controllable chirality of transition metal chalcogenide nanotubes through a chemical vapor deposition method catalyzed by gold nanoparticles. Background Art
[0002] With the continuous development of the preparation and structural regulation of two-dimensional transition metal chalcogenides, the types of two-dimensional transition metal chalcogenides are becoming more and more abundant, which further stimulates and promotes the in-depth exploration of their novel physical properties and device applications. At the same time, breaking through the original structure construction method and regulation strategy in the transition metal chalcogenide system and finding new research ideas have become the key to further expand the research and application of transition metal chalcogenides.
[0003] The transition metal sulfide nanotube structure is equivalent to a one-dimensional tubular structure formed by a two-dimensional transition metal sulfide curled along a specific direction. It has many unique properties compared to its two-dimensional and three-dimensional transition metal sulfide structures, such as the significantly enhanced bulk photovoltaic effect, superconductivity and lubrication in tungsten sulfide nanotubes, becoming a new world for the development of transition metal chalcogenides.
[0004] As early as 1992, transition metal sulfide nanotubes were first discovered by Professor Reshef Tenne. The preparation method is mainly based on the sulfurization reaction on the surface of transition metal oxide nanowires to form a multilayer nanotube structure. The preparation method has many processes and is difficult to control. The structure of the prepared nanotubes is random and cannot be regulated. As a result, the progress of transition metal sulfide nanotubes in chirality control, chirality-related physical property research and device applications has been slow in the past 30 years. Compared with the booming development of carbon nanotubes discovered in 1991 in the past 30 years, the development of transition metal chalcogenide nanotubes has almost stagnated. The main "bottleneck" hindering its development can be attributed to the lack of simple and effective growth methods and chirality control strategies for transition metal sulfide nanotubes. Recently, researchers have proposed a chemical vapor deposition method for growing tungsten sulfide and tungsten selenide nanotubes in a single temperature zone high temperature furnace in one step. However, this method cannot be adapted to the preparation of a variety of transition metal chalcogenide nanotubes, such as molybdenum sulfide, molybdenum selenide and molybdenum telluride. The main reason is that it is impossible to simultaneously evaporate transition metal oxides and sulfur (selenium) through a single-temperature zone high-temperature furnace, which limits the preparation, research and further application of these transition metal chalcogenide nanotubes. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for preparing transition metal chalcogenide nanotubes, and finally to realize a method for one-step growth and structure controllable transition metal chalcogenide nanotubes. The preparation method is a chemical vapor deposition method assisted by gold catalyst particles. A gold nanoparticle catalyst is obtained by annealing a gold film on a silicon substrate by magnetron sputtering, and the gold nanoparticle catalyst is used as a growth substrate to realize the growth of transition metal chalcogenide nanotubes in an inert atmosphere and at a certain temperature. The obtained transition metal chalcogenide nanotubes have uniform tube diameter, controllable diameter and adjustable number of layers, meeting the requirements of high crystal quality, high yield and controllable chirality of transition metal chalcogenide nanotubes.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0007] The present invention provides a method for achieving one-step growth and structure controllable transition metal chalcogenide nanotubes by controlling the evaporation of transition metal oxides and sulfur (selenium) respectively in a dual-temperature zone high-temperature furnace. Among them, gold nanoparticles are used as catalysts and are the key to the nucleation of transition metal chalcogenide nanotubes. By controlling the thickness of magnetron sputtering coating and the temperature and time of annealing, gold nanoparticles can form gold nanoparticle catalysts with different diameters and high catalytic activity after annealing. The preparation steps are as follows:
[0008] S1: Using high-purity gold as the sputtering target and silicon wafer as the sputtering substrate, sputtering for 35 seconds at 100°C and 50W DC power to obtain a gold film with a uniform thickness of 10nm;
[0009] S2: The gold film obtained by magnetron sputtering is placed in a high-temperature tube furnace for annealing. The temperature is first raised from 25°C to 750°C in 40 minutes, then kept at 750°C for 10 minutes, and finally dropped to 25°C in 10 minutes, thereby obtaining a gold nanoparticle catalyst with high catalytic activity and uniform particle diameter on the silicon wafer; the prepared silicon wafer with gold nanoparticles is placed on a rectangular sample table;
[0010] S3: Use a quartz boat (15mm*100mm) to weigh the transition metal oxide and chalcogenide powder respectively, spread the transition metal oxide evenly on the quartz boat, and place the chalcogenide powder on the feeding device;
[0011] S4: placing the quartz boat and the sample stage into specific areas of the high-temperature tube furnace respectively; placing the feeding device in the non-heating area on the right side of the high-temperature tube furnace;
[0012] S5: Set a specific heating interval and heating temperature. When the temperature reaches a certain temperature, start to introduce a certain amount of hydrogen and nitrogen mixed gas. At the same time, the feeding device slowly feeds the chalcogenide powder into the right temperature zone to make it reach the initial melting state, and evenly push the chalcogenide powder within a certain period of time until it is completely evaporated.
[0013] S6: When the insulation time of the left temperature zone is over, stop insulation and let the temperature drop naturally to 25°C. When the insulation time of the right temperature zone is over, stop insulation and let the temperature drop naturally to 25°C. Take out the sample table to obtain the finished product.
[0014] Furthermore, the feeding device includes a magnetic base and a magnet. The chalcogenide powder is placed on the magnetic base. The magnet is located outside the high-temperature tube furnace. By moving the magnet, the magnetic base inside the high-temperature tube furnace is driven to move.
[0015] Furthermore, the metal oxide in S3 is MoO3, and the chalcogen element powder is one of S and Se.
[0016] Compared with the prior art, this application has the following beneficial effects:
[0017] The present application prepares a highly active gold nanoparticle catalyst by magnetron sputtering and annealing process, and has excellent high temperature stability. Using the method of chemical vapor deposition (CVD), a silicon wafer modified with a gold nanoparticle catalyst is placed in a specific temperature zone of a dual-temperature high-temperature tube furnace, and this is used as a growth substrate to provide a growth platform for transition metal chalcogenide nanotubes. By controlling the different ratios and reaction conditions of transition metal oxides and chalcogen elements, the growth conditions of transition metal chalcogenide nanotubes with one-step growth and controllable chirality are achieved. The preparation method is simple to prepare, and one-step growth and controllable structure of transition metal chalcogenide nanotubes are achieved, and relatively uniform transition metal chalcogenide nanotubes are obtained. At the same time, the temperature of the growth substrate can be controlled to achieve controllable regulation of the diameter and number of layers of transition metal chalcogenide nanotubes. Chirality-controllable nanotubes play a very important role in basic research, high-performance optoelectronic devices, and new energy devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The SEM image of gold nanoparticles formed on the silicon wafer provided by the present invention;
[0019] Figure 2 The SEM image of the transition metal chalcogenide nanotube provided by the present invention;
[0020] Figure 3 TEM image and composition image of the molybdenum sulfide nanotube provided by the present invention;
[0021] Figure 4 Provides TEM images and composition images of prepared molybdenum selenide nanotubes in the present invention;
[0022] Figure 5 A schematic diagram of a device for preparing molybdenum sulfide and molybdenum selenide nanotubes is provided for the present invention. DETAILED DESCRIPTION
[0023] The present invention is further described in detail below by combining implementation examples, but the specific implementation scope is not limited to the examples given.
[0024] Example 1
[0025] Provided is a method for preparing molybdenum sulfide nanotubes, the preparation method consists of two parts: preparation of gold nanoparticle catalyst and chemical vapor deposition growth, and the preparation steps are as follows:
[0026] S1: Using high-purity gold as the sputtering target and silicon wafer as the sputtering substrate, sputtering for 35 seconds at 100°C and 50W DC power to obtain a gold film with a uniform thickness of 10nm;
[0027] S2: The gold film obtained by magnetron sputtering is placed in a high-temperature tube furnace for annealing. The temperature is first raised from 25°C to 750°C in 40 minutes, then kept at 750°C for 10 minutes, and finally dropped to 25°C in 10 minutes, thereby obtaining a gold nanoparticle catalyst with high catalytic activity and uniform particle diameter on the silicon wafer; Figure 1 As shown; the prepared silicon wafer with gold nanoparticle catalyst is placed on the rectangular sample stage;
[0028] S3: Use a quartz boat (15mm*100mm) to weigh 0.55g of nano molybdenum trioxide (99.9% metal base) and 0.8g of sulfur powder (>99.5%) respectively, spread the molybdenum trioxide evenly on the quartz boat, and place the sulfur powder on the feeding device;
[0029] S4: Place the quartz boat in the center of the left temperature zone of the high-temperature tube furnace, place the sample table in the right temperature zone of the tube furnace, and place the feeding device in the non-heating zone on the right side of the high-temperature tube furnace;
[0030] S5: First heat the right temperature zone of the high-temperature tube furnace, and raise the temperature of the right temperature zone from 25°C to 900°C within 40 minutes. When the right temperature zone starts to heat for 20 minutes, start heating the left temperature zone, and raise the temperature of the center of the left temperature zone of the high-temperature tube furnace from 25°C to 520°C within 20 minutes. When the temperature of the left temperature zone rises to 520°C and the temperature of the right temperature zone rises to 900°C, introduce 14sccm of hydrogen and 150sccm of nitrogen from the left side of the high-temperature tube furnace to adjust the high-temperature tube furnace. The air pressure is maintained at a constant low pressure; then the left and right temperature zones are heated up, the left temperature zone is heated up to 580°C within 4 minutes, and maintained at 580°C for 15 minutes. While the left temperature zone is heated up, the right temperature zone is heated up to 985°C within 5 minutes, and maintained at 985°C for 19 minutes. When the temperature of the left temperature zone reaches 580°C, the sulfur powder is slowly fed into the right temperature zone by a feeding device to make it reach an initial melting state, and the sulfur powder is evenly pushed forward within 15 minutes until it is completely evaporated.
[0031] S6: When the insulation time of the left temperature zone is over, stop insulation and let the temperature drop naturally to 25°C. When the insulation time of the right temperature zone is over, stop insulation and let the temperature drop naturally to 25°C. Take out the sample table to obtain the finished product.
[0032] Example 2
[0033] Provided is a method for preparing molybdenum selenide nanotubes, the preparation method consists of two parts: preparation of gold nanoparticle catalyst and chemical vapor deposition growth, and the preparation steps are as follows:
[0034] S1: Using high-purity gold as the sputtering target and silicon wafer as the sputtering substrate, sputtering for 35 seconds at 100°C and 50W DC power to obtain a gold film with a uniform thickness of 10nm;
[0035] S2: The gold film obtained by magnetron sputtering is placed in a high-temperature tube furnace for annealing. The temperature is first raised from 25°C to 750°C in 40 minutes, then kept at 750°C for 10 minutes, and finally dropped to 25°C in 10 minutes, thereby obtaining a gold nanoparticle catalyst with high catalytic activity and uniform particle diameter on the silicon wafer; Figure 1 As shown; the prepared silicon wafer with gold nanoparticle catalyst is placed on the rectangular sample stage;
[0036] S3: Use a quartz boat (15mm*100mm) to weigh 0.55g of nano molybdenum trioxide (99.9% metal base) and 2.0g of selenium powder (>99.5%) respectively, spread the molybdenum trioxide evenly on the quartz boat, and place the selenium powder on the feeding device;
[0037] S4: Place the quartz boat in the center of the left temperature zone of the high-temperature tube furnace, place the sample table in the right temperature zone of the tube furnace, and place the feeding device in the non-heating zone on the right side of the high-temperature tube furnace;
[0038] S5: First heat the right temperature zone of the high-temperature tube furnace, and raise the temperature of the right temperature zone from 25°C to 900°C within 40 minutes. When the right temperature zone starts to heat for 20 minutes, start heating the left temperature zone, and raise the temperature of the center of the left temperature zone of the high-temperature tube furnace from 25°C to 510°C within 20 minutes. When the temperature of the left temperature zone rises to 510°C and the temperature of the right temperature zone rises to 900°C, introduce 13sccm of hydrogen and 150sccm of nitrogen from the left side of the high-temperature tube furnace to adjust the high-temperature tube furnace. The air pressure is maintained at a constant low pressure; then the left and right temperature zones continue to be heated, the left temperature zone is heated to 580°C within 4 minutes, and maintained at 580°C for 15 minutes. While the left temperature zone is heated, the right temperature zone is heated to 985°C within 5 minutes, and maintained at 985°C for 15 minutes. When the temperature of the left temperature zone reaches 580°C, the feeding device is used to slowly feed the selenium powder into the right temperature zone to make it reach the initial melting state, and the selenium powder is evenly pushed forward within 15 minutes until it is completely evaporated.
[0039] S6: After the insulation time of the left temperature zone is over, stop insulation and let the temperature drop naturally to 25°C. After the insulation time of the right temperature zone is over, stop insulation and let the temperature drop naturally to 25°C. Take out the sample table to obtain the finished product.
[0040] The finished products were taken out, and the SEM and TEM test results showed that the grown nanotubes had uniform diameters and controllable number of layers, meeting the requirements of high-quality and large-scale growth.
Claims
1. A method for preparing transition metal chalcogenide nanotubes, characterized in that: The specific steps are as follows: S1: Using high-purity gold as the sputtering target and silicon wafer as the sputtering substrate, sputtering for 35 seconds at 100°C and 50W DC power to obtain a gold film with a uniform thickness of 10nm; S2: The gold film obtained by magnetron sputtering is placed in a high-temperature tube furnace for annealing. The temperature is first raised from 25°C to 750°C in 40 minutes, then kept at 750°C for 10 minutes, and finally dropped to 25°C in 10 minutes, thereby obtaining a gold nanoparticle catalyst with high catalytic activity and uniform particle diameter on the silicon wafer; the prepared silicon wafer with gold nanoparticles is placed on a rectangular sample table; S3: Use a quartz boat to weigh transition metal oxide and chalcogenide powder respectively, spread the transition metal oxide evenly on the quartz boat, and place the chalcogenide powder on the feeding device; S4: placing the quartz boat and the sample stage into specific areas of the high-temperature tube furnace respectively; placing the feeding device in the non-heating area on the right side of the high-temperature tube furnace; S5: Set a specific heating interval and heating temperature. When the temperature reaches a certain temperature, start to introduce a certain amount of hydrogen and nitrogen mixed gas. At the same time, the feeding device slowly feeds the chalcogenide powder into the right temperature zone to make it reach the initial melting state, and evenly push the chalcogenide powder within a certain period of time until it is completely evaporated. S6: When the insulation time of the left temperature zone is over, stop insulation and let the temperature drop naturally to 25°C. When the insulation time of the right temperature zone is over, stop insulation and let the temperature drop naturally to 25°C. Take out the sample table to obtain the finished product.
2. The method according to claim 1, characterized in that The feeding device includes a magnetic base and a magnet. Chalcogenide powder is placed on the magnetic base. The magnet is located outside the high-temperature tube furnace. By moving the magnet, the magnetic base in the high-temperature tube furnace is driven to move.
3. The method according to claim 2, characterized in that The metal oxide in S3 is MoO3, and the chalcogen element powder is one of S and Se.
Citation Information
Cited By
Method for preparing transition metal chalcogenide heterojunction nanotube with assistance of gold catalyst particles
CN119411098A
Method for the gold catalyst particle assisted preparation of transition metal chalcogenide heterostructure nanotubes
CN119411098B