Titanium dioxide-phenolic resin-crystalline flake graphite composite cathode and preparation method thereof

Through the preparation of titanium dioxide-phenolic resin-graphite composite cathode, the problem of graphite cathode surface emission defect and short life of metal cathode is solved, high conductivity and good electron emission performance are achieved, cathode life is extended and output power is improved.

CN118969580APending Publication Date: 2024-11-15UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028798.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing high-power microwave sources, the surface emission defect of the graphite cathode is severe, resulting in damage to the output power. The metal cathode plasma expands rapidly and has a short life, making it impossible to achieve stable pulse operation of tens of thousands of times.

Method used

The titanium dioxide-phenolic resin-graphite composite cathode is used to form a mixed extrusion of scale graphite powder, TiO2 particles and phenolic resin as matrix, dopant material and binder, and is made through a heat treatment process, combining gradient heating and mechanical processing. A cathode with high electrical conductivity and good electron emission properties is formed.

Benefits of technology

It effectively suppresses surface emission defects, extends the service life of the cathode, improves electron emission performance and conductivity, reduces plasma drift speed, simplifies the preparation process and reduces the cost of raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969580A_ABST
    Figure CN118969580A_ABST
Patent Text Reader

Abstract

The invention discloses a graphite-phenolic resin-graphite composite cathode and a preparation method thereof, and belongs to the technical field of high-power microwaves. The cathode is prepared by mixing, extruding and molding graphite powder, TiO2 particles and an adhesive, and then carrying out gradient heating treatment. The titanium dioxide is added into the graphite powder, so that the surface emission defect is effectively inhibited; phenolic resin is adopted as an adhesive, and a gradient heating process is adopted, so that the structural strength of graphite powder and titanium dioxide powder is effectively enhanced, and the graphite powder and the titanium dioxide powder can be directly machined into a required cathode shape. According to the titanium dioxide-phenolic resin-graphite composite cathode, the preparation method is simple and convenient, the cost of raw materials is low, and the prepared cathode has good electron emission performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-power microwaves, relates to a titanium dioxide-phenolic resin-graphite composite cathode and a preparation method thereof, and can be applied to the fields of large-area high-current pulse electron beam technology and high-power microwaves. Background Art

[0002] In a high-power microwave source, the cathode is guided by a strong electric field to emit electrons and form a strong electron beam. This electron beam exchanges energy with electromagnetic waves to generate high-power microwaves. Therefore, the cathode is the core component of a high-power microwave source.

[0003] The large-area explosive emission cathode is the most commonly used cathode in the orthogonal field high-power microwave source, and its commonly used materials include metal, velvet, graphite, etc. The plasma expansion rate of the metal cathode is relatively fast, which will lead to the problem of pulse shortening. The velvet cathode has a short life and cannot achieve stable operation of tens of thousands of pulses. The graphite cathode has the advantages of long life and low plasma expansion rate. Therefore, the large-area graphite cathode is one of the most commonly used cathodes in the orthogonal field high-power microwave source; however, the graphite cathode has serious surface emission defects, which damages the output power of the orthogonal field high-power microwave source. Suppressing the surface emission defects of the graphite cathode is an issue that needs to be urgently addressed to improve power.

[0004] Titanium dioxide is an excellent field emission material with the characteristics of low work function and high melting point. Cathode material modification technology based on titanium dioxide is expected to become a key technology to improve the performance of explosive emission cathodes. Krasik et al.'s paper "High-current electron beam generation by a metal-ceramic cathode[J].Journal of Applied Physics,2002,91(11):9385-9392." believes that titanium dioxide medium composite can generate plasma of stainless steel cathode under lower electric field. Li et al.'s paper "Cold atmospheric pressure plasmajet prepares TiO2 coating on carbon fiber for field emission and explosive electron emission[J].Journal of Physics D Applied Physics,2021,54(41):415201." The results show that the carbon fiber cathode coated with titanium dioxide particles has more emission micropoints than the carbon fiber cathode. However, titanium dioxide and its modified materials are difficult to directly process into cathodes with certain shapes and sizes, and special tooling is required for processing and drilling. Summary of the invention

[0005] The purpose of the present invention is to solve the problems pointed out in the background technology, and to provide a titanium dioxide-phenolic resin-graphite composite cathode and a preparation method thereof.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A titanium dioxide-phenolic resin-graphite composite cathode, characterized in that the composite cathode is formed by mixing and extruding a matrix material, a doping material and an adhesive, and then undergoing a heat treatment process; the matrix material is flake graphite powder, the doping material is TiO2 particles, and the adhesive is a mixed solution with a mass ratio of phenolic resin to alcohol of 1:1.

[0008] Preferably, the mass ratio of the matrix material to the doping material is 8:1 to 3:1; the mass ratio of the mixed powder of the matrix material and the doping material to the binder is 9:1 to 4:1.

[0009] Preferably, the particle diameter of the TiO2 particles is 20 nm to 1 μm.

[0010] Preferably, the carbon content of the flake graphite powder is greater than 99.99%, and the particle diameter of the flake graphite powder is one of 100 mesh, 320 mesh, 800 mesh, 3000 mesh or 10000 mesh, or a mixed powder of two or more thereof.

[0011] The present invention also proposes a method for preparing the titanium dioxide-phenolic resin-graphite composite cathode, comprising the following steps:

[0012] S1. Preheating the flake graphite powder and TiO2 particles separately.

[0013] S2. The preheated flake graphite powder and TiO2 particles are mixed evenly in proportion to obtain titanium dioxide-flake graphite mixed powder.

[0014] S3. The binder and the titanium dioxide-flake graphite mixed powder are mixed evenly in proportion to obtain a titanium dioxide-phenolic resin-graphite mixed powder.

[0015] S4. Put the titanium dioxide-phenolic resin-graphite mixed powder into a molding die, press it into shape by a molding method, and obtain a cathode embryo after demolding.

[0016] S5. The cathode embryo body is heat treated using a gradient heating method.

[0017] S6. Mechanically process the cathode embryo body after heat treatment into a preset size structure to obtain a titanium dioxide-phenolic resin-graphite composite cathode.

[0018] Preferably, in step S1, the flake graphite powder and TiO2 particles are respectively loaded into different crucibles and then placed in a muffle furnace for preheating treatment at a temperature of 200°C to 250°C and a preheating time of 2h to 3h.

[0019] Preferably, the mass ratio of flake graphite powder to TiO2 particles is 8:1 to 3:1; the mass ratio of titanium dioxide-flake graphite mixed powder to binder is 9:1 to 4:1.

[0020] Preferably, in step S2, the flake graphite powder and TiO2 particles are mixed as follows: the flake graphite powder and TiO2 particles are placed in a ball mill of a planetary ball mill, and stainless steel grinding balls of equal mass are placed therein; during grinding, the rotation speed of the planetary ball mill is 320 rpm to 480 rpm, and the grinding time is 2h to 6h.

[0021] In step S3, the titanium dioxide-flake graphite mixed powder and the binder are mixed in the following manner: first, a glass rod is used for stirring, the stirring speed of the glass rod is 30 rpm to 50 rpm, and the stirring time is 10 min to 30 min; then the mixture is placed in a ball mill of a planetary ball mill, and during grinding, the rotation speed of the planetary ball mill is 320 rpm to 480 rpm, and the grinding time is 2 h to 6 h.

[0022] Preferably, in step S4, the molding method is to use a hydraulic press to pressurize the mixed powder; the pressurization conditions are: 200-250 MPa for 20-30 min.

[0023] Preferably, in step S5, the gradient heating method is: keep warm at 60°C for 30min to 40min, then keep warm at 100°C for 30min to 40min, and finally keep warm at 150°C for 60min to 150min.

[0024] Beneficial effects of the present invention:

[0025] 1). The titanium dioxide-phenolic resin-graphite composite cathode of the present invention has a matrix made of flake graphite powder, which has good electrical and thermal conductivity and a high melting point, thereby ensuring the service life of the cathode.

[0026] 2). The titanium dioxide-phenolic resin-graphite composite cathode of the present invention uses TiO2 as a dopant. TiO2 has the characteristic of low work function, which can suppress surface emission defects and make the cathode have good electron emission performance; at the same time, TiO2 also has the characteristic of high melting point, which will not damage the life of the cathode.

[0027] 3). The titanium dioxide-phenolic resin-graphite composite cathode of the present invention uses dopant elements including Ti and O, which have atomic numbers higher than carbon, thereby further reducing the plasma drift velocity of the flake graphite.

[0028] 4). The titanium dioxide-phenolic resin-graphite composite cathode of the present invention uses phenolic resin as a binder, which can effectively enhance the structural strength of graphite powder and titanium dioxide powder, so that it can be directly machined into the desired cathode shape.

[0029] 5). The titanium dioxide-phenolic resin-graphite composite cathode of the present invention adopts a gradient heating process, which ensures that the gas generated by the decomposition of the phenolic resin during the heating process will not destroy the structure of the cathode.

[0030] 6). The titanium dioxide-phenolic resin-graphite composite cathode of the present invention has a simple and convenient preparation method, low raw material cost and strong operability. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the X-ray diffraction test result of the graphite used in Example 1 of the present invention.

[0032] Figure 2 This is the X-ray diffraction test result of the TiO2 particles used in Example 1 of the present invention.

[0033] Figure 3 This is the microstructure of the titanium dioxide-phenolic resin-graphite composite cathode prepared in Example 1 of the present invention.

[0034] Figure 4 This is the microstructure of the titanium dioxide-phenolic resin-graphite composite cathode prepared in Example 2 of the present invention.

[0035] Figure 5 This is a physical picture of the titanium dioxide-phenolic resin-graphite composite cathode prepared in comparative example 1 of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application, but the scope of protection of the present invention is not limited thereby.

[0037] The present invention is described in detail below in conjunction with the accompanying drawings. The materials and equipment designed in the following embodiments are all commercially available.

[0038] Embodiment 1:

[0039] This embodiment provides a titanium dioxide-phenolic resin-graphite composite cathode, which is prepared from flake graphite powder, titanium dioxide particles and a binder, wherein the binder is a phenolic resin-alcohol mixed solution with a mass ratio of 1:1.

[0040] In this embodiment, the mass ratio of the flake graphite powder, the titanium dioxide particles, and the binder is 3.8:1:1, calculated by mass fraction.

[0041] In this embodiment, the flake graphite powder used is 10000 mesh flake graphite powder. The X-ray diffractometer test results of the particles are as follows: Figure 1 As shown, it can be seen that a strong diffraction peak appears near 2Theta of 26.5°, which indicates that the graphite powder has a high degree of graphitization.

[0042] In this embodiment, the titanium dioxide powder used is 1 μm particles. The X-ray diffractometer test results of the particles are as follows: Figure 2 As shown, it can be seen that strong diffraction peaks appear simultaneously near 2Theta of 25.5° and 27.6°, which indicates that the titanium dioxide particles exist in both rutile phase and anatase phase.

[0043] The preparation steps of this embodiment are as follows:

[0044] S01. Pretreatment: First, 10000 mesh flake graphite powder and 1 μm TiO2 particles were loaded into crucibles respectively, and then placed in a muffle furnace for pretreatment at 200°C for 2 h.

[0045] S02. Mixing and primary grinding of powders: Weigh 100 g of pretreated 10000 mesh flake graphite powder and 25 g of pretreated 1 μm TiO2 particles; put both into a ball mill and load stainless steel grinding balls of equal mass; set the planetary ball mill speed to 480 rpm and the grinding time to 4 h.

[0046] S03. Mixing of binder and powder and secondary grinding: Weigh 100 g of the mixture and powder obtained in step S02 and put them into a beaker, then add 25 g of binder solution into the beaker; use a glass rod to stir at a speed of 30 rpm for 30 minutes; then put the stirred mixture into a ball mill, control the speed of the planetary ball mill to 400 rpm, and grind for 6 hours.

[0047] S04. Molding: Weigh 20 g of the mixture obtained in step S03 and put it into a stainless steel compression mold. Use a hydraulic press to maintain the pressure at 250 MPa for 30 minutes to obtain a cathode embryo.

[0048] S05. Heat treatment: Take out the pressed cathode embryo and put it into a blast drying oven for gradient heating. The gradient heating method is: keep warm at 60℃ for 30min, keep warm at 100℃ for 30min, and keep warm at 150℃ for 120min.

[0049] S06. Cathode processing: The cathode embryo after heat treatment is processed into a preset structural size, that is, a titanium dioxide-phenolic resin-graphite composite cathode is obtained, and its microstructure is as follows Figure 3 shown.

[0050] The titanium oxide-phenolic resin-graphite composite cathode prepared in the present embodiment is tested on a permanent magnet package 10-cavity sunburst radial extraction relativistic magnetron. Under a driving voltage of 400kV, the emission current is 16.2kA, the microwave pulse width is 62ns, and the microwave power amplitude is 480MW. While the graphite cathode of the same size has an emission current of 16.0kA, a microwave pulse width of 56ns, and a microwave power amplitude of 320MW under an excitation voltage of 400kV. It can be seen from this that the titanium dioxide-phenolic resin-graphite composite cathode microwave pulse width is larger, and the microwave power amplitude is larger, that is, the titanium dioxide-phenolic resin-graphite composite cathode has better electron emission performance.

[0051] Examples 2 and 3 mainly focus on the composition and process parameters of the titanium dioxide-phenolic resin-graphite composite cathode to illustrate the preparation method of this type of cathode. The electron emission performance of this type of cathode is comparable to that of Example 1, and is superior to that of a graphite cathode of the same size.

[0052] Embodiment 2:

[0053] This embodiment provides a titanium dioxide-phenolic resin-graphite composite cathode, which is prepared from flake graphite powder, titanium dioxide particles and a binder, wherein the binder is a phenolic resin-alcohol mixed solution with a mass ratio of 1:1.

[0054] In this embodiment, the mass ratio of the flake graphite powder, the titanium dioxide particles and the binder is 7:1:2 by mass fraction; the flake graphite powder is 100 mesh flake graphite powder; and the titanium dioxide powder is 40 nm particles.

[0055] The preparation steps of this embodiment are as follows:

[0056] S01. Pretreatment: First, 100 mesh flake graphite powder and 40 nm TiO2 particles were loaded into crucibles respectively, and then placed in a muffle furnace for pretreatment at 200 °C for 2 h.

[0057] S02. Mixing and primary grinding of powders: Weigh 100 g of pretreated 100-mesh flake graphite powder and 25 g of pretreated 40 nm TiO2 particles; put both into a ball mill and load stainless steel grinding balls of equal mass; set the planetary ball mill speed to 320 rpm and the grinding time to 6 h.

[0058] S03. Mixing of adhesive and powder and secondary grinding: weigh 60 g of the mixture and powder obtained in step S02 and put them into a beaker, then add 20 g of adhesive solution into the beaker; use a glass rod to stir at a speed of 50 rpm for 30 minutes; then put the stirred mixture into a ball mill, control the speed of the planetary ball mill to 450 rpm, and grind for 3 hours.

[0059] S04. Molding: Weigh 20 g of the mixture obtained in step S03 and put it into a stainless steel compression mold. Use a hydraulic press to maintain the pressure at 200 MPa for 30 minutes to obtain a cathode embryo.

[0060] S05. Heat treatment: Take out the pressed cathode embryo and put it into a blast drying oven for gradient heating. The gradient heating method is: keep warm at 60℃ for 40min, keep warm at 100℃ for 40min, and keep warm at 150℃ for 60min.

[0061] S06. Cathode processing: The cathode embryo body after heat treatment is processed into a preset structural size to obtain a titanium dioxide-phenolic resin-graphite composite cathode, whose microstructure is as follows Figure 4 As shown, graphite presents a layered structure, and titanium dioxide is embedded in the graphite layered structure.

[0062] Embodiment 3:

[0063] This embodiment provides a titanium dioxide-phenolic resin-graphite composite cathode, which is prepared from flake graphite powder, titanium dioxide particles and a binder, wherein the binder is a phenolic resin-alcohol mixed solution with a mass ratio of 1:1.

[0064] In this embodiment, the mass ratio of the flake graphite powder, the titanium dioxide particles, and the binder is 8:1:1, calculated by mass fraction; the flake graphite powder is 800 mesh flake graphite powder; and the titanium dioxide powder is 100 nm particles.

[0065] The preparation steps of this embodiment are as follows:

[0066] S01. Pretreatment: First, 800 mesh flake graphite powder and 100 nm TiO2 particles were loaded into crucibles respectively, and then placed in a muffle furnace for pretreatment at 250°C for 2 h.

[0067] S02. Mixing and primary grinding of powders: Weigh 80 g of pretreated 800 mesh flake graphite powder and 10 g of pretreated 100 nm TiO2 particles; put both into a ball mill and load stainless steel grinding balls of equal mass; set the planetary ball mill speed to 320 rpm and the grinding time to 6 h.

[0068] S03. Mixing of binder and powder and secondary grinding: weigh 70 g of the mixture and powder obtained in step S02 and put them into a beaker, then add 10 g of binder solution to the beaker; use a glass rod to stir at a speed of 45 rpm for 30 minutes; then put the stirred mixture into a ball mill, control the speed of the planetary ball mill to 400 rpm, and grind for 5 hours.

[0069] S04. Molding: Weigh 20 g of the mixture obtained in step S03 and put it into a stainless steel compression mold. Use a hydraulic press to maintain the pressure at 250 MPa for 20 minutes to obtain a cathode embryo.

[0070] S05. Heat treatment: Take out the pressed cathode embryo and put it into a blast drying oven for gradient heating. The gradient heating method is: keep warm at 60℃ for 30min, keep warm at 100℃ for 30min, and keep warm at 150℃ for 150min.

[0071] S06. Cathode processing: Processing the cathode embryo after heat treatment into a preset structural size to obtain a titanium dioxide-phenolic resin-graphite composite cathode.

[0072] Comparative Example 1:

[0073] This comparative example is a comparative example of Example 3, and the raw materials and proportions used are the same as those of Example 3, except that the comparative example does not use the gradient heating heat treatment method.

[0074] The preparation method of this comparative example comprises the following steps:

[0075] S01. Pretreatment: First, 800 mesh flake graphite powder and 100 nm TiO2 particles were loaded into crucibles respectively, and then placed in a muffle furnace for pretreatment at 250°C for 2 h.

[0076] S02. Mixing and primary grinding of powders: Weigh 80 g of pretreated 800 mesh flake graphite powder and 10 g of pretreated 100 nm TiO2 particles; put both into a ball mill and load stainless steel grinding balls of equal mass; set the planetary ball mill speed to 320 rpm and the grinding time to 6 h.

[0077] S03. Mixing of binder and powder and secondary grinding: weigh 70 g of the mixture and powder obtained in step S02 and put them into a beaker, then add 10 g of binder solution to the beaker; use a glass rod to stir at a speed of 45 rpm for 30 minutes; then put the stirred mixture into a ball mill, control the speed of the planetary ball mill to 400 rpm, and grind for 5 hours.

[0078] S04. Molding: Weigh 20 g of the mixture obtained in step S03 and put it into a stainless steel compression mold. Use a hydraulic press to maintain the pressure at 250 MPa for 20 minutes to obtain a cathode embryo.

[0079] S05. Heat treatment: Take out the pressed cathode embryo and put it into a forced air drying oven. The heating method is: keep warm at 150℃ for 150 minutes.

[0080] S06. Cathode processing: The cathode embryo after heat treatment is processed into a preset structural size to obtain a titanium dioxide-phenolic resin-graphite composite cathode. The appearance of the prepared cathode is as follows Figure 5 As shown, there are obvious cracks on the surface, which cannot meet the requirements of mechanical processing.

[0081] The above embodiments are intended to illustrate the present invention, not to limit the present invention. Any solution that is a simple transformation of the present invention belongs to the protection scope of the present invention.

Claims

1. A titanium dioxide-phenolic resin-graphite composite cathode, characterized in that: The composite cathode is formed by mixing and extruding a matrix material, a doping material and a binder, and then undergoing a heat treatment process; the matrix material is flake graphite powder, the doping material is TiO2 particles, and the binder is a mixed solution of phenolic resin: alcohol in a mass ratio of 1:

1.

2. A titanium dioxide-phenolic resin-graphite composite cathode as claimed in claim 1, characterized in that: The mass ratio of the matrix material to the doping material is 8:1 to 3:1; the mass ratio of the mixed powder of the matrix material and the doping material to the adhesive is 9:1 to 4:

1.

3. A titanium dioxide-phenolic resin-graphite composite cathode as claimed in claim 1, characterized in that: The particle diameter of the TiO2 particles is 20nm to 1μm; the carbon content of the flake graphite powder is greater than 99.99%, and the particle diameter of the flake graphite powder is one of 100 mesh, 320 mesh, 800 mesh, 3000 mesh or 10000 mesh, or a mixed powder of two or more thereof.

4. A method for preparing a titanium dioxide-phenolic resin-graphite composite cathode, characterized in that: It includes the following steps: S1. The flake graphite powder and TiO2 particles are preheated separately; S2. The preheated graphite flake powder and TiO2 particles are mixed uniformly in proportion to obtain a titanium dioxide - flake graphite mixed powder; S3. The binder and titanium dioxide - flake graphite mixed powder are uniformly mixed in proportion to obtain titanium dioxide - phenolic resin - graphite mixed powder; S4. The titanium dioxide - phenolic resin - graphite mixed powder is placed in a molding mold, pressed by a molding method, and the cathode embryo is obtained after demolding; S5. The cathode embryo is heat treated using a gradient heating method; S6. Mechanically process the cathode embryo body after heat treatment into a preset size structure to obtain a titanium dioxide-phenolic resin-graphite composite cathode.

5. The method for preparing a titanium dioxide-phenolic resin-graphite composite cathode according to claim 4, characterized in that: In step S5, the gradient heating method is: keep warm at 60°C for 30min to 40min, then keep warm at 100°C for 30min to 40min, and finally keep warm at 150°C for 60min to 150min.

6. The method for preparing a titanium dioxide-phenolic resin-graphite composite cathode according to claim 5, characterized in that: The mass ratio of flake graphite powder to TiO2 particles is 8:1 to 3:1; the mass ratio of titanium dioxide-flake graphite mixed powder to adhesive is 9:1 to 4:

1.

7. The method for preparing a titanium dioxide-phenolic resin-graphite composite cathode according to claim 6, characterized in that: In step S3, the titanium dioxide-flake graphite mixed powder and the binder are mixed in the following manner: first, a glass rod is used for stirring, the stirring speed of the glass rod is 30 rpm to 50 rpm, and the stirring time is 10 min to 30 min; then the mixture is placed in a ball mill of a planetary ball mill, and during grinding, the rotation speed of the planetary ball mill is 320 rpm to 480 rpm, and the grinding time is 2 h to 6 h.

8. The method for preparing a titanium dioxide-phenolic resin-graphite composite cathode according to claim 7, characterized in that: In step S2, the flake graphite powder and TiO2 particles are mixed in the following manner: the flake graphite powder and TiO2 particles are placed in a ball mill of a planetary ball mill, and stainless steel grinding balls of equal mass are placed therein; during grinding, the rotation speed of the planetary ball mill is 320 rpm to 480 rpm, and the grinding time is 2h to 6h.

9. The method for preparing a titanium dioxide-phenolic resin-graphite composite cathode according to claim 8, characterized in that: In step S1, flake graphite powder and TiO2 particles are respectively loaded into different crucibles, and then placed in a muffle furnace for preheating treatment. The preheating treatment is carried out at a temperature of 200°C to 250°C and a preheating time of 2h to 3h.

10. The method for preparing a titanium dioxide-phenolic resin-graphite composite cathode according to claim 9, characterized in that: In step S4, the molding method is to use a hydraulic press to pressurize the mixed powder; the pressurization conditions are: 200-250 MPa for 20-30 minutes.