Lithium phosphate coated ternary material as well as preparation method and application thereof

Through the combination of rare earth element doped with nickel-cobalt-manganese ternary material and amorphous lithium phosphate, the problem of low coating amount and complex method is solved, and the crystal phase transition and stress problems of the ternary material are suppressed. Improves the cycle performance and stability of the battery.

CN118969991APending Publication Date: 2024-11-15GEM WUXI ENERGY MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411023648.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, lithium phosphate coated ternary materials have a small amount of lithium phosphate, and the method is complicated, and it is impossible to effectively suppress the volume changes and anisotropic internal stress caused by crystal phase transition between ternary materials, resulting in attenuation of battery capacity and cycling performance.

Method used

Rare earth element doped with nickel-cobalt-manganese ternary material and amorphous lithium phosphate are coated. By combining rare earth element doping and amorphous lithium phosphate, a material with high surface energy and internal atomic arrangement is prepared. , inhibit crystal phase transition and stress concentration, and improve battery performance.

Benefits of technology

It significantly improves the electron conduction capability, lithium ion migration rate and charge transfer efficiency of lithium phosphate-coated ternary materials, extends the cycling durability and long-term stability of the battery, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967963110000101
    Figure BDA0004967963110000101
  • Figure BDA0004967963110000111
    Figure BDA0004967963110000111
  • Figure BDA0004967963110000112
    Figure BDA0004967963110000112
Patent Text Reader

Abstract

The invention belongs to the technical field of battery material preparation, and particularly relates to a lithium phosphate coated ternary material as well as a preparation method and application thereof. The lithium phosphate coated ternary material provided by the invention comprises a rare earth element doped nickel-cobalt-manganese ternary material and lithium phosphate, and the lithium phosphate coats the rare earth element doped nickel-cobalt-manganese ternary material; the lithium phosphate is amorphous lithium phosphate; the rare earth element is at least one of niobium, cerium, yttrium, lanthanum and scandium. The lithium phosphate coated ternary material can simultaneously inhibit crystal phase transformation between the materials and reduce stress between the materials, can be prepared on a large scale, and is simple and convenient in preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery material preparation, and in particular relates to a lithium phosphate coated ternary material and a preparation method and application thereof. Background Art

[0002] At present, nickel-cobalt-manganese (NCM) ternary materials have become common positive electrode materials for power batteries because of their high energy density, low cost and reliable safety. NCM ternary materials are secondary agglomerate microspheres formed by irregular and dense stacking of a large number of small single crystal blocks. During the charging process, as lithium ions are released, the layered structure of the ternary material undergoes a crystal phase transition from H1 to H2 and then to H3, accompanied by expansion and contraction along the c-axis, causing a certain volume change; this volume change causes anisotropic internal stress to form inside the secondary agglomerate particles, and then produces intercrystalline microcracks; as the number of cycles increases, the intercrystalline microcracks gradually become larger, and the entire secondary agglomerate particles will be crushed, so the exposed inner surface of the particles contacts the electrolyte, which will consume more lithium ions to form the positive electrode electrolyte interface film, causing the battery capacity to decay sharply; and high-voltage or high-nickel ternary materials will further aggravate the above hazards.

[0003] Rare earth element doping is often used in the prior art to inhibit local crystal phase transformation, but it cannot solve the generation of anisotropic internal stress in ternary materials, and the problem of capacity decay of ternary materials caused by particle breakage still exists; lithium phosphate-coated ternary materials have the characteristic of low water absorption, but it does not help to improve the capacity and cycle performance of ternary materials, and the common preparation method of lithium phosphate-coated ternary materials has a small amount of lithium phosphate prepared and uneven distribution, cumbersome method, high equipment requirements, which is not conducive to large-scale preparation; therefore, it is necessary to develop a lithium phosphate-coated ternary material that can simultaneously inhibit crystal phase transformation between materials, reduce stress between materials, and can be prepared on a large scale with a simple preparation method. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the prior art that the amount of lithium phosphate in the lithium phosphate-coated ternary material is small, the method is cumbersome, and the crystal phase transformation between the ternary materials leads to volume changes to form anisotropic internal stress, and the resulting intercrystalline cracks cause the capacity and cycle performance of the obtained battery to decay, thereby providing a lithium phosphate-coated ternary material and its preparation method and application.

[0005] To this end, the present invention provides the following technical solutions.

[0006] The present invention provides a lithium phosphate coated ternary material, comprising a rare earth element doped nickel-cobalt-manganese ternary material and lithium phosphate, wherein the lithium phosphate coats the rare earth element doped nickel-cobalt-manganese ternary material;

[0007] The lithium phosphate is amorphous lithium phosphate;

[0008] The rare earth element is at least one of niobium, cerium, yttrium, lanthanum and scandium.

[0009] In an optional embodiment, based on the molar amount of the rare earth element-doped nickel-cobalt-manganese ternary material, the molar amount of the lithium phosphate is 1000-3000 ppm.

[0010] In an optional embodiment, the molar ratio of the total molar amount of nickel, cobalt and manganese in the rare earth element-doped nickel-cobalt-manganese ternary material to the molar amount of the rare earth element is 1:(0.001-0.01);

[0011] Preferably, the rare earth element is at least one of niobium, cerium, lanthanum and scandium.

[0012] The present invention provides a method for preparing a lithium phosphate coated ternary material, comprising the following steps:

[0013] (1) preparing a rare earth element-doped nickel-cobalt-manganese sintered material; the rare earth element is at least one of niobium, cerium, yttrium, lanthanum and scandium;

[0014] (2) preparing lithium phosphate; the lithium phosphate is amorphous lithium phosphate;

[0015] (3) The rare earth element-doped nickel-cobalt-manganese sintering material is mixed with the lithium phosphate and then sintered.

[0016] In an optional embodiment, the molar ratio of the rare earth element doped nickel-cobalt-manganese sintering material to the lithium phosphate is 1:(0.001-0.003).

[0017] In an optional embodiment, the step (2), the step of preparing lithium phosphate comprises: placing a phosphoric acid solution in an environment of 70-95° C., adding a lithium hydroxide solution to the phosphoric acid solution while stirring, and aging;

[0018] Preferably, the concentration of the phosphoric acid solution is 0.3-0.6 mol / L;

[0019] Preferably, the aging is carried out at a pH value of 9.5-11;

[0020] Preferably, the aging time is 60-120 min.

[0021] In an optional embodiment, the lithium phosphate preparation step further includes washing and drying steps after aging;

[0022] Preferably, the washing solvent is ethanol;

[0023] Preferably, the drying temperature is 80-120°C; the drying time is 3-5h;

[0024] In an optional embodiment, the step (1), the step of preparing the rare earth element doped nickel-cobalt-manganese sintering material comprises: mixing a nickel-cobalt-manganese hydroxide precursor, a lithium source and a rare earth compound, and sintering;

[0025] Preferably, the ratio of the molar amount of lithium element in the lithium source to the total molar amount of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese hydroxide precursor is 1:(1.0-1.15);

[0026] Preferably, the ratio of the total molar amount of nickel, cobalt and manganese in the nickel-cobalt-manganese hydroxide precursor to the molar amount of the rare earth element in the rare earth compound is 1:(0.001-0.01);

[0027] Preferably, the D50 of the rare earth element doped nickel-cobalt-manganese sintering material is 3.5-4.0 μm;

[0028] Preferably, the structural formula of the nickel-cobalt-manganese hydroxide precursor is Ni x Co y Mn 1-x-y (OH)2, of which 0.5 <x<1,0<y<0.5,x+y<1;

[0029] Preferably, the lithium source is at least one of lithium carbonate, lithium hydroxide and lithium acetate;

[0030] Preferably, the specific steps of sintering include: heating to 500-700°C at a heating rate of 1-5°C / min and sintering for 4-8h, and then heating to 850-1000°C at a heating rate of 1-5°C / min and sintering for 8-12h.

[0031] In an optional embodiment, the step (3), the specific step of sintering comprises: heating to 250-650° C. at a heating rate of 2-5° C. / min and sintering for 4-6 hours;

[0032] Preferably, the temperature is increased to 350-450° C. at a heating rate of 2-5° C. / min and sintered for 4-6 hours.

[0033] In an optional embodiment, the D50 of the lithium phosphate-coated ternary material is 3.5-4.0 μm;

[0034] Preferably, the rare earth element is at least one of niobium, cerium, lanthanum and scandium.

[0035] The present invention provides an application of the lithium phosphate coated ternary material or the lithium phosphate coated ternary material prepared by the above preparation method in the battery field.

[0036] The technical solution of the present invention has the following advantages:

[0037] 1. The lithium phosphate-coated ternary material provided by the present invention specifically includes a rare earth element-doped nickel-cobalt-manganese ternary material and lithium phosphate, wherein the lithium phosphate coats the rare earth element-doped nickel-cobalt-manganese ternary material; the lithium phosphate is amorphous lithium phosphate; and the rare earth element is at least one of niobium, cerium, yttrium, lanthanum and scandium. The lithium phosphate coated ternary material overcomes the problem in the prior art that the volume change caused by the crystal phase transition between the ternary materials forms anisotropic internal stress, and the resulting intercrystalline cracks cause the capacity and cycle performance of the obtained battery to decay; specifically, the coating layer of the present invention is amorphous lithium phosphate, and the amorphous lithium phosphate has the following advantages: (1) It has the characteristics of disordered internal atomic arrangement and wide distribution, which provides a convenient shuttle channel for lithium ions and electrons, greatly accelerates the movement speed of lithium ions and electrons, and significantly improves the electronic conductivity and lithium ion migration rate of the lithium phosphate coated ternary material; (2) It also has the characteristics of high surface energy and activity, can fit tightly with the electrolyte, significantly reduce the interface resistance, and thus improve the charge transfer efficiency of the battery made of the lithium phosphate coated ternary material; (3) The amorphous lithium phosphate coating layer can also enhance the stability of the interface structure, reduce the stress concentration phenomenon inside the material, effectively inhibit the generation of cracks, and greatly improve the cycle durability and long-term stability of the lithium phosphate coated ternary material. The nickel-cobalt-manganese ternary material of the present invention is doped with rare earth elements, which have more extranuclear electrons and stronger RE-O bonds. On the one hand, the migration behavior of cations can be suppressed by electromagnetic interaction forces, thereby suppressing the local phase transition of the layered structure of the lithium phosphate-coated ternary material from H1 to H2 and then to H3; and the loss of lattice oxygen in the lithium phosphate-coated ternary material can be suppressed; on the other hand, it can serve as a "pillar" to support the layered structure to prevent it from collapsing due to expansion or contraction caused by lithium removal or lithium insertion. Through the coordination of amorphous lithium phosphate and rare earth elements, especially the coordination of amorphous lithium phosphate with niobium, cerium, lanthanum and scandium, the electrochemical performance, structural stability and conductive performance of the material can be comprehensively improved, thereby significantly improving the overall performance of the battery.

[0038] 2. The preparation method of the lithium phosphate coated ternary material provided by the present invention comprises: (1) preparing a nickel-cobalt-manganese sintered material doped with a rare earth element; the rare earth element is at least one of niobium, cerium, yttrium, lanthanum and scandium; (2) preparing lithium phosphate; the lithium phosphate is amorphous lithium phosphate; (3) mixing the rare earth element doped nickel-cobalt-manganese sintered material with the lithium phosphate and then sintering. The preparation method can produce a large amount of lithium phosphate with a simple method. The prepared lithium phosphate coated ternary material overcomes the problem in the prior art that the volume change caused by the crystal phase transition between the ternary materials forms anisotropic internal stress, and the resulting intercrystalline cracks cause the capacity and cycle performance of the prepared battery to decay. Specifically, the amorphous lithium phosphate has the following advantages: (1) It has the characteristics of disordered internal atomic arrangement and wide distribution, which provides a convenient shuttle channel for lithium ions and electrons, greatly accelerates the movement speed of lithium ions and electrons, and significantly improves the electronic conductivity and lithium ion migration rate of the prepared lithium phosphate coated ternary material; (2) It also has the characteristics of high surface energy and activity, can fit tightly with the electrolyte, significantly reduce the interface resistance, and thus improve the charge transfer efficiency of the battery prepared by the prepared lithium phosphate coated ternary material; (3) The amorphous lithium phosphate coating layer can also enhance the stability of the interface structure, reduce the stress concentration phenomenon inside the material, effectively inhibit the generation of cracks, and greatly improve the cycle durability and long-term stability of the prepared lithium phosphate coated ternary material. DETAILED DESCRIPTION

[0039] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0040] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0041] Example 1

[0042] This embodiment provides a method for preparing a lithium phosphate-coated ternary material, comprising the following steps:

[0043] (1) Preparation of amorphous lithium phosphate: 39.2 g H3PO4 was mixed with 1 L deionized water, and stirred at 85°C for 60 min to prepare a phosphoric acid solution with a concentration of 0.4 mol / L; while stirring, lithium hydroxide solution was slowly added to the phosphoric acid solution, and the pH value was adjusted to 9.5-11 for aging for 60 min to obtain a precipitate product; the precipitate product was washed with ethanol for multiple times, and the washed precipitate product was placed in an oven and dried at 110°C for 5 h to obtain amorphous lithium phosphate.

[0044] (2) Lithium carbonate, Ni 0.6 Co 0.1 Mn 0.3 (OH)2, CeO2, and Nd2O3 were mixed in a molar ratio of 0.5:1.1:0.002:0.003 under an oxygen atmosphere (oxygen flow rate of 3m 3 / h), the mixed material is placed in a box furnace and heated to 700°C at a heating rate of 5°C / min and sintered for 6h, then heated to 960°C at a heating rate of 5°C / min and sintered for 12h, and then ground at room temperature to obtain a nickel-cobalt-manganese sintered material with a median particle size D50 of 3.76μm.

[0045] (3) The nickel-cobalt-manganese sintering material and lithium phosphate were mixed at a molar ratio of 1:0.002, heated to 450°C in a box furnace at a heating rate of 5°C / min and sintered for 4 hours. The heating was stopped, and the mixture was cooled and sieved to obtain a lithium phosphate-coated ternary material with a median particle size D50 of 3.80 μm.

[0046] Example 2

[0047] This embodiment provides a method for preparing a lithium phosphate-coated ternary material, comprising the following steps:

[0048] (1) Lithium hydroxide, Ni 0.6 Co 0.1 Mn 0.3 (OH)2 and La2O3 were mixed in a molar ratio of 1:1:0.003 under an oxygen atmosphere (oxygen flow rate of 3m 3 / h), the mixed material is placed in a box furnace and heated to 500°C at a heating rate of 1°C / min and sintered for 4h, then heated to 850°C at a heating rate of 1°C / min and sintered for 8h, and then ground at room temperature to obtain a nickel-cobalt-manganese sintered material with a median particle size D50 of 3.52μm.

[0049] (2) The nickel-cobalt-manganese sintering material and lithium phosphate were mixed at a molar ratio of 1:0.002, heated to 400°C in a box furnace at a heating rate of 2°C / min and sintered for 6 hours. The heating was stopped, and the mixture was cooled and sieved to obtain a lithium phosphate-coated ternary material with a median particle size D50 of 3.55 μm.

[0050] Example 3

[0051] This embodiment provides a method for preparing a lithium phosphate-coated ternary material, comprising the following steps:

[0052] (1) Lithium acetate, Ni 0.6 Co 0.1 Mn 0.3 (OH)2, CeO2, Nd2O3 and Sc2O3 were mixed in a molar ratio of 1:1:0.003:0.0015:0.0015 under an oxygen atmosphere (oxygen flow rate of 3m 3 / h), the mixed material is placed in a box furnace and heated to 600°C at a heating rate of 3°C / min and sintered for 8h, then heated to 1000°C at a heating rate of 3°C / min and sintered for 10h, and then ground at room temperature to obtain a nickel-cobalt-manganese sintered material with a median particle size D50 of 3.95μm.

[0053] (2) The nickel-cobalt-manganese sintering material and lithium phosphate were mixed at a molar ratio of 1:0.002, heated to 450°C in a box furnace at a heating rate of 4°C / min and sintered for 5 hours. The heating was stopped, and the mixture was cooled and sieved to obtain a lithium phosphate-coated ternary material with a median particle size D50 of 3.98 μm.

[0054] Example 4

[0055] This embodiment provides a method for preparing a lithium phosphate-coated ternary material, comprising the following steps:

[0056] (1) Lithium hydroxide, Ni 0.6 Co 0.1 Mn 0.3 (OH)2 and Y2O3 were mixed in a molar ratio of 1:1:0.003 under an oxygen atmosphere (oxygen flow rate of 3m 3 / h), the mixed material is placed in a box furnace and heated to 500°C at a heating rate of 1°C / min and sintered for 4h, then heated to 850°C at a heating rate of 1°C / min and sintered for 8h, and then ground at room temperature to obtain a nickel-cobalt-manganese sintered material with a median particle size D50 of 3.55μm.

[0057] (2) The nickel-cobalt-manganese sintering material and lithium phosphate are mixed in a molar ratio of 1:0.002, heated to 350°C in a box furnace at a heating rate of 2°C / min, and sintered for 6 hours. The heating is stopped, and the mixture is cooled and sieved to obtain a lithium phosphate-coated ternary material, wherein the average particle size D50 is 3.58 μm.

[0058] Comparative Example 1

[0059] This comparative example provides a method for preparing a ternary material, which differs from Example 1 in that no rare earth element is added in step (2) when preparing the nickel-cobalt-manganese sintered material; and no lithium phosphate is added in step (3) when preparing the ternary material.

[0060] In this comparative example, not adding rare earth elements and lithium phosphate does not affect the particle size of the material, but has a greater impact on the electrical properties of the material.

[0061] Comparative Example 2

[0062] This comparative example provides a method for preparing a ternary material, which differs from Example 1 in that lithium phosphate is not added in step (3) of preparing the ternary material.

[0063] In this comparative example, not adding lithium phosphate does not affect the particle size of the material, but has a greater impact on the electrical properties of the material.

[0064] Comparative Example 3

[0065] This comparative example provides a method for preparing a ternary material, which differs from Example 1 in that no rare earth element is added in step (2) when preparing the nickel-cobalt-manganese sintered material.

[0066] In this comparative example, not adding rare earth elements does not affect the particle size of the material, but has a greater impact on the electrical properties of the material.

[0067] Test Example 1

[0068] This test example provides performance tests of lithium phosphate coated ternary materials in various embodiments and comparative ternary materials, as follows:

[0069] (1) Test method for average particle size D50 of lithium phosphate coated ternary material: The test was carried out using a particle size analyzer (Mastersizer3000+Lab, Malvern Panalytical). The results are shown in Table 1.

[0070] (2) Method for detecting the amount of lithium phosphate coating in lithium phosphate coated ternary materials:

[0071] 1) Weigh a certain amount of sample using an analytical balance;

[0072] 2) Place the weighed sample in a beaker, add appropriate amount of distilled water and heat with a magnetic stirrer until dissolved;

[0073] 3) The solution is cooled to room temperature, phenolphthalein indicator is added dropwise and stirred thoroughly to make the indicator evenly dispersed;

[0074] 4) Fill the burette with the calibrated acid titrant, record the initial reading, slowly drip the titrant (H2SO4, concentration is 0.2 mol / L) into the solution in step 3) while stirring the solution with a magnetic stirrer. When the solution suddenly changes from red to colorless and does not change within half a minute, the titration endpoint is reached, and record the endpoint reading;

[0075] 5) According to the volume and concentration of the consumed titrant, the amount of lithium phosphate coated in the lithium phosphate coated ternary material can be calculated. The reaction formula between the lithium phosphate coated ternary material and the titrant is as follows:

[0076] 2Li3PO4+3H2SO4→6LiHSO4+H3PO4

[0077] (3) Test method for rare earth element doping amount:

[0078] 1) Weigh 0.20g of sample (accurate to 0.0001g), place it in a 100mL polytetrafluoroethylene beaker, add 15mL of hydrochloric acid, 5mL of nitric acid, and about 1mL of hydrofluoric acid, cover with a watch glass, adjust the hot plate to about 150V, heat for about 20min, rinse the watch glass and the inner wall of the beaker after the sample is completely dissolved, add 2g of citric acid, place it on the hot plate and heat for about 10min, remove it, cool it slightly, transfer it to a 50mL plastic volumetric flask, dilute it to the mark with water, shake it well, and obtain the sample solution to be tested.

[0079] 2) In a 50 ml volumetric flask, 0 ml, 0.1 ml, 1 ml, 2 ml, 4 ml, 8 ml and 10 ml of a rare earth standard solution with a concentration of 10 μg / ml were added respectively, diluted to the mark with water, and shaken to obtain a series of rare earth standard working solutions with concentrations of 0 μg / ml, 0.02 μg / ml, 0.2 μg / ml, 0.4 μg / ml, 0.8 μg / ml, 1.6 μg / ml and 2.0 μg / ml, respectively. The intensity of the series of standard working solutions was detected by inductively coupled plasma atomic emission spectrometer, and a standard working curve was established with concentration as the abscissa and intensity as the ordinate. The sample solution to be tested was tested, and the concentration of the rare earth element in the sample solution to be tested was calculated according to the intensity, and then the content of the rare earth element in the ternary material was obtained, as shown in Table 1.

[0080] It should be noted that when the ternary material contains multiple rare earth elements, it is necessary to first establish standard curves for different rare earth elements and obtain the content of the corresponding rare earth elements according to the corresponding standard curves.

[0081] (4) Electrochemical properties of ternary materials:

[0082] Assemble the battery: Weigh the ternary materials (from each embodiment and each comparative example), PVDF and Super P in a mass ratio of 97.2:1.3:1.5 to prepare a positive electrode slurry, and evenly coat the slurry on an aluminum foil (surface density 15.0-17.0 mg / cm 2), dried at 80°C for 2 hours, punched, weighed, and baked to obtain a positive electrode. The LiPF6 concentration in the electrolyte was 1 mol / L, the solvent was EC and DEC in a volume ratio of 1:1, the negative electrode was a metal lithium sheet, and it was packaged into a CR2032 button battery; the battery was cycled 2 times at 0.1C for activation.

[0083] Test method:

[0084] (1) 1C specific capacity measurement: The battery was charged at 1C and discharged at 1C once. The results are shown in Table 2.

[0085] (2) Cycle test method: The battery was charged at 1C and discharged at 1C for 200 cycles, with a charge and discharge voltage range of 2.5-4.45V. The results are shown in Table 2. The capacity retention rate is calculated as follows:

[0086] Capacity retention rate = 100% × 200 th Discharge specific capacity / 1 st Discharge specific capacity

[0087] Table 1 Particle size, lithium phosphate content and rare earth element content of ternary materials

[0088]

[0089]

[0090] Note: The rare earth elements in Table 1 refer to the total amount of all rare earth elements in the ternary materials.

[0091] Table 2 Performance results of ternary materials obtained in various embodiments and comparative examples

[0092]

[0093] From Examples 1-4 and Comparative Examples 1-3, the lithium phosphate-coated ternary material prepared by the present invention is doped with rare earth elements and coated with amorphous lithium phosphate, which means that doping with rare earth elements when preparing the nickel-cobalt-manganese sintered material and coating amorphous lithium phosphate when preparing the ternary material can help improve the specific capacity and cycle performance of the lithium phosphate-coated ternary material. From the comparison between Example 2 and Example 4, when the rare earth element is at least one of niobium, cerium, lanthanum or scandium, it is more helpful to improve the electrochemical properties, structural stability and conductive properties of the lithium phosphate-coated ternary material, and optimize the specific capacity and cycle performance of the ternary material. In Comparative Example 1, no rare earth elements and lithium phosphate are added when preparing the ternary material, and the capacity retention rate of the obtained ternary material is low, 200 thThe discharge (1C) specific capacity is greatly reduced; in Comparative Example 2, no lithium phosphate is added. Without amorphous lithium phosphate, it is impossible to provide a convenient shuttle channel for lithium ions and electrons, which reduces the movement speed of lithium ions and electrons, causing the specific capacity and cycle performance of the prepared ternary material to decrease significantly; in Comparative Example 3, no rare earth elements are added, which cannot inhibit the local phase transition of the layered structure of the ternary material, causing the performance of the prepared ternary material to decrease significantly after long-term cycling, 200 th The discharge (1C) specific capacity and capacity retention rate both decreased significantly.

[0094] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A lithium phosphate coated ternary material, It is characterized in that It comprises a rare earth element doped nickel-cobalt-manganese ternary material and lithium phosphate, wherein the lithium phosphate covers the rare earth element doped nickel-cobalt-manganese ternary material; The lithium phosphate is amorphous lithium phosphate; The rare earth element is at least one of niobium, cerium, yttrium, lanthanum and scandium.

2. The lithium phosphate coated ternary material according to claim 1, It is characterized in that Based on the molar amount of the rare earth element-doped nickel-cobalt-manganese ternary material, the molar amount of the lithium phosphate is 1000-3000ppm.

3. The lithium phosphate coated ternary material according to claim 1, It is characterized in that The molar ratio of the total molar amount of nickel, cobalt and manganese in the rare earth element-doped nickel-cobalt-manganese ternary material to the molar amount of the rare earth element is 1:(0.001-0.01); Preferably, the rare earth element is at least one of niobium, cerium, lanthanum and scandium.

4. A method for preparing a lithium phosphate-coated ternary material, It is characterized in that The following steps are included: (1) preparing a rare earth element-doped nickel-cobalt-manganese sintered material; the rare earth element is at least one of niobium, cerium, yttrium, lanthanum and scandium; (2) preparing lithium phosphate; the lithium phosphate is amorphous lithium phosphate; (3) The rare earth element-doped nickel-cobalt-manganese sintering material is mixed with the lithium phosphate and then sintered.

5. The preparation method according to claim 4, It is characterized in that The molar ratio of the rare earth element doped nickel-cobalt-manganese sintering material to the lithium phosphate is 1:(0.001-0.003).

6. The preparation method according to claim 4, It is characterized in that The step (2) of preparing lithium phosphate comprises: placing a phosphoric acid solution in an environment of 70-95° C., adding a lithium hydroxide solution to the phosphoric acid solution while stirring, and aging; Preferably, the concentration of the phosphoric acid solution is 0.3-0.6 mol / L; Preferably, the aging is carried out at a pH value of 9.5-11; Preferably, the aging time is 60-120 min.

7. The preparation method according to claim 4, It is characterized in that The step (1), the preparation step of the rare earth element doped nickel-cobalt-manganese sintering material comprises: mixing a nickel-cobalt-manganese hydroxide precursor, a lithium source and a rare earth compound, and sintering; Preferably, the ratio of the molar amount of lithium element in the lithium source to the total molar amount of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese hydroxide precursor is 1:(1.0-1.15); Preferably, the ratio of the total molar amount of nickel, cobalt and manganese in the nickel-cobalt-manganese hydroxide precursor to the molar amount of the rare earth element in the rare earth compound is 1:(0.001-0.01); Preferably, the D50 of the rare earth element doped nickel-cobalt-manganese sintering material is 3.5-4.0 μm; Preferably, the structural formula of the nickel-cobalt-manganese hydroxide precursor is Ni x Co y Mn 1-x-y (OH) 2 , where 0.5 <x<1,0<y<0.5,x+y<1; Preferably, the lithium source is at least one of lithium carbonate, lithium hydroxide and lithium acetate; Preferably, the specific steps of sintering include: heating to 500-700°C at a heating rate of 1-5°C / min and sintering for 4-8h, and then heating to 850-1000°C at a heating rate of 1-5°C / min and sintering for 8-12h.

8. The preparation method according to claim 4, It is characterized in that The specific steps of sintering in step (3) include: heating to 250-650°C at a heating rate of 2-5°C / min and sintering for 4-6h; Preferably, the temperature is increased to 350-450° C. at a heating rate of 2-5° C. / min and sintered for 4-6 hours.

9. The preparation method according to claim 4, It is characterized in that The D50 of the lithium phosphate-coated ternary material is 3.5-4.0 μm; Preferably, the rare earth element is at least one of niobium, cerium, lanthanum and scandium.

10. Use of the lithium phosphate coated ternary material according to any one of claims 1 to 3 or the lithium phosphate coated ternary material prepared by the preparation method according to any one of claims 4 to 9 in the field of batteries.

Citation Information

Cited By

  • Positive electrode material and preparation method thereof, positive electrode plate and all-solid-state lithium battery