Positive electrode active material and preparation method thereof, positive electrode plate, battery and electric equipment

CN118970004APending Publication Date: 2024-11-15BEIJING EASPRING MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411048189.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

尖晶石型锰酸锂LiMn2O4是常见的锂离子电池正极活性材料之一,具有工作电压高、生产成本低、合成工艺简单、热稳定性好、倍率性能和低温性能优越等优点,然而,研究表明,LiMn2O4中的锰元素发生歧化反应溶解在电解液中以及因Jahn-Teller效应发生的晶格畸变,导致含有其的电池循环性能和容量差

Benefits of technology

[0006] According to the cathode active material according to the embodiment of the present invention, by providing a coating layer on the body of the cathode active material, the coating layer includes a continuous coating, and at least one of a dot-shaped coating and an island-shaped coating, It can better isolate the side reaction between the electrolyte and the body, improve the cycle performance of the battery containing it, and within the above thickness range, it will not affect the capacity of the positive active material. In summary, the cathode active material proposed in this application and the battery containing it have excellent capacity and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970004A_ABST
    Figure CN118970004A_ABST
Patent Text Reader

Abstract

The invention discloses a positive active material and a preparation method thereof, a positive pole piece, a battery and electric equipment, and relates to the technical field of batteries, the positive active material comprises a body and a coating layer formed on at least part of the surface of the body, the coating layer comprises a continuous coating and a second coating protruding out of the surface of the continuous coating, the second coating comprises at least one of a point-shaped coating and an island-shaped coating; the average thickness of the coating layer ranges from 0.5 nm to 5 nm, and the average thickness of the continuous coating ranges from 0.05 nm to 2 nm. Therefore, the battery containing the positive electrode active material has excellent capacity and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of batteries, and in particular relates to a positive electrode active material and a preparation method thereof, a positive electrode sheet, a battery and an electrical device. Background Art

[0002] The main components of lithium-ion batteries are electrolyte, diaphragm materials, positive electrode and negative electrode materials. Among them, the performance of the positive electrode of lithium-ion batteries directly affects the electrochemical performance of lithium-ion batteries. Spinel lithium manganese oxide LiMn2O4 is one of the common positive electrode active materials for lithium-ion batteries. It has the advantages of high operating voltage, low production cost, simple synthesis process, good thermal stability, superior rate performance and low temperature performance. However, studies have shown that the manganese element in LiMn2O4 undergoes a disproportionate reaction and dissolves in the electrolyte, as well as lattice distortion due to the Jahn-Teller effect, resulting in poor cycle performance and capacity of batteries containing it. Summary of the invention

[0003] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a positive electrode active material and a preparation method thereof, a positive electrode sheet, a battery and an electrical device, wherein the battery containing the positive electrode active material has excellent capacity and cycle performance.

[0004] In one aspect of the present invention, the present invention provides a positive electrode active material, the positive electrode active material comprises a body and a coating formed on at least a portion of the surface of the body, the coating comprises a continuous coating and a second coating protruding from the surface of the continuous coating, the second coating comprises at least one of a dot-shaped coating and an island-shaped coating;

[0005] The average thickness of the coating layer is 0.5nm-5nm, and the average thickness of the continuous coating is 0.05nm-2nm.

[0006] According to the positive electrode active material of the embodiment of the present invention, by setting a coating layer on the body of the positive electrode active material, the coating layer includes at least one of a continuous coating, a point coating and an island coating, which can better isolate the electrolyte from the body to produce side reactions, improve the cycle performance of the battery containing it, and within the above thickness range, it will not affect the capacity of the positive electrode active material. In summary, the positive electrode active material proposed in this application and the battery containing it have excellent capacity and cycle performance.

[0007] In addition, the positive electrode active material according to the above embodiment of the present invention may also have the following additional technical features:

[0008] In some embodiments of the present invention, the average thickness of the coating layer is 1 nm-2 nm.

[0009] In some embodiments of the present invention, the average thickness of the continuous coating is 0.1 nm-1 nm.

[0010] In some embodiments of the present invention, the average thickness of the second coating layer is 0.5 nm-20 nm, preferably 1 nm-10 nm.

[0011] In some embodiments of the present invention, the arithmetic mean roughness Ra of the coating layer satisfies: 0.5 nm≤Ra≤19.5 nm.

[0012] In some embodiments of the present invention, the area of ​​the second coating occupies 25%-45% of the area of ​​the coating layer.

[0013] In some embodiments of the present invention, the body comprises: LiMe y Mn 2-y O4, wherein Me includes at least one of Al, Mg, Co, Ni, Y, Nb, Zr, Ti, Sr, Ce and La, and 0≤y≤0.2.

[0014] In some embodiments of the present invention, the coating layer comprises: LiAl x Mn 2-x O4, of which 0.04 <x<0.8。

[0015] In some embodiments of the present invention, the average particle size of the positive electrode active material is 1.3 μm-8.0 μm.

[0016] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned positive electrode active material, comprising:

[0017] A manganese source, a lithium source, and an optional additive are mixed according to a stoichiometric ratio to obtain a mixed material, and the mixed material is sintered to obtain lithium manganate;

[0018] crushing the lithium manganate and mixing it with aluminum oxide to obtain a mixture;

[0019] The mixture is calcined to obtain a positive electrode active material.

[0020] Thus, the above-mentioned positive electrode active material can be prepared by this method. By setting a coating layer on the body of the positive electrode active material, the coating layer includes at least one of a continuous coating, a point coating, and an island coating, which can better isolate the electrolyte from the body to produce side reactions, improve the cycle performance of the battery containing it, and within the above-mentioned thickness range, it will not affect the capacity of the positive electrode active material. In summary, the positive electrode active material proposed in this application and the battery containing it have excellent capacity and cycle performance.

[0021] In some embodiments of the present invention, the manganese source includes at least one of trimanganese tetraoxide, manganese dioxide, manganese hydroxide, manganese carbonate and manganese phosphate.

[0022] In some embodiments of the present invention, the mass of the additive is 0.1%-6% of the manganese source.

[0023] In some embodiments of the present invention, the sintering is performed in an air atmosphere.

[0024] In some embodiments of the present invention, the sintering temperature is 850°C-1000°C.

[0025] In some embodiments of the present invention, the sintering holding time is 8h-15h.

[0026] In some embodiments of the present invention, the heating rate of the sintering is 1° C. / min-5° C. / min.

[0027] In some embodiments of the present invention, the median particle size of the lithium manganate is 5 μm-20 μm.

[0028] In some embodiments of the present invention, the mass of the aluminum oxide is 0.1%-1% of the lithium manganese oxide.

[0029] In some embodiments of the present invention, the calcination temperature is 550°C-850°C.

[0030] In some embodiments of the present invention, the calcination holding time is 6h-10h.

[0031] In some embodiments of the present invention, the heating rate during calcination is 1° C. / min-5° C. / min.

[0032] In a third aspect of the present invention, the present invention provides a positive electrode plate, comprising the positive electrode active material described in the first aspect of the present invention.

[0033] In a fourth aspect of the present invention, the present invention provides a battery, comprising the positive electrode sheet described in the third aspect of the present application, so that the battery has excellent capacity and cycle performance.

[0034] In a fifth aspect of the present invention, the present invention provides an electrical device, comprising the battery described in the fourth aspect of the present invention.

[0035] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1is a schematic diagram of measuring the ratio of the area of ​​the second coating to the area of ​​the coating layer in the embodiment of the present application;

[0037] Figure 2 This is an EDS spectrum test diagram of the positive electrode active material prepared in Example 1 of the present application;

[0038] Figure 3 This is an EDS spectrum test diagram of the positive electrode active material prepared in Comparative Example 2 of the present application;

[0039] Figure 4 It is a scanning electron microscope image of the positive electrode active material obtained in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 5 and Comparative Example 6 of the present application. DETAILED DESCRIPTION

[0040] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0041] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0042] In one aspect of the present invention, the present invention provides a positive electrode active material, which includes a main body and a coating formed on at least a portion of the surface of the main body, the coating including a continuous coating and a second coating protruding from the surface of the continuous coating, the second coating including at least one of a point-shaped coating and an island-shaped coating; the average thickness of the coating is 0.5nm-5nm, and the average thickness of the continuous coating is 0.05nm-2nm.

[0043] The average thickness of the coating layer is the average thickness of the entire coating layer, that is, the average thickness of all coatings including the continuous coating and the second coating. As an example, the average thickness of the coating layer can be 0.5nm, 1nm, 2nm, 3nm, 4nm, 5nm, etc. According to other embodiments of the present invention, the average thickness of the coating layer is 1nm-2nm.

[0044] As an example, the average thickness of the continuous coating is 0.05 nm, 0.1 nm, 0.3 nm, 0.5 nm, 0.7 nm, 0.9 nm, 1 nm, 1.5 nm, 2 nm, etc. According to some other embodiments of the present invention, the average thickness of the continuous coating is 0.1 nm-1 nm.

[0045] The inventors found that the present application controls the coating layer on the main body of the positive electrode active material layer to contain both a continuous coating and a dot-shaped / island-shaped coating. The mixed state of the continuous coating and the dot-shaped / island-shaped coating is the optimal situation. The solid solution shell formed by the coating layer can isolate the main body of the positive electrode active material from direct contact with the electrolyte, reducing the dissolution of the metal, and the coating layer doping suppresses the Jahn-Teller effect, thereby improving the capacity and cycle performance of the battery. On the other hand, the thickness of the coating layer and the continuous coating is controlled, and the coating layer includes a continuous coating and a second coating protruding from the surface of the continuous coating, so that the coating layer can isolate the electrolyte without affecting the transmission of lithium ions, ensuring that the battery has a small impedance and good cycle performance. In summary, the positive electrode active material proposed in the present application and the battery containing it have excellent cycle performance and capacity.

[0046] The embodiment of the present application uses an energy spectrum tester to test the integrated area of ​​the characteristic peak of the coating element on the surface of the positive electrode active material particles. The thickness of the coating = (integral area of ​​the characteristic peak of the coating element / integral area of ​​the characteristic peak of the standard containing the coating element) × the collection thickness of the standard; the coating element refers to the element with the highest molar content among the elements other than oxygen, lithium and manganese in the solid solution.

[0047] When measuring the average thickness of a continuous coating, only the continuous coating area is selected for signal collection; when testing the thickness of the second coating, that is, the point / island-shaped coating, only the point / island-shaped coating is selected for signal collection; when measuring the average thickness of the coating layer, the signal collection selects an area that occupies more than 60% of the projected area of ​​the single particle in the SEM, which includes the continuous coating and the point / island-shaped coating.

[0048] In the present application, the average thickness of each type of coating is calculated as (the sum of the thickness of each type of coating of n particles) / n, where n is 50.

[0049] It can be understood that a continuous coating refers to a coating with a smooth and continuous surface without obvious particles and dot-shaped / island-shaped coatings, and a dot-shaped / island-shaped coating refers to a dot-shaped and / or island-shaped coating that obviously protrudes from the surface of the coating layer.

[0050] According to an embodiment of the present invention, the average thickness of the second coating layer is 0.5nm-20nm, for example, it can be 0.5nm, 1nm, 5nm, 10nm, 15nm, 20nm, etc. The second coating layer is within the above range, which can provide a channel for lithium ion transmission, reduce the impedance of the battery, and improve the capacity and cycle performance. According to some other embodiments of the present invention, the average thickness of the second coating layer is 1nm-10nm.

[0051] According to an embodiment of the present invention, the arithmetic mean roughness Ra of the coating layer satisfies: 0.5nm≤Ra≤19.5nm. For example, it can be 0.5nm, 1nm, 5nm, 10nm, 15nm, 19.5nm, etc. By controlling the arithmetic mean roughness of the coating layer within the above range, the electrolyte can be isolated, the structural changes of the material during the charge and discharge process can be effectively alleviated, and the cycle stability of the material can be improved. According to other embodiments of the present invention, the roughness of the second coating layer is 0.5nm-9.5nm.

[0052] It can be understood that the arithmetic mean roughness refers to the result obtained by adding the absolute values ​​of the height measurements of all point-shaped / island-shaped coatings in a certain area of ​​the positive electrode active material coating layer and dividing the result by the number of measurement points.

[0053] The method for determining the surface arithmetic mean roughness of the coating layer of the positive electrode active material can be:

[0054] The arithmetic mean roughness Ra of the coating layer surface was measured using a three-dimensional scanning electron microscope (3D-SEM) according to the method of JIS B 0601 (2001).

[0055] In the embodiment of the present application, the height of the dot-shaped / island-shaped coating=the thickness of the dot-shaped / island-shaped coating-the thickness of the continuous coating.

[0056] According to an embodiment of the present invention, the area of ​​the second coating accounts for 25%-45% of the area of ​​the coating layer. For example, it can be 25%, 30%, 35%, 40%, 45%, etc. The ratio of the area of ​​the second coating to the area of ​​the coating layer is the coverage of the second coating. Specifically, the second coating mainly plays the role of isolating the electrolyte. Controlling the coverage of the second coating within the above range can ensure that the coating layer plays the role of isolating the electrolyte, and can avoid the influence of the transmission of lithium ions caused by the excessive second coating, thereby ensuring the capacity and cycle performance of the battery containing it.

[0057] The coverage of the second coating is calculated as 1 μm on the surface of a single particle under electron microscopy. 2 The total area of ​​the dot-like and / or island-like coatings in the region divided by 1 μm 2 The area of ​​the region. Figure 1For the region marked by the square box, take the average value of the regions on 50 different particles.

[0058] According to an embodiment of the present invention, the body includes: LiMe y Mn 2-y O4, wherein Me includes at least one of Al, Mg, Co, Ni, Y, Nb, Zr, Ti, Sr, Ce, and La, and 0 ≤ y ≤ 0.2. For example, y can be 0, 0.05, 0.1, 0.15, 0.2, etc. The above positive electrode active material is spinel-type lithium manganate, which has the advantages of high working voltage, low production cost, simple synthesis process, good thermal stability, excellent rate performance, and low-temperature performance. However, the disproportionation reaction of manganese element dissolved in the electrolyte and the lattice distortion caused by the Jahn-Teller effect are important factors leading to its poor cycle performance. Based on this, a coating layer is provided thereon, and the coating layer includes a continuous coating and a second coating protruding from the surface of the continuous coating, which can not only isolate the electrolyte but also avoid the influence on the transmission of lithium ions caused by excessive second coating, ensuring the capacity and cycle performance of the battery containing it.

[0059] According to an embodiment of the present invention, the coating layer includes: LiAl x Mn 2-x O4, wherein 0.04 < x < 0.8. For example, x can be 0.041, 0.1, 0.3, 0.5, 0.7, 0.79, etc. The coating layer is formed by doping aluminum into the material of the positive electrode active material layer. On the one hand, it can isolate the electrolyte, reduce the dissolution of manganese in the positive electrode active material, and does not affect the transmission of lithium ions. On the other hand, the doping of Al can inhibit the Jahn-Teller effect and improve the cycle performance of the battery.

[0060] According to an embodiment of the present invention, the average particle size of the positive electrode active material is 1.3 μm - 8.0 μm. For example, it can be 1.3 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, etc. Thus, by controlling the average particle size of the positive electrode active material within the above range, the battery containing it can have excellent cycle performance.

[0061] According to an embodiment of the present invention, when the average thickness of the second coating is too large, the overall thickness of the coating layer is too large, or the coverage rate of the second coating is too small, the coating state of the second coating is surface coating, which is in physical contact with the body, with poor contact effect and coating effect, and the coating is likely to fall off during the cycling process, resulting in poor cycle performance of the battery.

[0062] According to an embodiment of the present invention, when there is no second coating, the average thickness of the continuous coating is too large, or the coverage of the second coating is greater than 45%, the coating state is deep surface doping, and the formed solid solution will limit the Li ion transmission, resulting in poor battery cycle performance and increased DCR.

[0063] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned positive electrode active material. According to an embodiment of the present invention, the method comprises:

[0064] S100: mixing a manganese source, a lithium source and optional additives according to a stoichiometric ratio to obtain a mixed material, and sintering the mixed material to obtain lithium manganate.

[0065] According to an embodiment of the present invention, the manganese source, lithium source and additives may be commercially available products.

[0066] As an example, the manganese source includes one or more of manganese tetraoxide, manganese dioxide, manganese hydroxide, manganese carbonate, and manganese phosphate.

[0067] The lithium source includes one or more of lithium carbonate, lithium hydroxide, lithium nitrate and lithium acetate.

[0068] According to an embodiment of the present invention, the manganese source D 50 The particle size is 2.5 μm to 15.0 μm, for example, it can be 2.5 μm, 3 μm, 5 μm, 7 μm, 9 μm, 15 μm, etc. Specifically, the D of the manganese source is 50 When the particle size is controlled within the above range, lithium manganese oxide of suitable particle size can be obtained, and then when the coating layer is prepared, a uniform coating layer with suitable thickness is prepared on the surface of the lithium manganese oxide, thereby improving the capacity and stability of the positive electrode active material, thereby improving the capacity and cycle performance of the battery containing it.

[0069] According to an embodiment of the present invention, the manganese source and the lithium source are mixed according to a molar ratio of manganese element to lithium element of 2: (1.041.20), for example, it can be 2:1.04, 2:1.05, 2:1.1, 2:1.15, 2:1.2, etc., and the molar ratio of manganese element to lithium element is controlled within the above range, so that a lithium manganate material with stable structure and high capacity can be synthesized.

[0070] According to an embodiment of the present invention, the additive includes at least one of aluminum oxide, yttrium oxide, niobium oxide, zirconium oxide, titanium oxide, cerium oxide, magnesium oxide, lanthanum oxide and lithium fluoride. The above additives can significantly improve the electrochemical performance indicators of the positive electrode material, such as specific capacity, specific energy, charge and discharge efficiency, median voltage, average voltage, discharge platform capacity ratio, cycle capacity retention rate and cycle life.

[0071] It can be understood that when the additive is added, the obtained lithium manganese oxide is lithium manganese oxide containing the corresponding doping element.

[0072] According to an embodiment of the present invention, the mass of the additive is 0.1%-6% of the manganese source, for example, it can be 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, etc., and the capacity and cycle performance of the battery containing it can be improved by controlling the amount of the additive within the above range.

[0073] According to an embodiment of the present invention, the sintering is performed in an air atmosphere.

[0074] According to an embodiment of the present invention, the sintering temperature is 850°C-1000°C, for example, 850°C, 900°C, 950°C, 1000°C, etc. By controlling the sintering temperature within the above range, lithium manganese oxide with a suitable particle size can be obtained, and then when the coating layer is prepared, a uniform coating layer with a suitable thickness is prepared on the surface of the lithium manganese oxide, thereby improving the capacity and stability of the positive electrode active material, thereby improving the capacity and cycle performance of the battery containing the positive electrode active material.

[0075] According to an embodiment of the present invention, the sintering holding time is 8h-15h. For example, it can be 8h, 10h, 12h, 14h, 15h, etc. By controlling the sintering holding time within the above range, lithium manganese oxide with a suitable particle size can be obtained, and then when the coating layer is prepared, a uniform coating layer with a suitable thickness is prepared on the surface of the lithium manganese oxide, thereby improving the capacity and stability of the positive electrode active material, thereby improving the capacity and cycle performance of the battery containing it.

[0076] According to an embodiment of the present invention, the heating rate of the sintering is 1°C / min-5°C / min. For example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, etc. By controlling the heating rate of the sintering within the above range, lithium manganese oxide with a suitable particle size can be obtained, and then when the coating layer is prepared, a uniform coating layer with a suitable thickness is prepared on the surface of the lithium manganese oxide, thereby improving the capacity and stability of the positive electrode active material, thereby improving the capacity and cycle performance of the battery containing it.

[0077] According to an embodiment of the present invention, the median particle size of the lithium manganate is 5 μm-20 μm. For example, it can be 5 μm, 10 μm, 15 μm, 20 μm, etc. The median particle size of the lithium manganate is controlled within the above range. When the coating layer is prepared, a uniform coating layer with a suitable thickness is prepared on the surface of the lithium manganate, which improves the capacity and stability of the positive electrode active material, thereby improving the capacity and cycle performance of the battery containing it.

[0078] According to an embodiment of the present invention, after the prepared lithium manganese oxide is naturally cooled, the lithium manganese oxide is crushed and sieved;

[0079] Preferably, the lithium manganese oxide precursor after the primary sintering is crushed by a mechanical crusher, a colloid mill or a jet mill to obtain a product with a particle size of 512 microns, and a 400-mesh screen is used for primary screening.

[0080] S200: The lithium manganate is crushed and mixed with aluminum oxide to obtain a mixture.

[0081] According to an embodiment of the present invention, the mass of the aluminum oxide is 0.1%-1% of the lithium manganese oxide, for example, it can be 0.1%, 0.3%, 0.5%, 0.7%, 0.9%, 1%, etc. The amount of aluminum oxide added is controlled within the above range, and the surface of the single-crystal lithium manganese oxide positive electrode active material can be coated with aluminum oxide, and partial surface doping can be achieved by controlling the coating dosage and the secondary sintering system, limiting the coating state, thickness and coverage of the solid solution layer, avoiding direct contact between the lithium manganese oxide positive electrode material and the electrolyte, and improving the battery cycle performance; this core-shell structure can also improve resistance, improve the cycle performance of the material, etc.

[0082] S300: calcining the mixture to obtain a positive electrode active material.

[0083] According to an embodiment of the present invention, the calcination temperature is 550°C-850°C, for example, the calcination temperature can be 550°C, 600°C, 700°C, 750°C, 800°C, 850°C, etc.; thereby, by making the calcination temperature within the above range, partial surface doping of aluminum oxide can be achieved at high temperature, and the coating state (continuous coating and second coating), thickness and coverage of the solid solution coating layer can be controlled within the required range, which can avoid direct contact between the lithium manganese oxide positive electrode material and the electrolyte, thereby improving the battery cycle performance; this core-shell structure can also improve resistance, improve the cycle performance of the material, etc.

[0084] According to an embodiment of the present invention, the holding time of the calcination is 6h-10h, for example, it can be 6h, 7h, 8h, 9h, 10h, etc., and the holding time of the calcination is controlled within the above range, so that the aluminum oxide can be partially surface doped at high temperature, and the coating state (continuous coating and second coating), thickness and coverage of the solid solution coating layer can be further controlled within the required range, which can avoid direct contact between the lithium manganese oxide positive electrode material and the electrolyte, and improve the battery cycle performance; this core-shell structure can also improve resistance, improve the cycle performance of the material, etc.

[0085] According to an embodiment of the present invention, the heating rate during calcination is 1°C / min-5°C / min. For example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, etc. By controlling the heating rate of calcination within the above range, partial surface doping of aluminum oxide can be achieved at high temperature, and the coating state (continuous coating and second coating), thickness and coverage of the solid solution coating layer can be further controlled within the required range, which can avoid direct contact between the lithium manganese oxide positive electrode material and the electrolyte, and improve the battery cycle performance; this core-shell structure can also improve resistance, improve the cycle performance of the material, etc.

[0086] In summary, the positive electrode active material obtained by the above method forms a solid solution layer by doping Al on the surface of lithium manganese oxide. This solid solution shell can isolate the direct contact between the lithium manganese oxide positive electrode material and the electrolyte, reduce the dissolution of manganese, and Al doping can inhibit the Jahn-Teller effect and improve the cycle performance of the battery.

[0087] The present invention regulates the coating state, thickness and coverage of the solid solution layer by controlling the secondary calcination and the coating amount of Al2O3, thereby ensuring good electrical performance indicators in the final output product.

[0088] The method for preparing the core-shell structure lithium manganate positive electrode material provided by the present invention has a simple and controllable process, low production cost, and can realize large-scale production.

[0089] In a third aspect of the present invention, the present invention provides a positive electrode sheet. According to an embodiment of the present invention, the positive electrode sheet comprises the positive electrode active material described in the first aspect of the present invention, or the positive electrode active material prepared by the method described in the second aspect.

[0090] According to an embodiment of the present invention, the positive electrode plate includes a positive electrode collector and a positive electrode active material layer arranged on the positive electrode collector, the positive electrode active material layer includes the above-mentioned positive electrode active material, wherein the positive electrode collector can be a metal foil or a composite current collector (the metal material can be arranged on a polymer substrate to form a composite current collector), for example, the positive electrode collector can be aluminum foil.

[0091] According to some embodiments of the present invention, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, or fluorine-containing acrylate resin.

[0092] According to some embodiments of the present invention, the positive electrode active material layer may further optionally include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene or carbon nanofibers.

[0093] According to some embodiments of the present invention, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0094] It should be noted that the features and advantages described above for the positive electrode active material and the preparation method thereof are also applicable to the positive electrode plate and will not be described in detail here.

[0095] In a fourth aspect of the present invention, the present invention provides a battery. According to an embodiment of the present invention, the battery comprises at least one of the positive electrode sheets described in the third aspect.

[0096] As an example, a battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator, and the separator is located between the positive electrode sheet and the negative electrode sheet. During the charge and discharge process of the battery, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0097] According to an embodiment of the present invention, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer arranged on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, wherein the negative electrode current collector can be a metal foil or a composite current collector (the metal material can be arranged on a polymer substrate to form a composite current collector), for example, the positive electrode current collector can be a copper foil.

[0098] According to some embodiments of the present invention, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, sodium titanate, etc.

[0099] According to some embodiments of the present invention, the negative electrode active material layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, or carbon nanofibers.

[0100] According to some embodiments of the present invention, the negative electrode active material layer may further optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0101] According to some embodiments of the present invention, the negative electrode sheet can be prepared in the following manner: the above-mentioned components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, and the binder are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0102] According to some further embodiments of the present invention, the negative electrode plate may include a metal sodium plate or a sodium alloy, such as a sodium-indium alloy.

[0103] According to some other embodiments of the present invention, there is no particular restriction on the type of the isolation membrane, and any known porous structure isolation membrane with good chemical stability and mechanical stability can be selected. As an example, the material of the isolation membrane may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene or polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film without particular restriction. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different without particular restriction.

[0104] According to some other embodiments of the present invention, the type of electrolyte is not specifically limited and can be selected according to needs. For example, the electrolyte can be in a gel state or a fully solid state. According to some specific embodiments of the present invention, the electrolyte is an electrolyte solution, and the electrolyte solution includes a sodium salt and a solvent.

[0105] According to some specific embodiments of the present invention, the sodium salt may include at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethylsulfonate or sodium bis(trifluoromethylsulfonyl)imide.

[0106] According to some specific embodiments of the present invention, the solvent may include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, ethylene glycol dimethyl ether, methyl ethyl sulfone or diethyl sulfone.

[0107] In some embodiments of the present application, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0108] It should be noted that the above-mentioned features and advantages described for the positive electrode plate are also applicable to the solid-state battery and will not be repeated here.

[0109] In a fifth aspect of the present invention, the present invention provides an electric device. According to an embodiment of the present invention, the electric device includes the above-mentioned battery. According to an embodiment of the present invention, the electric device may include but is not limited to a mobile phone, a laptop computer, an electric vehicle, etc.

[0110] It should be noted that the features and advantages described above for the battery are also applicable to the electrical device and will not be repeated here.

[0111] Below, the embodiment of the present invention is described. The embodiment described below is exemplary, is only used to explain the present invention, and cannot be interpreted as limiting the present invention. If no specific technology or conditions are indicated in the embodiment, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments is not indicated, they are all conventional products that can be obtained commercially.

[0112] Example 1

[0113] (1) Lithium carbonate and manganese tetraoxide are mixed in a high-speed mixer at a molar ratio of manganese to lithium of 2:1.06, calcined at 930° C. in an air atmosphere for 16 h, cooled, crushed and sieved to obtain a lithium manganate core.

[0114] (2) The lithium manganate core and aluminum oxide were mixed in a mass ratio of 1:0.2%, and calcined at 700°C in an air atmosphere for 10 hours to obtain LiAl x Mn 2-x Lithium manganate positive electrode active material coated with O4 solid solution coating layer.

[0115] The solid solution coating includes continuous coating and dot / island coating. The average thickness of the dot / island coating is 5.62nm, the average thickness of the continuous coating is 0.75nm, the average thickness of the overall coating is 1.33nm, the surface roughness Ra is 4.87nm, and the coverage of the dot and / or island coating is 30.6%.

[0116] Example 2

[0117] The steps are basically the same as those in Example 1, except that in step (2), the lithium manganate precursor core and aluminum oxide are mixed in a mass ratio of 1:0.5% to obtain a positive electrode active material.

[0118] The solid solution coating includes continuous coating and point / island coating. The average thickness of the point / island coating is 5.97nm, the average thickness of the continuous coating is 1.32nm, the average thickness of the overall coating is 2.49nm, the surface roughness Ra is 5.65nm, and the coverage of the point / island coating is 54.8%.

[0119] Example 3

[0120] The steps are basically the same as those in Example 1, except that in step (2), the LiAl2O3 is calcined at 700°C in an air atmosphere for 15 h to obtain the LiAl2O3 x Mn 2-x Lithium manganate positive electrode active material coated with O4 solid solution coating layer.

[0121] The solid solution coating includes continuous coating and point / island coating. The average thickness of the point / island coating is 5.19nm, the average thickness of the continuous coating is 1.18nm, the average thickness of the overall coating is 1.51nm, the surface roughness Ra is 4.01nm, and the coverage of the point and / or island coating is 36.1%.

[0122] Example 4

[0123] The steps are basically the same as those in Example 1, except that in step (2), the LiAl2O3 is calcined at 700°C in an air atmosphere for 5 hours to obtain the LiAl2O3 x Mn 2-x Lithium manganate positive electrode active material coated with O4 solid solution coating layer.

[0124] The solid solution coating includes continuous coating and dot / island coating. The average thickness of the dot / island coating is 12.8nm, the average thickness of the continuous coating is 0.56nm, the average thickness of the overall coating is 1.84nm, the surface roughness Ra is 12.24nm, and the coverage of the dot and / or island coating is 25.6%.

[0125] Example 5

[0126] The steps are basically the same as those in Example 1, except that in step (2), the LiAl2O3 is calcined at 700°C in an air atmosphere for 3 h to obtain the LiAl2O3 x Mn 2-x Lithium manganate positive electrode active material coated with O4 solid solution coating layer.

[0127] The solid solution coating includes continuous coating and point / island coating. The average thickness of the point / island coating is 15.0nm, the average thickness of the continuous coating is 0.23nm, the average thickness of the overall coating is 1.76nm, the surface roughness Ra is 14.77nm, and the coverage of the point and / or island coating is 17.4%.

[0128] Comparative Example 1

[0129] The steps are basically the same as those in Example 1, except that the calcination temperature in step (2) is 530° C. to obtain a positive electrode active material.

[0130] The solid solution coating layer has a dot-shaped coating morphology, the average thickness of the dot-shaped coating is 37.4 nm, the average thickness of the overall coating is 5.46 nm, the surface roughness Ra is 36.82 nm, and the coverage of the dot-shaped coating is 15.8%.

[0131] Comparative Example 2

[0132] The steps are basically the same as those in Example 1, except that the calcination temperature in step (2) is 880° C. to obtain a positive electrode active material.

[0133] The solid solution coating layer has a continuous coating morphology, the average thickness of the continuous coating is 3.03 nm, the average thickness of the overall coating is 3.76 nm, and the surface roughness Ra is 2.10 nm.

[0134] Comparative Example 3

[0135] The steps are basically the same as those in Example 1, except that in step (2), the lithium manganate precursor core and aluminum oxide are mixed in a mass ratio of 1:0.05% to obtain a positive electrode active material.

[0136] The solid solution coating includes continuous coating and dot / island coating. The average thickness of the dot / island coating is 4.89nm, the average thickness of the continuous coating is 0.25nm, the average thickness of the overall coating is 0.83nm, the surface roughness Ra is 4.64nm, and the coverage of the dot and / or island coating is 19.3%.

[0137] Comparative Example 4

[0138] The steps are basically the same as those in Example 1, except that in step (2), the lithium manganate precursor core and aluminum oxide are mixed in a mass ratio of 1:2% to obtain a positive electrode active material.

[0139] The solid solution coating includes continuous coating and point / island coating. The average thickness of the point / island coating is 6.35nm, the average thickness of the continuous coating is 2.37nm, the average thickness of the overall coating is 3.98nm, the surface roughness Ra is 3.98nm, and the coverage of the point and / or island coating is 78.3%.

[0140] Comparative Example 5

[0141] The steps are basically the same as those in Example 1, except that step (2) is not performed to obtain a positive electrode active material.

[0142] Comparative Example 6

[0143] The steps are basically the same as those in Example 1, except that the aluminum oxide in step (2) is replaced by titanium oxide to obtain a positive electrode active material.

[0144] The performance parameters of the positive electrode active materials prepared in the above examples and comparative examples are specifically shown in Table 1.

[0145] Table 1

[0146]

[0147] (1) Perform EDS spectrum test on the cross section of the core-shell structure lithium manganese oxide positive electrode material of Example 1 and Comparative Example 2, and obtain Figure 2 and Figure 3 ,Depend on Figure 2 It can be seen that in Example 1, the aluminum content on the surface of the positive electrode active material particles is high, while the aluminum content inside is low, which proves that Al is enriched to form LiAl x Mn 2-x O4 solid solution. Figure 3 It can be seen that in Comparative Example 2, the aluminum content inside the positive electrode active material is higher than that on the surface, which proves that Al has entered the interior of the lithium manganese oxide.

[0148] (2) Scanning electron microscopy images of the positive electrode active materials obtained in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 5 and Comparative Example 6 were taken to obtain Figure 4 , Figure 4 In the figure, (A) is a scanning electron microscope image of the positive electrode active material of Example 1, (B) is a scanning electron microscope image of the positive electrode active material of Comparative Example 1, (C) is a scanning electron microscope image of the positive electrode active material of Comparative Example 2, (D) is a scanning electron microscope image of the positive electrode active material of Comparative Example 5, and (E) is a scanning electron microscope image of the positive electrode active material of Comparative Example 6. It can be seen that in Example 1, at a calcination temperature of 700°C, Al forms LiAl on the particle surface. x Mn 2-xO4 solid solution is surface doped, containing a continuous coating and a second coating, and the second coating has an island-like morphology; in comparative example 1, when the calcination temperature is 530°C, Al exists on the surface in the form of particles, showing a point-like morphology; in comparative example 2, when the calcination temperature is 880°C, Al diffuses into the interior of the particles, which is a doped morphology and presents a continuous layer morphology, comparative example 5 is lithium manganate and does not contain any coating layer; comparative example 6 also basically does not form a coating layer.

[0149] (3) The 0.1C discharge capacity, 50-cycle capacity retention rate at room temperature, DCR impedance before cycle, and DCR impedance after cycle of the embodiment and the comparative example were measured to obtain Table 2.

[0153] 0.1C discharge capacity measurement: Shenzhen Xinweier battery testing system was used to test the electrochemical performance of CR2032 button batteries. The button voltage window was 3.0-4.3V, the nominal specific capacity was 110mAh / g, and the battery was fully charged and fully discharged at 0.1C constant current and constant voltage. The 0.1C first week discharge specific capacity C0 was recorded.

[0154] Determination of capacity retention rate at room temperature for 80 weeks: The electrochemical performance of CR2032 button batteries was tested using Shenzhen Xinweier battery testing system. The button voltage window was 3.0-4.3V, the nominal specific capacity was 110mAh / g, and the battery was fully charged at 0.1C constant current and constant voltage and then fully discharged for two cycles. After 2 cycles at 0.1C, the battery was fully charged at 1C constant current and constant voltage and then fully discharged. The first-cycle discharge specific capacity C1 was recorded, and the discharge specific capacity C80 was recorded after 80 cycles. The capacity retention rate was calculated by C80 / C1×100%, and the room-temperature cycle performance was evaluated by the capacity retention rate.

[0155] Determination of DCR impedance before and after cycling: Before the battery is cycled at high temperature, the impedance at 50% SOC is tested after it is fully charged, which is the initial impedance; after the battery is tested at high temperature cycling, the impedance at 50% SOC is tested again after it is fully charged, which is the final impedance, and the impedance growth rate, % = (final impedance - initial impedance) / initial impedance × 100%.

[0156] Table 2

[0157]

[0158] It can be seen from Table 2 that the lithium ion battery prepared using the core-shell structure lithium manganese oxide positive electrode active material prepared in the embodiment of the present invention has a high initial charge and discharge capacity and capacity retention rate, and has a lower DCR impedance.

[0159] From Table 1 and Table 2, compared with Example 1, in Example 2, the amount of aluminum oxide added as the coating agent is increased, so that the continuous coating is thickened, the coverage of the dot / island coating is increased, the overall coating layer is thickened, and the cycle performance of the battery containing it is improved. However, due to the thickening of the coating layer, the capacity of the battery is reduced and the impedance is increased; in Example 3, the calcination and heat preservation time in step (2) is extended, so that the continuous coating becomes thicker and is not within the preferred range, the impedance of the battery increases, and the cycle performance deteriorates; in Example 4, the calcination and heat preservation time in step (2) is shortened, so that the dot / island coating The average thickness becomes larger and is not in the preferred range, the cycle performance of the battery is reduced, and the impedance is significantly increased. This is because the surface substrate is exposed more, and side reactions occur with the electrolyte during the cycle, affecting the performance; in Example 5 step (2), the roasting and heat preservation time is further shortened, the average thickness of the point / island-shaped coating becomes larger, and the coverage rate of the point / island-shaped coating decreases, both of which are not in the preferred range, resulting in reduced capacity and cycle performance of the battery containing it, and further increased impedance. This is because the second coating is easy to fall off during the cycle, resulting in a weakened effect of isolating the electrolyte and poor cycle performance.

[0160] From Table 1 and Table 2, compared with Example 1, the calcination temperature of Comparative Example 1 is too low, there is no continuous coating, the capacity of the battery is reduced, and the impedance is increased. This is because the second coating is not tightly connected to the substrate and falls off during the cycle, resulting in reduced cycle performance; the calcination temperature of Comparative Example 2 is too high, there is no point-shaped / island-shaped coating, the capacity and cycle performance of the battery are reduced, and the impedance growth rate before and after the cycle is high. This is because the overly thick coating layer affects the lithium ion transmission, causing the impedance to increase and the cycle performance to deteriorate; in Comparative Example 3, the amount of aluminum oxide added is too little, making the coating layer too thin, and the cycle performance of the battery is significantly reduced, indicating that The isolation effect of the coating layer electrolyte is not enough; in Comparative Example 4, too much aluminum oxide is added, which makes the coating layer, especially the continuous coating, too thick, resulting in a decrease in the capacity of the battery containing it, and the coating layer is too thick, which significantly increases the battery impedance; Comparative Example 5 does not add aluminum oxide, and no coating layer is formed. The metal element manganese in the positive electrode active material has obvious side reactions with the electrolyte, resulting in the deterioration of the cycle performance of the battery containing it and an increase in impedance; Comparative Example 6 replaces aluminum oxide with titanium oxide. Under the above preparation conditions, a solid solution coating layer cannot be formed, resulting in a decrease in the capacity and cycle performance of the battery containing it, and an increase in impedance.

[0161] In summary, it can be seen from the above results that the lithium-ion battery prepared using the core-shell structure lithium manganese oxide positive electrode active material prepared in the embodiment of the present invention has a high initial charge and discharge capacity and capacity retention rate, and has a lower DCR impedance. More importantly, the positive electrode active material in the embodiment of the present invention has improved high temperature cycle performance.

[0162] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0163] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A positive electrode active material, characterized in that: The positive electrode active material comprises a body and a coating formed on at least a portion of the surface of the body, the coating comprising a continuous coating and a second coating protruding from the surface of the continuous coating, the second coating comprising at least one of a dot-shaped coating and an island-shaped coating; The average thickness of the coating layer is 0.5nm-5nm, and the average thickness of the continuous coating is 0.05nm-2nm.

2. The positive electrode active material according to claim 1, characterized in that The average thickness of the coating layer is 1nm-2nm; Optionally, the average thickness of the continuous coating is 0.1 nm-1 nm; Optionally, the average thickness of the second coating layer is 0.5 nm-20 nm, preferably 1 nm-10 nm.

3. The positive electrode active material according to claim 1 or 2, characterized in that: The arithmetic average roughness Ra of the coating layer satisfies: 0.5nm≤Ra≤19.5nm; Optionally, the area of ​​the second coating occupies 25%-45% of the area of ​​the coating layer.

4. The positive electrode active material according to claim 1 or 2, characterized in that: The main body includes: LiMe y Mn 2-y O4, wherein Me includes at least one of Al, Mg, Co, Ni, Y, Nb, Zr, Ti, Sr, Ce and La, and 0≤y≤0.2; Optionally, the coating layer comprises: LiAl x Mn 2-x O4, of which 0.04 <x<0.8。 5. The positive electrode active material according to claim 1 or 2, characterized in that: The average particle size of the positive electrode active material is 1.3 μm-8.0 μm.

6. A method for preparing the positive electrode active material according to any one of claims 1 to 5, characterized in that: include: A manganese source, a lithium source, and an optional additive are mixed according to a stoichiometric ratio to obtain a mixed material, and the mixed material is sintered to obtain lithium manganate; crushing the lithium manganate and mixing it with aluminum oxide to obtain a mixture; The mixture is calcined to obtain a positive electrode active material.

7. The method according to claim 6, characterized in that The manganese source includes at least one of manganese tetraoxide, manganese dioxide, manganese hydroxide, manganese carbonate and manganese phosphate; Optionally, the mass of the additive is 0.1%-6% of the manganese source; Optionally, the sintering is performed in an air atmosphere; Optionally, the sintering temperature is 850°C-1000°C; Optionally, the sintering holding time is 8h-15h; Optionally, the heating rate of the sintering is 1°C / min-5°C / min; Optionally, the lithium manganate has a median particle size of 5 μm to 20 μm.

8. The method according to claim 6, characterized in that The mass of the aluminum oxide is 0.1%-1% of the lithium manganate; Optionally, the calcination temperature is 550°C-850°C; Optionally, the calcination holding time is 6h-10h; Optionally, the heating rate during the calcination is 1°C / min-5°C / min.

9. A positive electrode sheet, characterized in that: The invention comprises the positive electrode active material according to any one of claims 1 to 5.

10. A battery, characterized in that: Including the positive electrode sheet as described in claim 9.

11. An electrical device, characterized in that: Comprising the battery as claimed in claim 10.

Citation Information

Cited By

  • Single-crystal positive electrode active material and preparation method and application thereof

    CN120727787A