Preparation method and application of polymer composite solid electrolyte with multilayer heterostructure
By adopting polymer composite solid electrolyte with multi-layer heterostructure in lithium-ion batteries, the problems of poor safety and low energy density of liquid electrolytes in lithium-ion batteries are solved, and higher electrochemical stability and safety performance are achieved.
Patent Information
- Application Number
- CN202411292275.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
AI Technical Summary
The liquid electrolytes in existing lithium-ion batteries have problems of poor safety and low energy density, especially the solid electrolyte is unstable under the strong oxidation potential of the positive electrode and the strong reduction potential of the negative electrode, resulting in poor interface contact and irreversible electrochemical reactions, which affects the Battery capacity and life.
Using a multi-layer heterostructure polymer composite solid electrolyte, a multi-layer polymer electrolyte layer is formed on the electrode sheet by spin coating to ensure high lithium ion conductivity and reduce interface impedance. Different lithium salts and active fillers are used to adapt to the electrode potential. Improve electrochemical stability and mechanical strength.
It improves the interface contact performance and electrochemical stability between the electrode sheet and the solid electrolyte, improves the rate performance, cycle performance and safety performance of lithium-ion batteries, and is suitable for industrial production.
Smart Images

Figure CN118970169A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a preparation method and application of a multi-layer heterogeneous polymer composite solid electrolyte. Background Art
[0002] Lithium-ion batteries are widely used in technology fields such as consumer electronics, electric vehicles, and energy storage power stations. Existing lithium-ion batteries mostly use liquid electrolytes, which achieve lithium ion transmission by dissolving lithium salts in flammable organic solvents such as carbonates. Liquid electrolyte batteries are prone to safety issues such as bulging and leakage during use, and have high requirements for the battery system structure, so they have the disadvantages of poor safety and low energy density.
[0003] Solid-state batteries are an important direction for the development of lithium-ion batteries. For safety and energy density issues, the use of solid electrolytes is a good solution. On the one hand, solid electrolytes can replace electrolytes and diaphragms, adapt to high-energy-density lithium metal negative electrodes, and improve energy density. On the other hand, most solid electrolytes are not easy to burn and can achieve intrinsic safety. However, there are many technical problems that have not been solved, which restrict the application of solid electrolytes. One of the main problems is poor interface contact. Solid electrolytes and electrode sheets are usually in solid-solid two-phase contact, which inevitably produces areas such as holes or faults, which easily cause dendrites, dead lithium and reduce the uniformity of the interface. Another important problem is that it is difficult to keep solid electrolytes stable at both the strong oxidation potential of the positive electrode and the strong reduction potential of the negative electrode. This will inevitably cause irreversible electrochemical reactions at the electrode interface, consuming lithium salts and solvents (plasticizers or lithium salt complexes, etc.). These problems seriously affect the capacity and life of the battery. Therefore, how to solve the interface contact and electrochemical compatibility problems between electrodes and solid electrolytes has become an important research direction in the field of solid-state battery electrolytes. Summary of the invention
[0004] In view of the deficiencies of the prior art, an object of the present invention is to provide a polymer composite solid electrolyte with a multilayer heterogeneous structure.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned multi-layer heterostructured polymer composite solid electrolyte, which coats the electrolyte solution on the electrode sheet by regulating spin coating to ensure close fit between the interface of the electrolyte solution and the electrode sheet and high interfacial lithium ion conductivity, and according to the viscosity and fluidity of different types of electrolyte solutions, electrolyte solutions of different components and different numbers of layers are coated between the positive electrode sheet and the negative electrode sheet.
[0006] Another object of the present invention is to provide the application of the above-mentioned multilayer heterostructured polymer composite solid electrolyte in a solid-state lithium-ion battery. The polymer composite solid electrolyte improves its contact performance and electrochemical stability with the electrode sheet interface and has a certain mechanical strength. As a solid electrolyte in a solid-state lithium-ion battery, it can replace the electrolyte and the diaphragm in the lithium-ion battery system, while obtaining excellent rate performance, cycle performance and safety performance.
[0007] The purpose of the present invention is achieved through the following technical solutions.
[0008] A multi-layer heterogeneous polymer composite solid electrolyte, which is a layered structure composed of multiple polymer electrolyte layers, each of which is obtained by spin coating an electrolyte solution, wherein the electrolyte solution comprises: a polymer, a lithium salt and an active filler, wherein, by weight, the ratio of the polymer, the lithium salt and the active filler is (1-10): (1-16): 1, the polymer is a mixture of one or more of polyvinylidene fluoride (PVDF), polymethyl methacrylate (PMMA), polyethylene oxide (PEO) and polyacrylonitrile (PAN), and the lithium salt is lithium perchlorate (LiClO 4 ), lithium bis(trifluoromethanesulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium hexafluorophosphate (LiPF 6 ), lithium difluorophosphate (LiPO 2 F 2 ), lithium difluorooxalatophosphate (LiODFP) and lithium difluorooxalatoborate (LiODFB), wherein the active filler is lithium lanthanum zirconium oxide (LLZO, LLZTO), lithium lanthanum titanate (LLTO), lithium aluminum titanium phosphate (LATP), lithium aluminum germanium phosphate (LAGP), lithium germanium phosphorus sulfur (LGPS), silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) or a mixture of one or more thereof.
[0009] In the above technical solution, the lithium lanthanum titanium oxide (LLTO) comprises: Li 0.5 La 0.5 TiO3, the lithium aluminum titanium phosphate (LATP) comprises: Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 The lithium aluminum germanium phosphate (LAGP) comprises: Li 1.5 Al 0.5 Ge 1.5 (PO 4 ) 3The lithium germanium phosphorus sulfur (LGPS) comprises: Li 10 G 2 S 12 .
[0010] In the above technical solution, the polymer electrolyte layer in the polymer composite solid electrolyte for contacting the positive electrode plate is layer A, the polymer in layer A is preferably a mixture of one or more of polyvinylidene fluoride (PVDF), polymethyl methacrylate (PMMA) and polyacrylonitrile (PAN), the lithium salt in layer A is preferably lithium bistrifluoromethanesulfonyl imide (LiTFSI), and the active filler in layer A is preferably lithium lanthanum titanate (LLTO), lithium aluminum titanium phosphate (LATP) and aluminum oxide (Al 2 O 3 ) or a mixture of one or more of the following: the polymer electrolyte layer in the polymer composite solid electrolyte for contacting the negative electrode plate is layer B, the polymer in layer B is preferably a mixture of one or more of polyethylene oxide (PEO) and polyacrylonitrile (PAN), and the lithium salt in layer B is preferably lithium perchlorate (LiClO 4 ), the active filler in layer B is preferably lithium lanthanum titanate (LLTO), silicon dioxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) or a mixture of one or more thereof.
[0011] In the above technical solution, when the number of polymer electrolyte layers in the polymer composite solid electrolyte is greater than or equal to 3, the polymer electrolyte layer between layer A and layer B is layer C, and layer C is at least one polymer electrolyte layer.
[0012] In the above technical solution, the polymer in the C layer is preferably a mixture of one or more of polyoxyethylene (PEO) and polyacrylonitrile (PAN), and the lithium salt in the C layer is preferably lithium perchlorate (LiClO 4 ) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and the active filler in the C layer is preferably lithium lanthanum titanate (LLTO).
[0013] In the above technical solution, the electrolyte solution further comprises: a solvent, which is a mixture of one or more of acetonitrile, acetone, N-methylpyrrolidone, N,N-dimethylformamide (DMF) and tetrahydrofuran.
[0014] In the above technical solution, the ratio of the volume fraction of the solvent to the mass fraction of the polymer is (5-20):1, the unit of the volume fraction is mL, and the unit of the mass fraction is g.
[0015] In the above technical solution, the method for preparing the electrolyte solution comprises: mixing a polymer, a lithium salt and an active filler in a solvent to obtain an electrolyte solution.
[0016] In the above technical solution, the method of mixing the polymer, lithium salt and active filler in a solvent includes: stirring first and then ultrasonicating.
[0017] In the above technical solution, the stirring time is 120 to 600 minutes, and the stirring temperature is 20 to 50°C.
[0018] In the above technical solution, the number of ultrasounds is at least three times, the duration of each ultrasound is 10 to 60 minutes, and the frequency of each ultrasound is 40 to 100 kHz.
[0019] The preparation method of the above-mentioned multi-layer heterogeneous structure polymer composite solid electrolyte comprises: spin coating the electrolyte solution on the positive electrode plate M times to form M polymer electrolyte layers, spin coating the electrolyte solution on the negative electrode plate N times to form N polymer electrolyte layers, M and N are the same or different, M and N are both greater than or equal to 1, drying under nitrogen or inert gas atmosphere, making the side of the positive electrode plate spin coated with the polymer electrolyte layer and the side of the negative electrode plate spin coated with the polymer electrolyte layer face each other and fit together, and there is a polymer composite solid electrolyte between the positive electrode plate and the negative electrode plate, wherein the spin coating rotation speed is 1000 to 3500 rpm, and the spin coating time each time is 20 to 200 s.
[0020] In the above technical solution, the acceleration of the spin coating is 100-400 rpm / s.
[0021] In the above technical solution, the drying time is 6 to 24 hours, and the drying temperature is 20 to 50°C.
[0022] In the above technical steps, the thickness of each polymer electrolyte layer is 0.3 to 30 μm, preferably 0.3 to 2 μm.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The preparation method of the present invention obtains a multilayer heterogeneous polymer composite solid electrolyte that is widely applicable to strong oxidizing positive electrodes and strong reducing negative electrodes by coating electrolytes with different electrochemical windows onto the surfaces of positive and negative electrode sheets.
[0025] (2) The preparation method of the present invention uses a spin coating method to evenly distribute and infiltrate the electrolyte solution on the surface of the electrode sheet. The multilayer heterogeneous polymer composite solid electrolyte formed after drying has good interface contact with the electrode sheet, and the flexible contact between the polymer electrolyte layers after assembly can obtain a smaller interface resistance.
[0026] (3) The different lithium salts added to the multilayer heterogeneous polymer composite solid electrolyte prepared by the present invention can adapt to the potential of the positive and negative electrodes, reduce the decomposition of lithium salts, and improve the cycle performance. The addition of active fillers can improve the ionic conductivity of the polymer electrolyte, reduce the crystallinity of the polymer, and further reduce the interface impedance between it and the electrode.
[0027] (4) The raw materials used in the present invention are easily available, the preparation process is simple, the product performance is excellent, and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A cross-sectional scanning electron microscope image of a multilayer heterostructured polymer composite solid electrolyte prepared in Example 1;
[0029] Figure 2 The electrochemical impedance spectroscopy data of the NCM811 solid-state lithium-ion battery using the multilayer heterogeneous polymer composite solid electrolyte prepared in Example 1;
[0030] Figure 3 1C rate cycle curve of NCM811 solid-state lithium-ion battery using the multi-layer heterogeneous polymer composite solid electrolyte prepared in Example 1;
[0031] Figure 4 A cross-sectional scanning electron microscope image of a multilayer heterostructured polymer composite solid electrolyte prepared in Example 4;
[0032] Figure 5 The electrochemical impedance spectroscopy data of the NCM811 solid-state lithium-ion battery using the multilayer heterogeneous polymer composite solid electrolyte prepared in Example 4;
[0033] Figure 6 1C rate cycle curve of NCM811 solid-state lithium-ion battery using the multi-layer heterogeneous polymer composite solid electrolyte prepared in Example 4;
[0034] Figure 7 A cross-sectional scanning electron microscope image of a multilayer heterostructured polymer composite solid electrolyte prepared in Example 5;
[0035] Figure 8 The electrochemical impedance spectroscopy data of the NCM811 solid-state lithium-ion battery using the multilayer electrolyte membrane prepared in Comparative Example 1;
[0036] Fig. 9 The electrochemical impedance spectroscopy data of the NCM811 solid-state lithium-ion battery using the multilayer heterogeneous polymer composite solid electrolyte prepared in Comparative Example 2;
[0037] Fig.10This is the 1C rate cycle curve of the NCM811 solid-state lithium-ion battery using the multi-layer heterogeneous polymer composite solid electrolyte prepared in Comparative Example 2. DETAILED DESCRIPTION
[0038] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings.
[0039] In the following examples and comparative examples, the positive electrode plate is an NCM811 plate (purchased from CROOD), wherein the loading amount of active material in the positive electrode plates of Examples 1 to 5 and Comparative Examples 1 to 2 is shown in Table 1.
[0040] Table 1
[0041] Example <![CDATA[Loading amount (unit: mg / cm 2 )]]> Example 1 <![CDATA[7.6mg / cm 2 ]]> Example 2 <![CDATA[6.9mg / cm 2 ]]> Example 3 <![CDATA[7.9mg / cm 2 ]]> Example 4 <![CDATA[5.9mg / cm 2 ]]> Example 5 <![CDATA[6.1mg / cm 2 ]]> Comparative Example 1 <![CDATA[6.1mg / cm 2 ]]> Comparative Example 2 <![CDATA[6.7mg / cm 2 ]]>
[0042] In the following embodiments and comparative examples, the negative electrode plate is a metal lithium plate.
[0043] Example 1
[0044] A multi-layer heterogeneous polymer composite solid electrolyte is a layered structure consisting of M+N polymer electrolyte layers, M=1, N=1, the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the positive electrode plate is layer A, and the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the negative electrode plate is layer B.
[0045] Each polymer electrolyte layer is obtained by spin coating an electrolyte solution, wherein the electrolyte solution includes: a polymer, a lithium salt, an active filler and a solvent, wherein the ratio of the polymer, the lithium salt and the active filler is X, the volume fraction of the solvent to the mass fraction of the polymer is Y, the unit of the volume fraction is mL, and the unit of the mass fraction is g. The polymer, the lithium salt, the active filler and the solvent in the electrolyte solution used for spin coating to form the A layer and the B layer are shown in Table 2. X, Y corresponding to each polymer electrolyte layer and the thickness of each polymer electrolyte layer are shown in Table 2.
[0046] Table 2
[0047]
[0048] The preparation method of the electrolyte solution includes: mixing a polymer, a lithium salt, an active filler and a solvent, stirring at 25° C. for 600 minutes, and then ultrasonicating for 3 times at a frequency of 100 kHz, each time for 60 minutes, so that the polymer and the lithium salt are completely dissolved, and the active filler is evenly dispersed in the electrolyte solution.
[0049] The preparation method of the above-mentioned multi-layer heterogeneous structure polymer composite solid electrolyte comprises: spin coating the electrolyte solution on the positive electrode plate M times to form M polymer electrolyte layers, spin coating the electrolyte solution on the negative electrode plate N times to form N polymer electrolyte layers, drying at 25°C in an argon atmosphere in a glove box for 24 hours, and facing and laminating the side of the positive electrode plate with the polymer electrolyte layer and the side of the negative electrode plate with the polymer electrolyte layer, and the laminating process ensures that the two sides are aligned and there is no relative sliding. The polymer composite solid electrolyte is between the positive electrode plate and the negative electrode plate. Wherein, each time the electrolyte solution is spin coated, the spin coating speed is 3000rpm (the spin coating acceleration is 250rpm / s), and the spin coating time is 60s.
[0050] Figure 1 This is a cross-sectional scanning electron microscope image of the multilayer heterogeneous polymer composite solid electrolyte prepared in Example 1. Figure 1 It can be seen that the thickness of the multi-layer heterogeneous polymer composite solid electrolyte prepared in Example 1 is 2 μm, and it is a polymer composite solid electrolyte composed of a double polymer electrolyte layer.
[0051] The positive and negative electrodes of the polymer composite solid electrolyte with the multilayer heterogeneous structure prepared in Example 1 were placed in a CR2032 battery shell to assemble into a NCM811 solid-state lithium-ion battery. The electrochemical impedance was tested at 30°C. Figure 2 As shown by Figure 2 It can be seen that the main resistance of the polymer composite solid electrolyte is 39Ω and the interface impedance is 342Ω.
[0052] The 1C rate cycle curve of NCM811 solid-state lithium-ion battery was further tested at 30°C. Figure 3 As shown by Figure 3 It can be seen that at a rate of 1C, the NCM811 solid-state lithium-ion battery achieved a capacity of 170.7 mAh / g in the first cycle. After 100 cycles of constant current charge and discharge, the capacity was able to maintain 141 mAh / g, with a capacity retention rate of 83%, showing good cycle performance.
[0053] Example 2
[0054] A multi-layer heterogeneous polymer composite solid electrolyte is a layered structure consisting of M+N polymer electrolyte layers, M=1, N=1, the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the positive electrode plate is layer A, and the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the negative electrode plate is layer B.
[0055] Each polymer electrolyte layer is obtained by spin coating an electrolyte solution, wherein the electrolyte solution includes: a polymer, a lithium salt, an active filler and a solvent, wherein the ratio of the polymer, the lithium salt and the active filler is X, the volume fraction of the solvent to the mass fraction of the polymer is Y, the unit of the volume fraction is mL, and the unit of the mass fraction is g. The polymer, the lithium salt, the active filler and the solvent in the electrolyte solution used for spin coating to form the A layer and the B layer are shown in Table 3. X, Y corresponding to each polymer electrolyte layer and the thickness of each polymer electrolyte layer are shown in Table 3.
[0056] Table 3
[0057]
[0058] The preparation method of the electrolyte solution includes: mixing a polymer, a lithium salt, an active filler and a solvent, stirring at 25° C. for 600 minutes, and then ultrasonicating for 3 times at a frequency of 100 kHz, each time for 60 minutes, so that the polymer and the lithium salt are completely dissolved, and the active filler is evenly dispersed in the electrolyte solution.
[0059] The preparation method of the above-mentioned multi-layer heterogeneous structure polymer composite solid electrolyte comprises: spin coating the electrolyte solution on the positive electrode plate M times to form M polymer electrolyte layers, spin coating the electrolyte solution on the negative electrode plate N times to form N polymer electrolyte layers, drying at 25°C in an argon atmosphere in a glove box for 24 hours, and facing and laminating the side of the positive electrode plate with the polymer electrolyte layer and the side of the negative electrode plate with the polymer electrolyte layer, and the laminating process ensures that the two sides are aligned and there is no relative sliding. The polymer composite solid electrolyte is between the positive electrode plate and the negative electrode plate. Wherein, each time the electrolyte solution is spin coated, the spin coating speed is 3000rpm (the spin coating acceleration is 250rpm / s), and the spin coating time is 60s.
[0060] Through cross-sectional scanning electron microscopy, it can be seen that the thickness of the multi-layer heterogeneous polymer composite solid electrolyte prepared in Example 2 is 8 μm, and it is a polymer composite solid electrolyte composed of a double polymer electrolyte layer.
[0061] The positive and negative electrode sheets of the polymer composite solid electrolyte with the multilayer heterogeneous structure prepared in Example 2 were loaded into a CR2032 battery shell to assemble into an NCM811 solid-state lithium-ion battery. The electrochemical impedance spectrum of the NCM811 solid-state lithium-ion battery was tested at 30°C. The main resistance of the polymer composite solid electrolyte was 33Ω and the interface impedance was 394Ω.
[0062] The cycle curve of NCM811 solid-state lithium-ion battery at 1C rate was tested at 30°C. The NCM811 solid-state lithium-ion battery obtained a capacity of 145.1mAh / g in the first cycle. After 100 cycles of constant current charge and discharge, the capacity was able to maintain 123.4mAh / g, and the capacity retention rate was 85.1%, showing good cycle performance.
[0063] Example 3
[0064] A multi-layer heterogeneous polymer composite solid electrolyte is a layered structure consisting of M+N polymer electrolyte layers, M=1, N=1, the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the positive electrode plate is layer A, and the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the negative electrode plate is layer B.
[0065] Each polymer electrolyte layer is obtained by spin coating an electrolyte solution, wherein the electrolyte solution includes: a polymer, a lithium salt, an active filler and a solvent, wherein the ratio of the polymer, the lithium salt and the active filler is X, the volume fraction of the solvent to the mass fraction of the polymer is Y, the unit of the volume fraction is mL, and the unit of the mass fraction is g. The polymer, the lithium salt, the active filler and the solvent in the electrolyte solution used for spin coating to form the A layer and the B layer are shown in Table 4. X, Y corresponding to each polymer electrolyte layer and the thickness of each polymer electrolyte layer are shown in Table 4.
[0066] Table 4
[0067]
[0068] The preparation method of the electrolyte solution comprises: mixing a polymer, a lithium salt, an active filler and a solvent, stirring at 25° C. for 600 minutes, and then ultrasonicating at a frequency of 100 kHz for 60 minutes, and repeating three times to achieve complete dissolution of the polymer and the lithium salt, and uniform dispersion of the active filler in the electrolyte solution.
[0069] The preparation method of the above-mentioned multi-layer heterogeneous structure polymer composite solid electrolyte comprises: spin coating the electrolyte solution on the positive electrode plate M times to form M polymer electrolyte layers, spin coating the electrolyte solution on the negative electrode plate N times to form N polymer electrolyte layers, drying at 25°C in an argon atmosphere in a glove box for 24 hours, and facing and laminating the side of the positive electrode plate with the polymer electrolyte layer and the side of the negative electrode plate with the polymer electrolyte layer, and the laminating process ensures that the two sides are aligned and there is no relative sliding. The polymer composite solid electrolyte is between the positive electrode plate and the negative electrode plate. Wherein, each time the electrolyte solution is spin coated, the spin coating speed is 3000rpm (the spin coating acceleration is 250rpm / s), and the spin coating time is 60s.
[0070] Through cross-sectional scanning electron microscopy, it can be seen that the thickness of the multi-layer heterogeneous polymer composite solid electrolyte prepared in Example 3 is 27 μm, and it is a polymer composite solid electrolyte composed of a double polymer electrolyte layer.
[0071] The positive and negative electrode sheets of the polymer composite solid electrolyte with the multilayer heterogeneous structure prepared in Example 3 were loaded into a CR2032 battery shell to assemble into an NCM811 solid-state lithium-ion battery. The electrochemical impedance of the NCM811 solid-state lithium-ion battery was tested at 30°C. The main resistance of the polymer composite solid electrolyte was 61Ω and the interface impedance was 592Ω.
[0072] The cycle curve of NCM811 solid-state lithium-ion battery at 1C rate was tested at 30°C. The capacity of NCM811 solid-state lithium-ion battery reached 120.6mAh / g in the first cycle. After 100 cycles of constant current charge and discharge, the capacity was able to maintain 109mAh / g, and the capacity retention rate was 90.4%, showing good cycle performance.
[0073] Example 4
[0074] A multi-layer heterogeneous polymer composite solid electrolyte is a layered structure consisting of M+N polymer electrolyte layers, M=2, N=1, the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the positive electrode plate is layer A, the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the negative electrode plate is layer B, and the polymer electrolyte layer between layer A and layer B is layer C.
[0075] Each polymer electrolyte layer is obtained by spin coating an electrolyte solution, wherein the electrolyte solution includes: a polymer, a lithium salt, an active filler and a solvent, wherein the ratio of the polymer, the lithium salt and the active filler is X, the volume fraction of the solvent to the mass fraction of the polymer is Y, the unit of the volume fraction is mL, and the unit of the mass fraction is g. The polymer, the lithium salt, the active filler and the solvent in the electrolyte solution used for spin coating to form the A layer, the B layer and the C layer are shown in Table 5. X, Y corresponding to each polymer electrolyte layer and the thickness of each polymer electrolyte layer are shown in Table 5.
[0076] Table 5
[0077]
[0078] The preparation method of the electrolyte solution includes: mixing a polymer, a lithium salt, an active filler and a solvent, stirring at 25° C. for 600 minutes, and then ultrasonicating for 3 times at a frequency of 100 kHz, each time for 60 minutes, so that the polymer and the lithium salt are completely dissolved, and the active filler is evenly dispersed in the electrolyte solution.
[0079] The preparation method of the above-mentioned multi-layer heterogeneous structure polymer composite solid electrolyte comprises: spin coating the electrolyte solution M times on the positive electrode plate to form M polymer electrolyte layers, spin coating the electrolyte solution N times on the negative electrode plate to form N polymer electrolyte layers, drying at 25°C for 24 hours in an argon atmosphere in a glove box, and facing and laminating the side of the positive electrode plate with the polymer electrolyte layer and the side of the negative electrode plate with the polymer electrolyte layer, and the laminating process ensures that the two sides are aligned and there is no relative sliding. The polymer composite solid electrolyte is between the positive electrode plate and the negative electrode plate. Among them, when the electrolyte solution is spin coated on the A layer and the B layer, the spin coating speed is 2000rpm (the acceleration of the spin coating is 200rpm / s), and the time of each spin coating is 60s. When the electrolyte solution of the C layer is spin coated, the spin coating speed is 3000rpm (the acceleration of the spin coating is 300rpm / s), and the spin coating time is 60s.
[0080] Figure 4 This is a cross-sectional scanning electron microscope image of the multi-layer heterostructured polymer composite solid electrolyte prepared in Example 4. The thickness of the multi-layer heterostructured polymer composite solid electrolyte prepared in Example 4 is 21 μm, and it is a polymer composite solid electrolyte composed of three polymer electrolyte layers.
[0081] The positive and negative electrodes of the polymer composite solid electrolyte with the multilayer heterogeneous structure prepared in Example 4 were loaded into a CR2032 battery shell to assemble into a NCM811 solid-state lithium-ion battery, and the electrochemical impedance was tested at 30°C. Figure 5 As shown by Figure 5 It can be seen that the main resistance of the polymer composite solid electrolyte is 81Ω and the interface impedance is 416Ω.
[0082] The 1C rate cycle curve of NCM811 solid-state lithium-ion battery was further tested at 30°C. Figure 6 As shown by Figure 6 It can be seen that at a rate of 1C, the NCM811 solid-state lithium-ion battery achieved a capacity of 159.9 mAh / g in the first cycle. After 100 cycles of constant current charge and discharge, the capacity was able to maintain 144.1 mAh / g, with a capacity retention rate of 90%, showing good cycle performance.
[0083] Example 5
[0084] A multi-layer heterogeneous polymer composite solid electrolyte is a layered structure composed of M+N polymer electrolyte layers, M=5, N=1, the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the positive electrode plate is layer A, the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the negative electrode plate is layer B, the polymer electrolyte layer between layer A and layer B is layer C, layer C is M+N-2 polymer electrolyte layers, and the M+N-2 polymer electrolyte layers in layer C are, in order from close to layer A to far from layer A, a first intermediate layer, a second intermediate layer, a third intermediate layer and a fourth intermediate layer.
[0085] Each polymer electrolyte layer is obtained by spin coating an electrolyte solution, wherein the electrolyte solution includes: a polymer, a lithium salt, an active filler and a solvent, wherein the ratio of the polymer, the lithium salt and the active filler is X, the volume fraction of the solvent to the mass fraction of the polymer is Y, the unit of the volume fraction is mL, and the unit of the mass fraction is g. The polymer, the lithium salt, the active filler and the solvent in the electrolyte solution used for spin coating to form the A layer, the B layer, the first intermediate layer, the second intermediate layer, the third intermediate layer and the fourth intermediate layer are shown in Table 6. X, Y corresponding to each polymer electrolyte layer and the thickness of each polymer electrolyte layer are shown in Table 6.
[0086] Table 6
[0087]
[0088] The preparation method of the electrolyte solution includes: mixing a polymer, a lithium salt, an active filler and a solvent, stirring at 25° C. for 600 minutes, and then ultrasonicating for 3 times at a frequency of 100 kHz, each time for 60 minutes, so that the polymer and the lithium salt are completely dissolved, and the active filler is evenly dispersed in the electrolyte solution.
[0089] The preparation method of the above-mentioned multi-layer heterogeneous structure polymer composite solid electrolyte comprises: spin coating the electrolyte solution M times on the positive electrode plate to form M polymer electrolyte layers, spin coating the electrolyte solution N times on the negative electrode plate to form N polymer electrolyte layers, drying at 25°C in an argon atmosphere in a glove box for 24 hours, and facing and laminating the side of the positive electrode plate with the polymer electrolyte layer and the side of the negative electrode plate with the polymer electrolyte layer, and the laminating process ensures that the two sides are aligned and there is no relative sliding. The polymer composite solid electrolyte is between the positive electrode plate and the negative electrode plate. Among them, when spin coating the electrolyte solution of the A layer, the second intermediate layer and the fourth intermediate layer, the spin coating speed is 2000rpm (the spin coating acceleration is 250rpm / s), and the spin coating time is 60s each time, and when spin coating the electrolyte solution of the B layer, the first intermediate layer and the third intermediate layer, the spin coating speed is 2000rpm (the spin coating acceleration is 200rpm / s), and the spin coating time is 60s each time.
[0090] Figure 7 This is a cross-sectional scanning electron microscope image of the multi-layer heterostructured polymer composite solid electrolyte prepared in Example 5. The thickness of the multi-layer heterostructured polymer composite solid electrolyte prepared in Example 5 is 42 μm, and it is a polymer composite solid electrolyte composed of 6 polymer electrolyte layers.
[0091] The positive and negative electrodes of the polymer composite solid electrolyte with the multilayer heterogeneous structure prepared in Example 5 were loaded into a CR2032 battery shell to assemble an NCM811 solid-state lithium-ion battery. The electrochemical impedance of the NCM811 solid-state lithium-ion battery was tested at 30°C, and the resistance of the polymer composite solid electrolyte was 101Ω, and the interface impedance was 882Ω.
[0092] The cycle curve of NCM811 solid-state lithium-ion battery at 1C rate was further tested at 30°C. The capacity of NCM811 solid-state lithium-ion battery reached 133.7 mAh / g in the first cycle. After 80 cycles of constant current charge and discharge, the capacity was able to maintain 118.2 mAh / g, and the capacity retention rate was 88.4%, showing good cycle performance.
[0093] Comparative Example 1
[0094] A multilayer electrolyte membrane has a layered structure consisting of two layers of electrolyte membranes, wherein the layer of electrolyte membrane used for contacting the positive electrode plate is layer A, and the layer of electrolyte membrane used for contacting the negative electrode plate is layer B.
[0095] Each layer of electrolyte membrane is obtained by casting from an electrolyte solution, wherein the electrolyte solution includes: a polymer, a lithium salt, an active filler and a solvent, wherein the ratio of the polymer, the lithium salt and the active filler is X, the volume fraction of the solvent to the mass fraction of the polymer is Y, the unit of the volume fraction is mL, and the unit of the mass fraction is g. The polymer, the lithium salt, the active filler and the solvent in the electrolyte solution used to form the A layer and the B layer by casting are shown in Table 7. X, Y corresponding to each layer of the electrolyte membrane and the thickness of each layer of the electrolyte membrane are shown in Table 7.
[0096] Table 7
[0097]
[0098] The preparation method of the electrolyte solution includes: mixing a polymer, a lithium salt, an active filler and a solvent, stirring at 25° C. for 600 minutes, and then ultrasonicating three times at a frequency of 100 kHz, each time for 60 minutes, so as to completely dissolve the polymer and the lithium salt, and uniformly disperse the active filler in the electrolyte solution.
[0099] The preparation method of each layer of the above-mentioned electrolyte membrane includes: pouring the electrolyte solution into a 20mm*50mm*5mm polytetrafluoroethylene mold, drying at normal pressure and 70°C for 24 hours to initially evaporate the solvent, and then vacuum drying at 95°C for 24 hours to further remove the solvent, removing the polytetrafluoroethylene mold, and obtaining the electrolyte membrane.
[0100] The positive electrode sheet, A layer, B layer, and negative electrode sheet are sequentially loaded into a CR2032 battery shell to assemble a NCM811 solid-state lithium-ion battery. The electrochemical impedance of the NCM811 solid-state lithium-ion battery is tested at 30°C. Figure 8 As shown by Figure 8 It can be seen that the bulk resistance of the multilayer electrolyte membrane is 221Ω and the interface impedance is 1100Ω.
[0101] The cycle curve of NCM811 solid-state lithium-ion battery at 0.1C rate was tested at 30°C. The NCM811 solid-state lithium-ion battery was able to obtain a capacity of 133.1mAh / g in the first cycle, and the coulombic efficiency was 69.1%. It quickly failed at a rate of 0.5C, and the cycle performance was poor.
[0102] Comparative Example 2
[0103] A multi-layer heterogeneous polymer composite solid electrolyte is a layered structure consisting of two polymer electrolyte layers, wherein the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the positive electrode plate is layer A, and the polymer electrolyte layer in the polymer composite solid electrolyte used for contacting the negative electrode plate is layer B.
[0104] Each polymer electrolyte layer is obtained by spin coating an electrolyte solution, wherein the electrolyte solution includes: a polymer, a lithium salt, an active filler and a solvent, wherein the ratio of the polymer, the lithium salt and the active filler is X, the volume fraction of the solvent to the mass fraction of the polymer is Y, the unit of the volume fraction is mL, and the unit of the mass fraction is g. The polymer, the lithium salt, the active filler and the solvent in the electrolyte solution used for spin coating to form the A layer and the B layer are shown in Table 8. X, Y corresponding to each polymer electrolyte layer and the thickness of each polymer electrolyte layer are shown in Table 8.
[0105] Table 8
[0106]
[0107]
[0108] The preparation method of the electrolyte solution includes: mixing a polymer, a lithium salt, an active filler and a solvent, stirring at 25° C. for 600 minutes, and then ultrasonicating for 3 times at a frequency of 100 kHz, each time for 60 minutes, so that the polymer and the lithium salt are completely dissolved, and the active filler is evenly dispersed in the electrolyte solution.
[0109] The preparation method of the above-mentioned multi-layer heterogeneous structure polymer composite solid electrolyte comprises: spin coating an electrolyte solution on the positive electrode plate once to form a polymer electrolyte layer, spin coating an electrolyte solution on the negative electrode plate once to form a polymer electrolyte layer, drying at 25°C for 24 hours in an argon atmosphere in a glove box, and facing and laminating the side of the positive electrode plate with the polymer electrolyte layer and the side of the negative electrode plate with the polymer electrolyte layer, and the laminating process ensures that the two sides are aligned and there is no relative sliding. The polymer composite solid electrolyte is between the positive electrode plate and the negative electrode plate. Wherein, each time the electrolyte solution is spin coated, the spin coating speed is 800rpm (the spin coating acceleration is 100rpm / s), and the spin coating time is 60s.
[0110] Through cross-sectional scanning electron microscopy, it can be seen that the thickness of the multi-layer heterogeneous polymer composite solid electrolyte prepared in Comparative Example 2 is 24 μm, and it is a polymer composite solid electrolyte composed of two polymer electrolyte layers.
[0111] The positive and negative electrodes of the polymer composite solid electrolyte with the multilayer heterogeneous structure prepared in Comparative Example 2 were loaded into a CR2032 battery shell to assemble into a NCM811 solid-state lithium-ion battery. The electrochemical impedance spectrum of the NCM811 solid-state lithium-ion battery was tested at 30°C. Fig. 9 As shown by Fig. 9 It can be seen that the main resistance of the polymer composite solid electrolyte is 91Ω and the interface impedance is 692Ω.
[0112] The cycle curve of NCM811 solid-state lithium-ion battery at 1C rate was further tested at 30°C. Fig.10 As shown by Fig.10 It can be seen that the NCM811 solid-state lithium-ion battery has a capacity of 151.2 mAh / g in the first cycle, and can maintain a capacity of 121 mAh / g after 21 cycles of constant current charge and discharge, with a capacity retention rate of 80%. After 90 cycles, the remaining capacity is 30 mAh / g, with a capacity retention rate of 20%, and the cycle performance is poor. This may be due to the slow spin coating rate, low surface airflow velocity during film formation, and poor drying effect, resulting in a high solvent content in the electrolyte membrane, a rough membrane surface, and poor adhesion.
[0113] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.
Claims
1. A multilayer heterostructured polymer composite solid electrolyte, characterized in that: The invention discloses a layered structure composed of multiple polymer electrolyte layers, each of which is obtained by spin coating an electrolyte solution. The electrolyte solution comprises: a polymer, a lithium salt and an active filler, wherein, by weight, the ratio of the polymer, the lithium salt and the active filler is (1-10): (1-16): 1, the polymer is a mixture of one or more of polyvinylidene fluoride, polymethyl methacrylate, polyethylene oxide and polyacrylonitrile, the lithium salt is a mixture of one or more of lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorobis(oxalato)phosphate and lithium difluoroborate, and the active filler is a mixture of one or more of lithium lanthanum zirconium oxide, lithium lanthanum titanium oxide, lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium germanium phosphorus sulfur, silicon dioxide and aluminum oxide.
2. The polymer composite solid electrolyte according to claim 1, characterized in that: The layer of polymer electrolyte layer in the polymer composite solid electrolyte used to contact the positive electrode plate is layer A, and the layer of polymer electrolyte layer in the polymer composite solid electrolyte used to contact the negative electrode plate is layer B. When the number of polymer electrolyte layers in the polymer composite solid electrolyte is greater than or equal to 3, the polymer electrolyte layer between layer A and layer B is layer C, and layer C is at least one polymer electrolyte layer.
3. The polymer composite solid electrolyte according to claim 1, characterized in that: The electrolyte solution further includes: a solvent, which is a mixture of one or more of acetonitrile, acetone, N-methylpyrrolidone, N,N-dimethylformamide and tetrahydrofuran.
4. The polymer composite solid electrolyte according to claim 3, characterized in that: The volume fraction ratio of the solvent to the mass fraction of the polymer is (5-20):1, the unit of the volume fraction is mL, and the unit of the mass fraction is g.
5. The polymer composite solid electrolyte according to claim 1, characterized in that: The preparation method of the electrolyte solution comprises: mixing a polymer, a lithium salt and an active filler in a solvent to obtain the electrolyte solution.
6. The polymer composite solid electrolyte according to claim 1, characterized in that: The thickness of each polymer electrolyte layer is 0.3 to 30 μm, preferably 0.3 to 2 μm.
7. The method for preparing a multilayer heterostructured polymer composite solid electrolyte according to any one of claims 1 to 6, characterized in that: The invention comprises: spin coating an electrolyte solution on a positive electrode plate M times to form M polymer electrolyte layers, spin coating an electrolyte solution on a negative electrode plate N times to form N polymer electrolyte layers, drying under a nitrogen or inert gas atmosphere, and placing a side of the positive electrode plate spin coated with the polymer electrolyte layer and a side of the negative electrode plate spin coated with the polymer electrolyte layer opposite to each other and fitting them together, with a polymer composite solid electrolyte between the positive electrode plate and the negative electrode plate, wherein the spin coating speed is 1000 to 3500 rpm, and the spin coating time for each time is 20 to 200 s.
8. The preparation method according to claim 6, characterized in that: M and N are the same or different, and both M and N are greater than or equal to 1.
9. The preparation method according to claim 6, characterized in that: The acceleration of the spin coating is 100-400 rpm / s.
10. The preparation method according to claim 6, characterized in that: The drying time is 6 to 24 hours, and the drying temperature is 20 to 50°C.
Citation Information
Cited By
Lithium gallium germanate modified PEO-based composite solid electrolyte, preparation method thereof and solid-state battery
CN119419340A
Organic composite solid electrolyte, preparation method thereof and battery
CN119419353A
Organic composite solid electrolyte and preparation method thereof, and battery
CN119419353B
Multilayer composite solid electrolyte as well as preparation method and application thereof
CN119419354A
A multilayer composite solid electrolyte and its preparation method and application