High-ionic-conductivity nanocellulose lithium ion battery diaphragm and preparation method thereof
By using tert-butanol as a dispersion medium and combining low-temperature freeze-drying and high-temperature drying methods, the porosity and electrolyte absorption of nanocellulose lithium-ion battery separators are significantly improved, and the problem of low ion conductivity of the separator in the prior art is solved. , improves electrochemical performance.
Patent Information
- Application Number
- CN202310537331.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-14
- Publication Date
- 2024-11-15
AI Technical Summary
The existing natural cellulose lithium-ion battery separators have large pore sizes, low mechanical strength and poor thermal stability, which lead to battery self-discharge and lithium dendrites. The nanocellulose separators have low ionic conductivity, affecting electrochemical performance.
T-butanol is used as the dispersion medium of nanocellulose suspension, and then filtered into a wet film by magnetic stirring and ultrasonic dispersion. Combined with low-temperature freeze-drying and high-temperature drying, and hot-pressing treatment, significantly improving the porosity and electrolysis of the membrane. liquid absorption rate, thereby improving ionic conductivity.
It significantly improves the porosity and electrolyte absorption rate of nanocellulose lithium-ion battery separators, improves ionic conductivity, improves electrochemical performance, and is suitable for high-performance power battery applications.
Smart Images

Figure CN118970358A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and specifically relates to a high ion conductivity nanocellulose lithium ion battery separator and a preparation method thereof. Background Art
[0002] Cellulose is the most widely distributed and abundant biomass material. It is biodegradable, renewable, and has excellent thermal stability. It has been successfully used in polymer separator matrices, additives in gel polymers, and solid polymer electrolytes for lithium-ion batteries. However, separators made from natural cellulose have disadvantages such as large pore size, low mechanical strength, and poor thermal stability, which may lead to severe self-discharge of the battery and the formation of lithium dendrites. Therefore, it is necessary to modify the natural cellulose separator to meet the development requirements of lithium batteries.
[0003] In recent years, nanocellulose has attracted widespread attention due to its excellent properties. Nanocellulose has excellent mechanical properties and thermal stability, and its surface is rich in hydrophilic groups, such as hydroxyl and carboxyl groups, which makes it have excellent electrolyte wettability. Nevertheless, the strong hydrogen bonding between cellulose fibers reduces the porosity of the nanocellulose membrane, which has a negative impact on the ion transfer rate. At present, changing the polarity of the cellulose suspension dispersion medium or changing the drying method of the membrane is the most common method to control the pore structure of pure nanocellulose membranes. However, using ethanol or isopropanol as a debonding agent, although it can weaken the hydrogen bonding between nanocellulose fibers, the pore structure of the membrane is still not obvious, so the ionic conductivity of the membrane is relatively low, which will directly affect the electrochemical performance of lithium-ion batteries. Therefore, it is necessary to further regulate the nanocellulose membrane to improve its ionic conductivity to meet the application needs of high-performance power batteries. Summary of the invention
[0004] Therefore, it is necessary to provide a high ionic conductivity nanocellulose lithium ion battery separator and a preparation method thereof to improve the performance of the lithium battery separator.
[0005] To achieve the above object, the present invention provides a high ionic conductivity nanocellulose lithium ion battery separator and a preparation method thereof, comprising the following steps: (1) Mixing and dispersion: The nanocellulose / water suspension and tert-butanol are mixed, and a uniform nanocellulose / water / tert-butanol suspension is obtained after magnetic stirring and ultrasonic dispersion; (2) Filtration to obtain a wet film: Filtration of the nanocellulose / water / tert-butyl alcohol suspension obtained in step (1) to obtain a nanocellulose wet film; (3) Wet film drying: subjecting the nanocellulose wet film obtained in step (2) to low-temperature freeze-drying or high-temperature drying to obtain a dry nanocellulose film; (4) Hot pressing to form a diaphragm: The dried nanocellulose film obtained in step (3) is subjected to hot pressing to obtain a nanocellulose diaphragm.
[0006] Furthermore, in step (3), the low-temperature freeze-drying treatment temperature of the nanocellulose wet film is -80°C, and the high-temperature drying treatment temperature is 80°C.
[0007] Furthermore, the porosity of the nanocellulose lithium-ion battery separator prepared by the preparation method is 50% to 80%, the electrolyte absorption rate of the separator is 200% to 300%, and the ion conductivity of the separator is 1.0 mS / cm to 2.0 mS / cm.
[0008] Different from the prior art, the present invention uses tert-butyl alcohol as the dispersion medium of the nanocellulose suspension and adopts high-temperature drying and low-temperature drying methods, which can significantly improve the porosity and electrolyte absorption rate of the nanocellulose lithium-ion battery separator, thereby facilitating the improvement of ion conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 It is a bar graph of the liquid absorption rate and porosity of lithium ion battery separators of specific examples 1-2 and comparative examples 1-3; Figure 2 It is a bar graph of the ionic conductivity of the lithium ion battery separators of specific examples 1-2 and comparative example 3. DETAILED DESCRIPTION
[0010] In order to explain in detail the technical content, features, achieved objectives and effects of the technical solution, the following is a detailed description in conjunction with specific embodiments. Example 1
[0011] A method for preparing a nanocellulose lithium-ion battery separator with high ionic conductivity, the specific preparation method comprising the following steps: (1) Weigh 10 g of nanocellulose suspension with a solid content of 1.58% and add it to a beaker. Then weigh 100 mL of tert-butyl alcohol and add it to the beaker. Stir magnetically for 24 h. Place the stirred nanocellulose suspension in an ultrasonic cleaner for ultrasonic dispersion for 2 h until all the nanofibers are evenly dispersed. (2) A nylon filter membrane with a pore size of 0.45 μm and a diameter of 8 cm is placed in a sand core filter, and 28 mL of the nanocellulose suspension obtained in step (1) is drawn with a syringe, and the nanocellulose wet membrane is obtained by filtration; (3) The wet film obtained in the above step (2) is placed in a refrigerator and frozen for 12 h, and then placed in a freeze drying oven and freeze-dried for 24 h at -80 °C and 0.01 MPa to obtain a low-temperature freeze-dried nanocellulose film; (4) The freeze-dried nanocellulose film obtained in the above step (3) is hot-pressed at a pressure of 5 MPa and a temperature of 80°C for 2 min to obtain a freeze-dried nanocellulose membrane. Example 2
[0012] A method for preparing a nanocellulose lithium-ion battery separator with high ionic conductivity, the specific preparation method comprising the following steps: (1) Weigh 20 g of nanocellulose suspension with a solid content of 1.58% and add it to a beaker. Then weigh 200 mL of tert-butyl alcohol and add it to the beaker. Stir magnetically for 24 h. Place the stirred nanocellulose suspension in an ultrasonic cleaner for ultrasonic dispersion for 2 h until all the nanofibers are evenly dispersed. (2) A nylon filter membrane with a pore size of 0.45 μm and a diameter of 8 cm is placed in a sand core filter, and 28 mL of the nanocellulose suspension obtained in step (1) is drawn with a syringe, and the nanocellulose wet film is obtained by filtration; (3) placing the wet film obtained in the above step (2) in a drying oven at 80°C for 24 h to obtain a high-temperature dried nanocellulose film; (4) The high-temperature dried nanocellulose film obtained in the above step (3) is hot-pressed at a pressure of 5 MPa and a temperature of 80°C for 2 min to obtain a high-temperature dried nanocellulose membrane.
[0013] Comparative Example 1 A method for preparing a nanocellulose lithium-ion battery separator, the specific preparation method comprising the following steps: (1) Weigh 20 g of nanocellulose suspension with a solid content of 1.58% and add it to a beaker. Then weigh 200 mL of tert-butyl alcohol and add it to the beaker. Stir magnetically for 24 h. Place the stirred nanocellulose suspension in an ultrasonic cleaner for ultrasonic dispersion for 2 h until all the nanofibers are evenly dispersed. (2) A nylon filter membrane with a pore size of 0.45 μm and a diameter of 8 cm is placed in a sand core filter, and 28 mL of the nanocellulose suspension obtained in step (1) is drawn with a syringe, and the nanocellulose wet film is obtained by filtration; (3) drying the wet film obtained in the above step (2) at room temperature of 25°C for 24 hours to obtain a room temperature dried nanocellulose film; (4) The room temperature dried nanocellulose membrane obtained in the above step (3) is hot pressed at a pressure of 5 MPa and a temperature of 80°C for 2 min to obtain a room temperature dried nanocellulose membrane.
[0014] Comparative Example 2 A method for preparing a nanocellulose lithium-ion battery separator, the specific preparation method comprising the following steps: (1) Weigh 20 g of nanocellulose suspension with a solid content of 1.58% and add it to a beaker. Then weigh 200 mL of ethanol and add it to the beaker. Stir magnetically for 24 h. Place the stirred nanocellulose suspension in an ultrasonic cleaner for ultrasonic dispersion for 2 h until all the nanofibers are evenly dispersed. (2) A nylon filter membrane with a pore size of 0.45 μm and a diameter of 8 cm is placed in a sand core filter, and 28 mL of the nanocellulose suspension obtained in step (1) is drawn with a syringe, and the nanocellulose wet film is obtained by filtration; (3) The wet film obtained in the above step (2) is placed in a refrigerator and frozen for 12 h, and then placed in a freeze drying oven and freeze-dried for 24 h at -80°C and 0.01 MPa to obtain a low-temperature freeze-dried nanocellulose film; (4) The freeze-dried nanocellulose film obtained in the above step (3) is hot-pressed at a pressure of 5 MPa and a temperature of 80°C for 2 min to obtain a nanocellulose membrane.
[0015] Comparative Example 3 A method for preparing a nanocellulose lithium-ion battery separator, the specific preparation method comprising the following steps: (1) Weigh 20 g of nanocellulose suspension with a solid content of 1.58% and add it to a beaker. Then weigh 200 mL of ethanol and add it to the beaker. Stir magnetically for 24 h. Place the stirred nanocellulose suspension in an ultrasonic cleaner for ultrasonic dispersion for 2 h until all the nanofibers are evenly dispersed. (2) A nylon filter membrane with a pore size of 0.45 μm and a diameter of 8 cm is placed in a sand core filter, and 28 mL of the nanocellulose suspension obtained in step (1) is drawn with a syringe, and the nanocellulose wet film is obtained by filtration; (3) placing the wet film obtained in the above step (2) in a drying oven at 80°C for 24 h to obtain a high-temperature dried nanocellulose film; (4) The high-temperature dried nanocellulose film obtained in the above step (3) is hot-pressed at a pressure of 5 MPa and a temperature of 80°C for 2 min to obtain a nanocellulose membrane.
[0016] The liquid absorption rate of the lithium ion battery separators of Examples 1-2 and Comparative Examples 1-3 was tested: The prepared lithium-ion battery separator was cut into discs with a diameter of 17 mm, and its weight was weighed and recorded as M1; then it was immersed in the electrolyte for 1 h, the electrolyte on the surface was absorbed with filter paper, and its weight was weighed again and recorded as M2; the liquid absorption rate of the lithium-ion battery separator can be calculated by the following formula: η=(M2-M1) / M1*100% Where η is the liquid absorption rate of the lithium-ion battery separator (%), M1 is the mass of the lithium-ion battery separator before immersion (g), and M2 is the mass of the lithium-ion battery separator after immersion (g). The experimental results are shown in Figure 1 And as shown in Table 1.
[0017] The porosity test was performed on the lithium ion battery separators of Examples 1-2 and Comparative Examples 1-3: The porosity of the diaphragm was measured by the n-butanol immersion method. The cut diaphragm with a diameter of 17 mm was immersed in n-butanol for 1 h. The excess n-butanol on the surface of the diaphragm was removed with filter paper and weighed. The porosity of the diaphragm was calculated by the following formula: P = (W b / ρ b ) / V s * 100% Among them, P (%), W b (g), ρ b (g / cm -3 ) and V s They are the porosity of the membrane, the weight of the absorbed n-butanol, the density of n-butanol (0.81 g / mL) and the volume of the membrane after drying. The experimental results are shown in Figure 1 And as shown in Table 1.
[0018] The ionic conductivity test was performed on the lithium ion battery separators of Examples 1-2 and Comparative Examples 1-3: The steel sheet / diaphragm / steel sheet battery was assembled and the bulk resistance of the diaphragm was tested by an electrochemical workstation. The frequency was set to 0.1 Hz-0.1 MHz and the scan rate was 10 mV / S. The ionic conductivity of the diaphragm was calculated by the following formula: σ = L / AR Where L (cm) is the thickness of the diaphragm, A (cm 2 ) is the area of the stainless steel electrode sheet, R (Ω) is the diaphragm resistance, and the experimental results are as follows Figure 2 And as shown in Table 1.
[0019] The physical properties of the lithium battery separator of the present invention are shown in Table 1 below:
[0020] Depend on Figure 1 , Figure 2It can be concluded from Table 1 that the porosity, liquid absorption rate and ionic conductivity of the embodiment are greater than those of the comparative example.
[0021] In summary, the following conclusions can be drawn: using tert-butanol as the dispersing medium of nanocellulose suspension and adopting high temperature and low temperature drying methods can effectively improve the porosity and liquid absorption rate of nanocellulose lithium-ion battery separators, and the increase in liquid absorption rate and porosity can effectively improve the ionic conductivity of nanocellulose lithium-ion battery separators.
[0022] The above descriptions are merely embodiments of the present invention, and are not intended to limit the patent protection scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention's specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a high ionic conductivity nanocellulose lithium ion battery separator, characterized in that: The following steps are involved: (1) Mixing and dispersion: The nanocellulose / water suspension and tert-butanol are mixed, and a uniform nanocellulose / water / tert-butanol suspension is obtained after magnetic stirring and ultrasonic dispersion; (2) Filtration to obtain a wet film: Filtration of the nanocellulose / water / tert-butyl alcohol suspension obtained in step (1) to obtain a nanocellulose wet film; (3) Wet film drying: subjecting the nanocellulose wet film obtained in step (2) to low-temperature freeze-drying or high-temperature drying to obtain a dry nanocellulose film; (4) Hot pressing to form a diaphragm: The dried nanocellulose film obtained in step (3) is subjected to hot pressing to obtain a nanocellulose diaphragm.
2. The preparation method according to claim 1, characterized in that: The low-temperature freeze-drying treatment temperature of the nanocellulose wet film in step (3) is -80°C, and the high-temperature drying treatment temperature is 80°C.
3. The preparation method according to claim 1, characterized in that: The diaphragm prepared by the method has a porosity of 50% to 80%, an electrolyte absorption rate of 200% to 300%, and an ion conductivity of 1.0 mS / cm to 2.0 mS / cm.
Citation Information
Cited By
Nanocellulose-based sodium-ion battery diaphragm as well as preparation method and application thereof
CN119944227A
Preparation method of lignin-coated cellulose nanofiber sodium-ion battery diaphragm
CN120089904A
A method for preparing a lignin-coated cellulose nanofiber sodium-ion battery separator
CN120089904B
Preparation Method for Lignin-Coated Cellulose Nanofiber Sodium-Ion Battery Separator
NL4000751A