Method for manufacturing magnetic sheet
By using heat treatment and adhesion layer adhesion methods in the manufacturing process of nanocrystal alloy thin tape magnetic sheets, the problems of low productivity and poor magnetic properties of nanocrystal alloy thin tape magnetic sheets in the prior art are solved, and high efficiency is achieved , the production of low-cost nanocrystal alloy thin tape magnetic sheets has excellent magnetic properties and good isotropy.
Patent Information
- Application Number
- CN202380031761.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-29
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, when manufacturing nanocrystal alloy thin tape magnetic sheets, it is difficult to obtain materials with excellent magnetic properties and good isotropicity through high productivity methods, and the process efficiency of multiple rolling and winding is low.
The amorphous alloy thin strip is contacted with the heating body and applied tension to heat it, reducing the number of times of rolling out and taking, and attaching the adhesive layer to the heat-treated nanocrystalline alloy thin strip, by adjusting the tension of the adhesive layer and The structure is to suppress deterioration of magnetic properties and improve the productivity of the magnetic sheet.
It has achieved the reduction of the number of rolling and winding times, improved productivity, and obtained a nanocrystalline alloy thin strip magnetic sheet with excellent magnetic characteristics and good isotropy, with high saturation magnetic flux density and low iron loss.
Smart Images

Figure CN118974848A_ABST
Abstract
Description
[0001] Cross-reference to related applications
[0002] This international application claims the priority based on Japanese Patent Application No. 2022-055680 filed with the Japan Patent Office on March 30, 2022, the entire contents of which are hereby incorporated by reference into this international application. Technical Field
[0003] The present disclosure relates to a method for producing a magnetic sheet in which an adhesive layer is attached to one surface of a nanocrystalline alloy ribbon. Background Art
[0004] In recent years, electronic devices such as smart phones, tablet information terminals or mobile phones are rapidly becoming popular. In particular, mobile phones (for example, smart phones), web terminals, music players, etc. are required to be able to be used continuously for a long time in order to be convenient as portable devices. In these small portable devices, secondary batteries such as lithium-ion batteries are used as power sources. The charging method of the secondary battery includes a contact charging method in which the electrode on the power receiving side is directly contacted with the electrode on the power supply side for charging, and a non-contact charging method in which a transmission coil is set on both the power supply side and the power receiving side and the charging is performed by power transmission using electromagnetic induction. The non-contact charging method does not require an electrode for direct contact between the power supply device and the power receiving device, so different power receiving devices can also be charged using the same power supply device. In addition, the non-contact charging method is a technology that can be used not only in portable devices, but also in other electronic devices, electric vehicles, drones, etc.
[0005] In the contactless charging method, the magnetic flux generated in the primary transmission coil of the power supply device generates an electromotive force in the secondary transmission coil of the power receiving device through the housings of the power supply device and the power receiving device, thereby supplying power. In order to obtain high power transmission efficiency, a magnetic sheet is provided as a coil yoke on the opposite side of the contact surface between the power supply device and the power receiving device relative to the transmission coil. The magnetic sheet has the following functions.
[0006] The first function is to act as a magnetic shielding material. For example, when leakage magnetic flux generated during the charging operation of a non-contact charging device flows through other parts such as metal components constituting a secondary battery, these parts will generate heat due to eddy currents. The magnetic sheet can suppress this heat as a magnetic shielding material.
[0007] The second function of the magnetic sheet is to function as a yoke member for recirculating the magnetic flux generated by the coil during charging.
[0008] Conventionally, ferrite materials have been the mainstream of soft magnetic materials for magnetic sheets used in non-contact charging devices. However, recently, as disclosed in Japanese Patent Application Laid-Open No. 2008-112830, soft magnetic alloy ribbons made of amorphous alloys and nanocrystalline alloys have begun to be used.
[0009] International Publication No. 2014 / 157526 discloses a magnetic sheet using a thin ribbon obtained by heat-treating Fe-based amorphous material and having a magnetic permeability μr of 220 to 770 at 500 kHz.
[0010] In addition, International Publication No. 2020 / 235643 discloses a method for manufacturing a nanocrystalline alloy ribbon with a resin film, which comprises: a process of preparing an amorphous alloy ribbon capable of nanocrystallization, a process of performing a nanocrystallization heat treatment under a state of applying tension to the amorphous alloy ribbon to obtain a nanocrystalline alloy ribbon, and a process of maintaining the nanocrystalline alloy ribbon on the resin film via an adhesive layer. In addition, a process of forming cracks in the nanocrystalline alloy ribbon is also disclosed.
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Laid-Open No. 2008-112830
[0014] Patent Document 2: International Publication No. 2014 / 157526
[0015] Patent Document 3: International Publication No. 2020 / 235643 Summary of the invention
[0016] Problems to be solved by the invention
[0017] Patent Document 1 does not disclose specific means of the heat treatment method.
[0018] Patent document 2 discloses the following process: a heat treatment process for a thin plate-shaped magnetic body 10 composed of an Fe-based metal magnetic material and having a single layer thickness of 15 μm to 35 μm, thereby setting the AC relative permeability μr of the thin plate-shaped magnetic body 10 at a frequency of 500 kHz to be greater than 220 and less than 770; and a lamination process for maintaining the heat-treated thin plate-shaped magnetic body 10 on a resin film (substrate 20) via an adhesive layer 15 to form a magnetic sheet 1; and the heat treatment process and the lamination process are respectively independent processes.
[0019] Patent Document 3 discloses a step of unwinding, heat treating, and then winding up as a heat treatment step, and also discloses a step of holding a nanocrystalline alloy ribbon on a resin film via an adhesive layer, which is different from the heat treatment step.
[0020] When heat treating an amorphous alloy ribbon to produce a nanocrystalline alloy ribbon, for example, as described in Patent Document 3, the following operation is performed: an amorphous alloy ribbon for a nanocrystalline alloy ribbon wound into a coil is unwound, heat treated, and then wound into a coil.
[0021] When attaching a resin film to a nanocrystalline alloy ribbon, for example, as described in Patent Documents 2 and 3, the following operation is performed: the nanocrystalline alloy ribbon wound into a coil is unwound, and the resin film is attached via an adhesive layer and then wound into a coil.
[0022] Thus, when manufacturing a magnetic sheet using nanocrystalline alloy ribbons, each step such as the heat treatment step and the resin film attachment step requires the step of unwinding the coiled strip, treating the coiled strip, and then winding the coiled strip again.
[0023] As described above, when a magnetic sheet using a nanocrystalline alloy ribbon is produced, the step of winding into a coil shape and the step of unwinding from the coil shape are performed multiple times.
[0024] In addition, the nanocrystalline alloy strip is manufactured by the following method: the alloy melt adjusted to a specified alloy composition is ejected onto a rotating cooling roller, and the alloy strip is manufactured by rapid solidification, and then the alloy strip is heat treated. The thickness of the nanocrystalline alloy strip is thin, and it can be manufactured into a long strip with a specified width. According to this manufacturing method, it is easy to introduce anisotropy in the casting direction (length direction), and even after heat treatment, there is a tendency that the magnetic properties are different in the length direction of the long strip and the width direction orthogonal to the length direction.
[0025] Depending on the application, magnetic properties are required to be as isotropic as possible. However, as mentioned above, it is difficult to obtain nanocrystalline alloy thin strips with excellent magnetic properties (high saturation magnetic flux density, low iron loss) and good isotropy by a method with high productivity.
[0026] The present invention aims to provide a method for manufacturing a magnetic sheet with high productivity, which reduces the number of unwinding and winding. In addition, the present invention aims to provide a method for manufacturing a magnetic sheet having a nanocrystalline alloy ribbon having excellent magnetic properties and good isotropy.
[0027] Methods for solving problems
[0028] The first mode of manufacturing a magnetic sheet disclosed in the present invention comprises: a heat treatment step of heat-treating an amorphous alloy strip to produce a nanocrystalline alloy strip, and an attaching step of attaching an adhesive layer to one surface of the nanocrystalline alloy strip; in the heat treatment step, the amorphous alloy strip is unrolled from the amorphous alloy strip wound into a coil, and the amorphous alloy strip is brought into contact with a heating body while being conveyed, and a strip pressing member is brought into contact with the opposite surface of the amorphous alloy strip that is in contact with the heating body, thereby heating the amorphous alloy strip while being pressed against the heating body, applying a tension of less than 18 MPa to the amorphous alloy strip and introducing it into the heating body; in the attaching step, the nanocrystalline alloy strip conveyed from the heat treatment step is conveyed while an adhesive layer is attached to the one surface of the nanocrystalline alloy strip.
[0029] Effects of the Invention
[0030] According to the present disclosure, a method for manufacturing a magnetic sheet with high productivity can be provided, which reduces the number of unwinding and winding times. In addition, a method for manufacturing a magnetic sheet having a nanocrystalline alloy ribbon having excellent magnetic properties and good isotropy can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a conceptual diagram showing one embodiment of the present disclosure.
[0032] Figure 2 This is a conceptual diagram showing an embodiment of the heat treatment process of the present disclosure.
[0033] Figure 3 It is a cross-sectional view showing the structure of the adhesive layer of the present disclosure.
[0034] Figure 4 This is a cross-sectional view showing a structure after the protective sheet of the adhesive layer of the present disclosure is peeled off.
[0035] Figure 5 It is a cross-sectional view showing a structure in which a nanocrystalline alloy thin strip is attached to an adhesive layer of the present disclosure.
[0036] Figure 6 This is a cross-sectional view showing a structure in which cracks are formed in a nanocrystalline alloy ribbon attached to the adhesive layer of the present disclosure.
[0037] Figure 7 This is a cross-sectional view showing the structure of one embodiment of the magnetic sheet of the present disclosure. DETAILED DESCRIPTION
[0038] Hereinafter, embodiments of the present disclosure will be described in detail. The present disclosure is not limited to the following embodiments at all, and can be implemented by appropriately adding modifications within the scope of the purpose of the present disclosure.
[0039] In the present disclosure, the numerical range represented by "to" represents a range including the numerical values recorded before and after "to" as the lower limit and the upper limit, respectively. In the numerical range recorded in stages in the present disclosure, the upper limit or lower limit recorded in a certain numerical range may also be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In addition, in the numerical range recorded in the present disclosure, the upper limit or lower limit recorded in a certain numerical range may also be replaced by the value shown in the embodiments.
[0040] In the present disclosure, a combination of two or more preferred aspects is a more preferred aspect.
[0041] exist Figure 1 2 is a conceptual diagram illustrating a method for producing a magnetic sheet according to an embodiment of the present disclosure.
[0042] exist Figure 1 In the method, first, an amorphous alloy ribbon 12 wound into a coil shape for the nanocrystalline alloy ribbon 3 is prepared. Figure 1 1 shows a coil 11 in which an amorphous alloy ribbon 12 for the nanocrystalline alloy ribbon 3 is wound into a coil. The amorphous alloy ribbon 12 (hereinafter also simply referred to as "ribbon 12") is rolled out from the coil 11. The rolled out amorphous alloy ribbon 12 is transported to a heat treatment step.
[0043] <Heat treatment process>
[0044] The heat treatment method disclosed in the present invention is a method for heating the amorphous alloy thin strip 12 by contacting it with a heating body. When the amorphous alloy thin strip 12 is heated by contacting it with a heating body, the amorphous alloy thin strip 12 is conveyed, and a thin strip pressing member is brought into contact with the opposite surface of the amorphous alloy thin strip 12 that contacts the heating body, and the amorphous alloy thin strip 12 is heated while being pressed against the heating body.
[0045] In the present disclosure, a soft member may be used as the thin-belt pressing member.
[0046] As the soft member, a metal member is preferable. It should be noted that the soft member refers to a member that can be deformed along the roller.
[0047] In addition, the thin strip pressing member may be a belt or a roller.
[0048] Figure 2 A conceptual diagram showing the heat treatment process.
[0049] The tension of the rolled amorphous alloy ribbon 12 is adjusted by the dancer rollers 51 and 52. The amorphous alloy ribbon 12 given a predetermined tension is heated by contacting the heating roller 16 that functions as a heating body. Nanocrystals are generated in the amorphous alloy ribbon 12 by the heating, and the amorphous alloy ribbon 12 becomes a nanocrystalline alloy ribbon 3.
[0050] At this time, the tension applied to the amorphous alloy ribbon 12 is preferably 18 MPa or less, more preferably 17 MPa or less, and preferably 3 MPa or more, more preferably 3.5 MPa or more, and even more preferably 5.5 MPa or more.
[0051] In this embodiment, after the heat treatment process, the adhesive layer 2 is attached to the nanocrystalline alloy ribbon 3, but in the attachment of the adhesive layer 2, tension is applied to the adhesive layer 2 for attachment. After the adhesive layer 2 is attached to the nanocrystalline alloy ribbon 3, the tension applied to the adhesive layer 2 is released, and the adhesive layer 2 tends to shrink. In this way, stress is applied to the nanocrystalline alloy ribbon 3 along the direction in which it tends to shrink.
[0052] If excessive stress is applied to the nanocrystalline alloy ribbon 3 , desired magnetic properties may not be obtained.
[0053] In the present disclosure, by applying tension to the amorphous alloy strip 12 and pre-heat-treating it, it is expected that the effect of suppressing the deterioration of the characteristics caused by the stress in the direction of contraction of the adhesive layer 2 after the adhesive layer 2 is attached can be suppressed. Thus, the deterioration of the magnetic characteristics caused by applying useless stress to the nanocrystalline alloy strip 3 can be suppressed. However, if a large tension is applied to the amorphous alloy strip 12, it is difficult to obtain isotropic characteristics. Therefore, it is preferred to apply a tension of less than 18MPa to the amorphous alloy strip 12 and introduce the amorphous alloy strip 12 to the heating body.
[0054] exist Figure 2 , there are shown a heating roller 16 that can be used in the heat treatment process of the present embodiment, a thin strip pressing metal belt 19 that functions as a thin strip pressing member, a first roller 17 on the process upstream side that supports the thin strip pressing metal belt 19, and a second roller 18 on the process downstream side. The thin strip pressing metal belt 19 is an example of a mechanism for forming a state in which the amorphous alloy thin strip 12 is pressed against the heating roller 16.
[0055] The amorphous alloy strip 12 is passed between the heating roller 16 and the strip pressing metal strip 19 , and the amorphous alloy strip 12 is heated while being pressed against the heating roller 16 . Figure 2 The arrows in show the operation of each part, and the heating roller 16, the first roller 17, and the second roller 18 are configured to rotate. Thus, the amorphous alloy strip 12 is conveyed and heated while being pressed against the heating roller 16.
[0056] Here, the ribbon 12 heated by the heating roller 16 becomes the nanocrystalline alloy ribbon 3 .
[0057] It should be noted that it is preferred to use a heating roller that can also heat the first roller 17 and the second roller 18. Therefore, it is preferred to heat the metal belt 19 for pressing the thin strip in advance. When the first roller 17 and the second roller 18 are used as heating rollers, it is preferred to set the temperature of the metal belt 19 for pressing the thin strip (that is, the temperature when in contact with the thin strip 12) to a temperature that is equal to or slightly lower than the heating temperature of the thin strip 12. The temperature of the first roller 17 and the second roller 18 can be set to a temperature for making the temperature of the metal belt 19 for pressing the thin strip an appropriate temperature. For example, it is preferred to set the temperature of the first roller 17 and the second roller 18 to be about 50°C higher than the temperature of the heating roller 16. The temperature of the metal belt 19 for pressing the thin strip, the first roller 17 and the second roller 18 can be selected to be a temperature suitable for heat treatment of the thin strip 12.
[0058] exist Figure 2 In the figure, the first guide bevel 41 on the upstream side of the process and the second guide bevel 42 on the downstream side of the process for the thin strip 12 are shown. By using the inclined first guide bevel 41 and the second guide bevel 42 before and after the heating roller 16 (i.e., on both sides of the upstream and downstream of the process), the amorphous alloy thin strip 12 can be supplied to the heating roller 16 in a manner of simultaneously contacting the thin strip to press the metal strip 19 and the heating roller 16, and can also be discharged. That is, by adjusting the inclination angle of the first guide bevel 41 and the second guide bevel 42, the angle of supply and discharge of the amorphous alloy thin strip 12 is set, and the surface and back of the amorphous alloy thin strip 12 can be heated at the same time, and cooled at the same time. It is more preferred to configure the first guide bevel 41 and the second guide bevel 42 in a manner that the extension lines of each of the first guide bevel 41 and the second guide bevel 42 are consistent with the tangent line of the heating roller 16. It should be noted that the surface and back of the amorphous alloy thin strip 12 are the first surface of the amorphous alloy thin strip 12 and the second surface on the opposite side of the first surface.
[0059] The thin strip pressing metal strip 19 is an example of a soft member, and from the viewpoint of flexibility and strength, the soft member is preferably a metal member. For example, as the soft member, it is more preferable to use a material having excellent heat resistance, such as heat-resistant stainless steel or nickel-based superalloy.
[0060] According to the above-mentioned heat treatment method, a structure is formed in which the soft member (the strip pressing metal belt 19 in this embodiment) is brought into contact with the surface of the amorphous alloy strip 12 opposite to the surface in contact with the heating roller 16, and the amorphous alloy strip 12 is pressed against the heating roller 16, thereby the amorphous alloy strip 12 is in a state of being pressed against the heating roller 16. It should be noted that the amorphous alloy strip 12 is preferably brought into close contact with the heating roller 16 by the strip pressing metal belt 19, so that the amorphous alloy strip 12, the strip pressing metal belt 19 and the heating roller 16 are moved as one.
[0061] Here, the heating roller 16 is an example of a heating body (heating body disclosed in the present invention) for directly contacting and heating the amorphous alloy strip 12. The amorphous alloy strip 12 contacts and is heated by a portion of the outer peripheral surface of the cylindrical heating roller 16 (i.e., a portion of the circumferential area). The heating roller 16 can also have a conveying driving force for the amorphous alloy strip 12. The roller used to drive the strip to press the metal strip 19 can be both the first roller 17 and the second roller 18, or either one. For example, it can also be configured so that the second roller 18 on the downstream side of the process has a driving force, and the first roller 17 on the upstream side of the process is mechanically subordinate. In this way, complex control such as the electrical synchronous operation of the first roller 17 and the second roller 18 can be avoided, and there is no need to correct the synchronization deviation caused by the thermal expansion difference between the first roller 17 and the second roller 18.
[0062] It should be noted that the heating roller 16 is an example of a heating body having a convex surface for contacting and heating the amorphous alloy thin strip 12. In addition, the "convex surface" refers to a surface that is raised on the side of the amorphous alloy thin strip 12, such as Figure 1 As shown in the figure, the heating roller 16 may have a curved surface formed by a cylindrical (or columnar) side surface or a curved surface formed as a part of a component, such as a curved surface portion of a substantially D-shaped component, as long as the amorphous alloy thin strip 12 follows and ensures sufficient contact. It should be noted that the heating body of the present disclosure may be a non-rotating structure, or a structure in which the thin strip 12 moves (i.e., slides) on the heating body.
[0063] In the heat treatment method of the present disclosure, a ribbon pressing roller can also be used as the ribbon pressing member. It should be noted that the ribbon pressing roller is also preferably a heatable heating roller.
[0064] In the heat treatment method disclosed in the present invention, the following structure may be adopted: a substantially D-shaped heating body is used instead of the heating roller 16, and a thin strip pressing metal strip and a roller supporting the thin strip pressing metal strip are provided as a mechanism for pressing the amorphous alloy thin strip 12 against the heating body. In this case, the heating body may be a fixed structure and the amorphous alloy thin strip 12 may slide on the heating body. It should be noted that the amorphous alloy thin strip 12 is pressed against the heating body by the thin strip pressing metal strip. Thus, the amorphous alloy thin strip 12 is transported and heated while being pressed against the heating body.
[0065] In the heat treatment method disclosed in the present invention, the heating rate of the amorphous alloy strip 12 is preferably set to 50°C / sec to 4000°C / sec. When the nanocrystalline alloy strip 3 is obtained by heat treatment, the heating rate for achieving a fine nanocrystalline structure varies according to the composition, but the composition with low Cu, low M elements, and high Fe content that can obtain a high saturation magnetic flux density requires a faster heating rate. In the case of one embodiment of the present invention, the lower limit of the heating rate is 50°C / sec, and the upper limit can be determined according to the equipment capacity of the heat treatment device, the temperature of the heating body and the strip pressing member, the contact state of the heating body and the strip pressing member with the strip 12, etc., but it is substantially about 4000°C / sec. Preferably, it is above 500°C / sec.
[0066] The heating body preferably has a width wider than the width of the amorphous alloy strip 12. Thus, when the amorphous alloy strip 12 is pressed against the heating body, the entire width of the strip 12 is in close contact with the heating body. In addition, the strip pressing member also preferably has a width wider than the width of the amorphous alloy strip 12. Thus, when the amorphous alloy strip 12 is pressed against the heating body, the entire width of the strip 12 is easily in close contact with the heating body.
[0067] In addition, when the amorphous alloy strip 12 is heated while being pressed against the heating body, the distance from the contact of the amorphous alloy strip 12 with the heating body to the separation is preferably 50 mm or more on the length of the heating body surface. In addition, the distance from the contact of the amorphous alloy strip 12 with the heating body to the separation is more preferably 150 mm or more on the length of the heating body surface. This distance is equivalent to the movement distance of the amorphous alloy strip 12 from the contact of the amorphous alloy strip 12 with the heating body to the separation.
[0068] The conveying speed of the amorphous alloy ribbon 12 is preferably set to 1 m / min or more. In mass production, the higher the conveying speed, the higher the production volume, so the conveying speed is more preferably set to 10 m / min or more.
[0069] The contact time of the amorphous alloy thin strip 12 and the heating body is preferably 0.1 to 30 seconds. The lower limit of the contact time is more preferably 0.2 seconds, the upper limit of the contact time is more preferably 10 seconds, further more preferably 5 seconds, and most preferably 2 seconds. In order to improve mass production, the contact time is preferably 0.2 to 2 seconds in the case of high speed and stabilization.
[0070] According to the heat treatment method disclosed in the present invention, by forming a state in which the amorphous alloy strip 12 is pressed against a heating body, the contact between the heating body and the strip 12 is improved, the heat transferability is improved, and the heating rate is accelerated. In addition, the heat generated by crystallization can be released more by the heating body and the strip pressing metal (belt, roller), and the maximum temperature of the strip 12 can be suppressed (that is, the temperature rise caused by self-heating can be suppressed). Furthermore, by forming a state in which the strip 12 is pressed by a strip pressing member (belt, roller), wrinkles or stripes that are easily generated during crystallization can be suppressed. As a result, heat treatment at a higher temperature can be performed, and heat treatment with a fast heating rate and short contact time can be performed. Therefore, productivity can be improved and a uniform nanocrystalline structure can be obtained, and a nanocrystalline alloy strip 3 with a higher saturation magnetic flux density and excellent magnetic properties can be obtained.
[0071] The pressure at which the amorphous alloy thin strip 12 is pressed against the heating body is preferably 0.03 MPa or more, more preferably 0.04 MPa or more, further preferably 0.05 MPa or more, and further preferably 0.07 MPa or more.
[0072] In order to further improve the contact between the amorphous alloy thin strip 12 and the heater, the heater has a curvature. The curvature of the heater preferably has a radius of curvature of 25 mm or more.
[0073] In order to increase the heating rate of the amorphous alloy thin strip 12, it is also effective to heat the thin strip pressing metal (belt, roller) to the same temperature as the heating body and to heat from both sides of the thin strip. In order to suppress the heat generated by the crystallization of bccFe in the thin strip, it is also effective to set the temperature of the thin strip pressing metal (belt, roller) to be lower than the heating body temperature Ta°C.
[0074] <Attachment process>
[0075] After the heat treatment step, the nanocrystalline alloy ribbon 3 is transported to the bonding step of the adhesive layer 2. Figures 3 to 7 Provide explanation. Figure 3 , Figure 4 It is a cross-sectional view for explaining the structure of the adhesive layer 2 , and is a cross-sectional view in a direction intersecting (for example, a direction orthogonal to) the longitudinal direction of the adhesive layer 2 . Figures 5 to 7It is a cross-sectional view for explaining the structure of the magnetic sheet 100 , and is a cross-sectional view in a direction intersecting (for example, a direction perpendicular to) the longitudinal direction of the magnetic sheet 100 .
[0076] A cross-sectional view showing the structure of the adhesive layer 2 is shown in Figure 3 . The adhesive layer 2 includes a support 21 and an adhesive 22 respectively arranged on both sides of the support 21. More specifically, the adhesive 22 is respectively arranged on the first side 11A and the second side 11B of the support 21 in a film or layer form. Then, a protective sheet 4 is attached to the adhesive 22 on the first side 11A of the support 21 in the adhesive layer 2, and a pad 6 is attached to the adhesive 22 on the second side 11B of the support 21. It should be noted that the support 21 is a film member formed in a long strip shape, for example, a film member formed in a rectangular shape. The support 21 is formed using a flexible resin material. As the resin material, polyethylene terephthalate (PET: Polyethyleneterephthalate) can be used. For example, a pressure-sensitive adhesive can be used for the adhesive 22. For example, well-known adhesives such as acrylic adhesives, silicone adhesives, polyurethane adhesives, synthetic rubbers, and natural rubbers can be used as the adhesive 22. Acrylic adhesives are preferred as the adhesive 22 because they are excellent in heat resistance and moisture resistance and can adhere to a wide range of materials.
[0077] For example, the adhesive layer 2 may have a total thickness of 3 μm, including the adhesive 22 on the first surface 11A of the support 21 , the support 21 , and the adhesive 22 on the second surface 11B of the support 21 .
[0078] By removing at least one of the protective sheet 4 and the liner 6 attached to the adhesive layer 2 , the adhesive layer 2 can be attached to another member.
[0079] like Figure 1 As shown, the adhesive layer 2 is unwound from the roll 72 on which the adhesive layer 2 is wound, and the protective sheet 4 on the adhesive 22 mounted on the first surface 11A of the support 21 in the adhesive layer 2 is peeled off to expose the adhesive 22 on the first surface 11A. Figure 4 Then, the adhesive layer 2 and the nanocrystalline alloy ribbon 3 with the adhesive 22 exposed on the first surface 11A are respectively conveyed and guided to the attaching roller 71. Then, the adhesive layer 2 and the nanocrystalline alloy ribbon 3 with the adhesive 22 exposed on the first surface 11A are attached using the attaching roller 71. Figure 5 Indicates the state of adhesion. At this time, the adhesive layer 2 is conveyed with tension applied thereto, and the nanocrystalline alloy ribbon 3 is also conveyed with tension applied thereto. Furthermore, the adhesive layer 2 and the nanocrystalline alloy ribbon 3 are adhered to each other.
[0080] In addition, the nanocrystalline alloy ribbon 3 passes through the ribbon end surface arrangement device 61 before being guided to the attachment roller 71, and then passes through the ribbon end surface detection unit 62, and after the ribbon end surface of the nanocrystalline alloy ribbon 3 is adjusted, it is attached to the adhesive layer 2. Thus, the positional relationship between the nanocrystalline alloy ribbon 3 and the adhesive layer 2 is adjusted, and then attached.
[0081] The strip end surface aligning device 61 includes a mechanism for moving and aligning the nanocrystalline alloy strips 3 so as to be inclined in the width direction.
[0082] Through the attaching process performed by the attaching roller 71, as Figure 5 As shown, a magnetic sheet 100 composed of a nanocrystalline alloy thin strip 3 with an adhesive layer 2 attached to one surface can be produced. Figure 1 In the process, the magnetic sheet 100 to which the nanocrystalline alloy ribbon 3 and the adhesive layer 2 are attached is transported to the cracking process performed by the cracking roller 81. Alternatively, after the nanocrystalline alloy ribbon 3 and the adhesive layer 2 are attached, the magnetic sheet 100 may be wound into a coil without performing the cracking process. In addition, the magnetic sheet 100 may be cut into a desired length.
[0083] Figure 1 The magnetic sheet 100 shown includes a layer of nanocrystalline alloy thin strip 3. It is also possible to use a plurality of such magnetic sheets 100 and stack them to produce a magnetic sheet stacked with nanocrystalline alloy thin strips 3. In this case, the liner 6 of the magnetic sheet 100 can be peeled off, and another nanocrystalline alloy thin strip 3 can be attached and stacked to form a magnetic sheet stacked with multiple layers of nanocrystalline alloy thin strips 3.
[0084] Figure 7 The positional relationship between the nanocrystalline alloy thin strip 3 and the adhesive layer 2 in the magnetic sheet 100 according to one embodiment of the present disclosure is shown. The nanocrystalline alloy thin strip 3 and the adhesive layer 2 preferably have a shape that satisfies the relationship shown in the following formula (see Figure 7 ).
[0085] 0.2mm≤(width A-width B)≤3mm
[0086] Width A is a dimension related to the adhesive layer 2, and more preferably a dimension related to the region of the adhesive layer 2 where the adhesive 22 for bonding the nanocrystalline alloy thin strip 3 is provided. Width B is a dimension related to the nanocrystalline alloy thin strip 3. It should be noted that, when the adhesive 22 is provided on the entire surface of the support 21 of the adhesive layer 2, width A is a dimension related to the adhesive layer 2 or the support 21.
[0087] Here, the lower limit of (width A-width B) is preferably 0.5 mm, and more preferably 1.0 mm. In addition, the upper limit of (width A-width B) is preferably 2.5 mm, and more preferably 2.0 mm.
[0088] The nanocrystalline alloy thin strip 3 may be arranged with the adhesive layer 2 in the width direction with the center aligned, or may be arranged with the center separated. In this case, the relationship of 0 mm < gap a and 0 mm < gap b is satisfied (see Figure 7 ) method.
[0089] The gap a and the gap b are the distances from the end of the adhesive layer 2 to the end of the nanocrystalline alloy thin strip 3. Specifically, the gap a is the distance from the first adhesive layer end 10X of the adhesive layer 2 to the first thin strip end 20X of the nanocrystalline alloy thin strip 3. The gap b is the distance from the second adhesive layer end 10Y of the adhesive layer 2 to the second thin strip end 20Y of the nanocrystalline alloy thin strip 3.
[0090] The first thin strip end 20X is the end on the same side as the first adhesive layer end 10X in the nanocrystalline alloy thin strip 3. The second adhesive layer end 10Y is the end on the opposite side of the first adhesive layer end 10X of the adhesive layer 2. The second thin strip end 20Y is the end on the same side as the second adhesive layer end 10Y in the nanocrystalline alloy thin strip 3.
[0091] The width A, the width B, the gap a, and the gap b are dimensions in a direction intersecting, more preferably orthogonal to, the length direction of the magnetic sheet 100. The length direction of the magnetic sheet 100 is the same as the length direction of the adhesive layer 2. In addition, the length direction of the magnetic sheet 100 is the same as the length direction of the nanocrystalline alloy strip 3.
[0092] By making the width A of the region in the adhesive layer 2 where the adhesive 22 is provided wider than the width B of the nanocrystalline alloy strip 3, when the nanocrystalline alloy strip 3 is attached to the adhesive layer 2, even if the adhesive layer 2 and the nanocrystalline alloy strip 3 meander, the adhesive 22 of the adhesive layer 2 can be easily arranged on the entire surface of the nanocrystalline alloy strip 3. By arranging the adhesive layer 2 on the entire surface of the nanocrystalline alloy strip 3, it is possible to prevent the cracks 5 from being formed in the nanocrystalline alloy strip 3 and the small pieces from falling off after being formed.
[0093] By setting the value obtained by subtracting the width B from the width A to be greater than 0.2 mm, it is easy to prevent the nanocrystalline alloy strip 3 from having a portion where the adhesive 22 is not arranged when the nanocrystalline alloy strip 3 is attached to the adhesive layer 2. By setting the value obtained by subtracting the width B from the width A to be less than 3 mm, it is easy to prevent the portion where the nanocrystalline alloy strip 3 is not arranged in the magnetic sheet 100 from becoming larger. In addition, when the magnetic sheets 100 are arranged in parallel, it is easy to prevent the interval (magnetic gap) between the nanocrystalline alloy strips 3 from becoming larger.
[0094] By satisfying the relationship of 0 mm < gap a and 0 mm < gap b, when the nanocrystalline alloy strip 3 is attached to the adhesive layer 2, the nanocrystalline alloy strip 3 can be prevented from protruding from the area where the adhesive 22 is provided. Therefore, it is easy to prevent the generation of a portion where the adhesive 22 is not provided in the nanocrystalline alloy strip 3. Thus, it is possible to prevent the nanocrystalline alloy strip 3 from falling off after cracks are formed and small pieces are formed.
[0095] Furthermore, when the magnetic sheet 100 is attached to another material, the adhesive layer 2 is completely present between the nanocrystalline alloy strip 3 and another nanocrystalline alloy strip 3 or another material, and insulation and adhesion can be ensured.
[0096] <Cracking process>
[0097] After the attaching step, a cracking step is preferably performed.
[0098] exist Figure 1 In one embodiment of the present disclosure shown, after the adhesive layer 2 is attached to one surface of the nanocrystalline alloy ribbon 3 by the attachment roller 71 , the nanocrystalline alloy ribbon 3 is conveyed to a cracking process performed by a cleavage roller 81 .
[0099] In the cracking process, the cleavage roller 81 is pressed against the nanocrystalline alloy ribbon 3 to form cracks 5 in the nanocrystalline alloy ribbon 3. The cleavage roller 81 has a predetermined convex portion on the surface. Through the convex portion, an external force is directly applied to the nanocrystalline alloy ribbon 3 to form cracks 5 in the nanocrystalline alloy ribbon 3. Since the cleavage roller 81 is directly in contact with the nanocrystalline alloy ribbon 3, the cracks 5 can be easily formed. A pressing roller is provided on the adhesive layer 2 side of the nanocrystalline alloy ribbon 3. A cross-sectional view showing a structure in which cracks 5 are formed is shown in FIG. Figure 6 .
[0100] After the cracking step, the magnetic sheet 100 is passed through the nip roller unit 82 and the flattening roller unit 83 and is wound up in the roll body 9 .
[0101] The process performed by the flattening roller unit 83 is a process of clamping the magnetic sheet 100 with rollers to flatten the uneven state generated in the magnetic sheet 100 by the cracking process. That is, the process performed by the flattening roller unit 83 is to pass the magnetic sheet 100 between rollers set with a predetermined pressure. The predetermined pressure is preferably 0.1 to 1.0 MPa.
[0102] One embodiment of the present disclosure is a method for manufacturing a magnetic sheet 100 having an adhesive layer 2 attached to one surface of a nanocrystalline alloy ribbon 3, wherein a coiled amorphous alloy ribbon 12 for the nanocrystalline alloy ribbon 3 is prepared, the amorphous alloy ribbon 12 is unrolled from the coiled roll 11, and a heat treatment process and an attachment process are continuously performed on the amorphous alloy ribbon 12. In the past, after heat treatment, the nanocrystalline alloy ribbon was wound into a coiled roll, the nanocrystalline alloy ribbon was unrolled from the roll, and an adhesive layer was attached to the nanocrystalline alloy ribbon. In contrast, according to an embodiment of the present disclosure, the heat treatment process and the attachment process are performed in one unrolling.
[0103] Therefore, according to one embodiment of the present disclosure, the number of times of winding and unwinding can be reduced, and a method for producing a magnetic sheet with high productivity can be obtained.
[0104] In addition, if Figure 1 As shown in one embodiment of the present disclosure, by providing a cracking process, such as Figure 6 As shown, it is possible to manufacture the magnetic sheet 100 composed of the nanocrystalline alloy ribbon 3 having the adhesive layer 2 attached to one surface and the cracks 5 formed thereon. Thus, it is possible to obtain a method for manufacturing the magnetic sheet 100 with high productivity.
[0105] In one embodiment of the present disclosure, in the heat treatment process, the amorphous alloy thin strip 12 is sandwiched between a heating body and a thin strip pressing member for heating. In addition, the amorphous alloy thin strip 12 is heated while being pressed against the heating body by a thin strip pressing member that contacts the opposite surface of the surface of the amorphous alloy thin strip 12 that contacts the heating body. In this way, by heating in a state where the amorphous alloy thin strip 12 is sandwiched and pressed, the amorphous alloy thin strip 12 can be heated uniformly. Thus, a nanocrystalline alloy thin strip 3 with excellent magnetic properties can be obtained.
[0106] Furthermore, according to this heat treatment, by heating in a state where the amorphous alloy ribbon 12 is sandwiched and pressed, it is possible to obtain a nanocrystalline alloy ribbon 3 having excellent isotropy.
[0107] For example, it is preferable that the magnetic flux density B80 when a magnetic field of 80 A / m is applied in the length direction of the magnetic sheet 100 made of the nanocrystalline alloy thin strip 3 of the present disclosure is L The magnetic flux density B80 when a magnetic field of 80A / m is applied in the width direction perpendicular to the length direction W Ratio (B80 L / B80 W ) is 0.60~1.40, and B80 L 、B80 W All are above 0.1T. L / B80 W) is more preferably 0.70 to 1.30. L 、B80 W Both are more preferably 0.4 T or more, and more preferably 0.5 T or more.
[0108] In addition, according to the heat treatment disclosed in the present invention, the generation of wrinkles or streaks can be suppressed by setting the state of clamping and pressing the amorphous alloy thin strip 12. Furthermore, it also has the effect of correcting wrinkles and the like generated by cooling deviation when casting the amorphous alloy thin strip 12. Therefore, according to the present invention, wrinkles or streaks can be suppressed, and a nanocrystalline alloy thin strip 3 with good flatness can be obtained.
[0109] In addition, the nanocrystalline alloy ribbon 3 of the present disclosure is preferably composed of the composition formula (Fe 1-x A x ) a Si b B c Cu d M e It means that A is at least one of Ni and Co, M is at least one element selected from Nb, Mo, V, Zr, Hf and W, and in terms of atomic %, 72.0≤a≤81.0, 9.0≤b≤18.0, 5.0≤c≤10.0, 0.02≤d≤1.5, 0.1≤e≤3.5, and 0≤x≤0.1.
[0110] In addition, during the heat treatment disclosed in the present invention, when the bccFe crystallization start temperature of the amorphous alloy strip 12 measured at a heating rate of 20 K / min is set to Tx1°C, the above-mentioned heating body is preferably heated to a heating temperature Ta of not less than Tx1+80°C and not more than Tx1+230°C.
[0111] The thickness of the nanocrystalline alloy ribbon 3 disclosed in the present invention is preferably 25 μm or less, more preferably 20 μm or less. In addition, the thickness is preferably 5 μm or more, more preferably 10 μm or more. The width of the nanocrystalline alloy ribbon 3 disclosed in the present invention is preferably 10 mm or more, more preferably 30 mm or more, and further preferably 50 mm or more.
[0112] In addition, if the width of the nanocrystalline alloy ribbon 3 of the present disclosure is too wide, it is difficult to achieve stable production, so the width is preferably 500 mm or less, and more preferably 400 mm or less.
[0113] In addition, the saturation magnetic flux density Bs of the nanocrystalline alloy ribbon 3 of the present disclosure is preferably 1.15 T or more. Furthermore, the saturation magnetic flux density Bs is preferably 1.20 T or more, more preferably 1.35 T or more, more preferably 1.36 T or more, more preferably 1.37 T or more, and more preferably 1.40 T or more.
[0114] [Example 1]
[0115] The alloy composition becomes Fe 76.8 Si 14.0 B 8.0 Cu 0.7 Nb 0.5 The element source is combined in a manner, heated to 1350°C to produce an alloy melt, and the alloy melt is ejected onto a cooling roller with an outer diameter of 400 mm and a width of 200 mm rotating at a peripheral speed of 30 m / sec, and rapidly solidified on the cooling roller to produce an amorphous alloy thin strip 12. It should be noted that the outer periphery of the cooling roller is composed of a Cu alloy with a thermal conductivity of 150 W / (m·K), and a cooling mechanism for controlling the temperature of the outer periphery is provided inside.
[0116] The amorphous alloy ribbon 12 has a width of 50 mm and a thickness of 16.4 μm.
[0117] The amorphous alloy thin strip 12 is wound up to form a coiled body 11 .
[0118] The roll 11 of the amorphous alloy thin strip 12 is used by Figure 1 The magnetic sheet 100 is produced by the steps shown. At this time, the cracking step is not performed until the adhesive layer 2 is attached to the nanocrystalline alloy ribbon 3 .
[0119] The amorphous alloy thin strip 12 was introduced into the heating roller 16 with the tension being set to 3.1 MPa, 5.0 MPa, 6.3 MPa, 12.5 MPa, 15.0 MPa, and 17.5 MPa.
[0120] At this time, the heating roller 16 is heated to 660° C., the conveying speed of the thin strip 12 is set to 50 mm / sec, the contact time between the thin strip 12 and the heating roller 16 is set to 1.2 seconds, and the pressure of the thin strip 12 pressed against the heating roller 16 by the thin strip pressing member is set to 0.115 MPa.
[0121] The adhesive layer 2 has a thickness of 3 μm (adhesive 22 on the first surface 11A of the support 21 + support 21 + adhesive 22 on the second surface 11B of the support 21). A magnetic sheet 100 having one layer of nanocrystalline alloy thin strips 3 is prepared, and five of the magnetic sheets 100 are stacked to prepare a magnetic sheet having five layers of nanocrystalline alloy thin strips 3.
[0122] In addition, similarly, using Figure 1 The cracking step shown above was performed to produce a cracked magnetic sheet 100. Five cracked magnetic sheets 100 were stacked to produce a magnetic sheet having five layers of nanocrystalline alloy thin strips 3. The properties of the five-layer magnetic sheet were evaluated. The evaluation results are shown in Table 1.
[0123] As shown in Table 1, in order to obtain a high saturation magnetic flux density Bs, it is preferred that the tension of the amorphous alloy thin strip 12 be set to 17 MPa or less. L / B80 W The tension of the amorphous alloy strip 12 is preferably set to 3.5 MPa or more, and more preferably set to 5.5 MPa or more.
[0124] [Table 1]
[0125]
[0126] [Saturation magnetic flux density Bs]
[0127] In a DC magnetization characteristic test device manufactured by Metron Technology Co., Ltd., a single plate sample of the heat-treated nanocrystalline alloy thin strip 3 was subjected to a magnetic field of 8000 A / m, and the maximum magnetic flux density at this time was measured as Bs. The nanocrystalline alloy thin strip 3 disclosed in the present invention has the characteristic of being easy to saturate, so it reaches saturation when the 8000 A / m magnetic field is applied, and Bs is 8000 The saturation magnetic flux density Bs is approximately the same value, so the saturation magnetic flux density Bs is expressed as B 8000 express.
[0128] [Magnetic flux density B80]
[0129] In a DC magnetization characteristic test device manufactured by Metron Giken Co., Ltd., a magnetic field of 80 A / m was applied in the longitudinal direction (i.e., casting direction) and in the width direction perpendicular to the longitudinal direction of the magnetic sheet, and the maximum magnetic flux density at this time was set as B80 L 、B80 W , calculate the ratio B80 L / B80 W , for isotropic evaluation.
[0130] [Average grain size]
[0131] The average crystal grain size is obtained by the Scherrer formula using the integral width of the diffraction peak from the (110) plane in the X-ray diffraction pattern obtained by the X-ray diffraction experiment. The integral width of the diffraction peak from the (110) plane is obtained by peak decomposition using the pseudo-Voigt function for the diffraction pattern. If the average grain size is set to D, the integral width is set to β, the diffraction angle is set to θ, the Scherrer constant is set to K, and the wavelength of the X-ray is set to λ, then D is obtained according to the Scherrer formula (Formula 1) given below. However, in this case, it is assumed that the wavelength of the X-ray is λ = 0.154050nm and the Scherrer constant K = 1.333. In addition, the integral width uses a value corrected in a manner that the integral width is narrowed by the expansion amount of the diffraction line width from the device.
[0132] [Number 1]
[0133]
[0134] [Volume rate]
[0135] The volume ratio is the volume ratio of the nanocrystals, and the portion other than the nanocrystals is an amorphous portion.
[0136] The volume fraction is calculated by the ratio of the integrated intensity of the diffraction peak from the (110) plane of Fe to the integrated intensity of the halo pattern. The integrated intensity of the halo pattern is the integrated intensity of the diffraction peak from the (110) plane of Fe + the integrated intensity near 2θ=44°. The integrated intensity of the peak shown by the nanocrystal and the halo pattern shown by the amorphous are calculated by peak decomposition using the pseudo-Voigt function for the X-ray diffraction pattern. When the integrated intensity of the (110) peak of the nanocrystal is set to Ic and the integrated intensity of the halo pattern near 2θ=44° is set to Ia, the volume fraction V is calculated by the formula (number 2) given below. However, in the case of the composition of this embodiment, Fe and Fe 2 The peaks of the integrated intensity of B overlap and are difficult to resolve, so trace amounts of precipitated Fe may also be included in Ic and Ia. 2 The integrated intensity of B.
[0137] [Number 2]
[0138]
[0139] According to the embodiments of the present disclosure, a method for manufacturing a magnetic sheet with high productivity and reduced number of unwinding and winding is obtained. In addition, a magnetic sheet having a nanocrystalline alloy ribbon having excellent magnetic properties and good isotropy can be manufactured. For example, a nanocrystalline alloy ribbon with a Bs of 1.15T or more can be obtained. In addition, a B80 L 、B80 W All of them are above 0.10T. In addition, according to the present disclosure, a magnetic sheet having good isotropic properties is obtained. In addition, a magnetic sheet having a strength of B80 L / B80 W The magnetic sheet was in the range of 0.60 to 1.40. In addition, a magnetic sheet having a low coercive force Hc and excellent magnetic properties was obtained.
[0140] In addition, in the present disclosure, a nanocrystalline alloy ribbon having a structure in which crystal grains having an average crystal grain size of 50 nm or less are present in an amorphous phase is obtained.
Claims
1. A method for manufacturing a magnetic sheet, comprising: a heat treatment step of heat-treating an amorphous alloy ribbon to produce a nanocrystalline alloy ribbon, and a bonding step of bonding an adhesive layer to one surface of the nanocrystalline alloy ribbon. In the heat treatment step, the amorphous alloy thin strip is unwound from the amorphous alloy thin strip wound into a coil shape, the amorphous alloy thin strip is brought into contact with a heating body while being conveyed, a thin strip pressing member is brought into contact with a surface of the amorphous alloy thin strip opposite to a surface of the amorphous alloy thin strip in contact with the heating body, thereby heating the amorphous alloy thin strip while being pressed against the heating body, applying a tension of 18 MPa or less to the amorphous alloy thin strip and introducing it into the heating body, In the attaching step, the adhesive layer is attached to the one surface of the nanocrystalline alloy ribbon while the nanocrystalline alloy ribbon delivered from the heat treatment step is delivered.
2. According to the manufacturing method of the magnetic sheet described in claim 1, a cracking process is provided after the attaching process, that is: while conveying the nanocrystalline alloy strip, a cracking roller is brought into direct contact with the opposite side of the one side of the nanocrystalline alloy strip, and the opposite side of the nanocrystalline alloy strip is pressurized by the cracking roller to form cracks in the nanocrystalline alloy strip. 3 . The method for producing a magnetic sheet according to claim 1 , wherein after the attaching step, the magnetic sheet is wound into a coil shape. 4 . The method for producing a magnetic sheet according to claim 2 , wherein after the cracking step, the magnetic sheet is wound into a coil shape. 5 . The method for producing a magnetic sheet according to claim 1 , wherein when the amorphous alloy thin ribbon is brought into contact with the heating body for heating, a heating rate of the amorphous alloy thin ribbon is 50° C. / sec to 4000° C. / sec. 6 . The method for producing a magnetic sheet according to claim 1 , wherein the contact time between the amorphous alloy ribbon and the heating body is 0.1 to 30 seconds. 7 . The method for producing a magnetic sheet according to claim 1 , wherein the nanocrystalline alloy ribbon has a structure in which crystal grains having an average crystal grain size of 50 nm or less exist in an amorphous phase.
8. The method for producing a magnetic sheet according to any one of claims 1 to 7, wherein the adhesive layer comprises a support body formed in a belt shape and an adhesive provided on both surfaces of the support body, When the dimension related to the adhesive layer and the dimension in the direction intersecting the length direction of the adhesive layer is defined as width A, and the dimension related to the nanocrystalline alloy strip and the dimension in the direction intersecting the length direction of the nanocrystalline alloy strip is defined as width B, The relationship of 0.2 mm ≤ (width A - width B) ≤ 3 mm is satisfied. 9 . The method for producing a magnetic sheet according to claim 1 , further comprising a device for aligning the end faces of the nanocrystalline alloy ribbon before attaching the adhesive layer to the nanocrystalline alloy ribbon.
10. The method for producing a magnetic sheet according to any one of claims 1 to 9, wherein the nanocrystalline alloy ribbon has a composition formula (Fe 1-x A x ) a Si b B c Cu d M e It means that A is at least one of Ni and Co, M is at least one selected from Nb, Mo, V, Zr, Hf and W, and in atomic %, 72.0≤a≤81.0, 9.0≤b≤18.0, 5.0≤c≤10.0, 0.02≤d≤1.5, 0.1≤e≤3.5, and 0≤x≤0.
1.
11. The method for manufacturing a magnetic sheet according to any one of claims 1 to 10, wherein when the bccFe crystallization start temperature of the amorphous alloy ribbon measured at a heating rate of 20 K / min is set to Tx1°C, the heating body is heated to a heating temperature Ta of not less than Tx1+80°C and not more than Tx1+230°C. 12 . The method for producing a magnetic sheet according to claim 1 , wherein the pressure at which the amorphous alloy ribbon is pressed against the heating body is 0.03 MPa or more. 13 . The method for producing a magnetic sheet according to claim 1 , wherein the nanocrystalline alloy ribbon has a saturation magnetic flux density Bs of 1.15 T or more.
14. The method for producing a magnetic sheet according to any one of claims 1 to 13, wherein a magnetic flux density B80 when a magnetic field of 80 A / m is applied along the longitudinal direction of the magnetic sheet is L The magnetic flux density B80 when a magnetic field of 80 A / m is applied along the width direction orthogonal to the length direction W The ratio of B80 L / B80 W 0.60~1.40, and B80 L 、B80 W All are above 0.1T.
Citation Information
Cited By
Preparation method of short-process nanocrystalline magnetism isolating material
CN119446701A
Distributed air gap iron core for high-frequency transformer and preparation method of distributed air gap iron core
CN121726220A
A distributed air gap core for a high frequency transformer and a method of manufacturing the same
CN121726220B