Inorganic super-ionic conductor material and preparation method and application thereof

By doping metal cations and non-metal anions in apatite, high-performance sheet-shaped inorganic superion conductor materials are prepared, which solves the pore problem of inorganic solid electrolytes in lithium-ion batteries and improves the cycle time and safety of the batteries , meets high energy density and safety requirements.

CN118978138APending Publication Date: 2024-11-19BEIJING UNIV OF CHEM TECH +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411044997.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The inorganic solid electrolytes of existing lithium-ion batteries have many pores after tableting, resulting in a decrease in ionic conductivity and short-circuit risk. The ionic conductivity and flame retardant properties of the composite solid electrolyte are poor, which cannot meet high energy density and safety. need.

Method used

Apatite is used as the basic material, and metal cations and non-metal anions are doped by solid phase sintering to prepare sheet-like inorganic superion conductor materials for the preparation of inorganic or composite solid electrolytes with high ionic conductivity and mechanical strength.

Benefits of technology

It improves the battery cycle time, low overpotential, high capacity retention rate, excellent reversible capacity, and has flame retardant characteristics and air thermal stability, making it suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978138A_ABST
    Figure CN118978138A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of secondary batteries, and discloses an inorganic super-ion conductor material and a preparation method and application thereof. The inorganic super-ion conductor material comprises apatite and doped ions doped in the apatite; wherein the doped ions comprise metal cations and non-metal anions; the inorganic super-ion conductor material is in a sheet shape. The inorganic super-ion conductor material is obtained through a solid-phase sintering method. The inorganic super-ion conductor material can be used as an inorganic solid electrolyte membrane or a composite solid electrolyte membrane in a lithium battery and other secondary batteries. The inorganic super-ion conductor material provided by the invention is sheet-shaped and can be better subjected to secondary processing to prepare various forms of solid electrolyte materials such as ceramic chips, clay, composite materials and the like, and meanwhile, the sheet-shaped hydroxyapatite is higher in mechanical strength and more stable in property and has a flame-retardant characteristic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to an inorganic superionic conductor material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have attracted wide attention and applications due to their high energy density, light weight, and low self-discharge rate. With the rapid development of the mobile device market, such as the popularity of mobile phones and laptops, the demand for lithium-ion batteries has increased dramatically. At the same time, electric vehicles, energy storage systems and other fields have also begun to use lithium-ion batteries as the main energy storage solution. Lithium-ion batteries still need to be continuously improved and innovated with the goal of continuously improving their performance in terms of energy density, safety, and cycle life.

[0003] At present, most commercial lithium-ion batteries use graphite based on intercalation reactions, which have good cycle life, but have the problem of low energy density. They are not suitable for some applications that require longer driving range or higher energy density, and cannot meet the needs of lithium-ion batteries for further development in higher fields such as new energy vehicles and aerospace. Lithium metal has a high theoretical specific capacity (3860mAh g -1 ) and extremely low reduction potential (-3.04V vs. standard hydrogen electrode) make it the best choice for the negative electrode of future energy storage systems. Secondary batteries with lithium metal as the negative electrode have high specific energy (>500Wh kg -1 ) and high energy density (>1500Wh L -1 ). However, the use of volatile, flammable electrolytes will continue to react with metallic lithium, consuming the electrolyte and metallic lithium. The resulting lithium dendrites may cause battery short circuits and safety risks such as overheating, fire or explosion.

[0004] Compared with traditional liquid electrolytes, solid electrolytes are not only safer, but also more resistant to high temperatures, greatly reducing the possibility of safety hazards such as short circuits and thermal runaway in batteries. In addition, solid electrolytes also provide new possibilities for metallic lithium to be used as the negative electrode of batteries, avoiding the safety risks brought about by the formation of lithium dendrites in traditional electrolytes, thereby improving the cycle life and stability of batteries. At the same time, the application of solid electrolytes makes it possible to use metallic lithium as the negative electrode of batteries, opening up a new path for improving the energy density of batteries and further promoting the development of electric vehicles and other fields.

[0005] Solid electrolytes are divided into inorganic solid electrolytes, polymer solid electrolytes and composite solid electrolytes. Inorganic solid electrolytes have high ionic conductivity (some can reach 10 -3 S cm -1) high mechanical strength. However, due to process problems, most inorganic solid electrolytes, especially oxide solid electrolytes, still have many pores after tableting, which not only reduces the ionic conductivity, but also makes it very easy to short-circuit during the charge and discharge process due to dendrite growth, resulting in low yield; polymer solid electrolytes have high flexibility and good interface contact with electrodes, but the disadvantage is that the ionic conductivity is low and it can hardly work at room temperature; composite solid electrolytes combine the advantages of inorganic and polymer solid electrolytes, and have high ionic conductivity, high mechanical strength, high flexibility and good interface contact with electrodes.

[0006] Nowadays, most common inorganic solid electrolytes for lithium-ion batteries are oxides and sulfides. Among them, oxides are mainly perovskite (LLTO) and garnet (LLZO). This type of solid electrolyte has good thermal stability, wide electrochemical window, high mechanical strength, but average conductivity (higher than polymers and lower than sulfides, most of which are below 10 -4 S cm -1 About), it is brittle and difficult to process, and has a poor contact interface; sulfides, by comparison, have high conductivity and are easier to process into compact solid electrolyte ceramic sheets because of their soft texture. Sulfides are highly active and toxic, requiring argon atmosphere protection throughout the process, and the process is complex and has a low yield, making them only suitable for laboratory-scale preparation.

[0007] Although traditional composite solid electrolytes have solved the problems of interface impedance and low ion conductivity to a certain extent, the ion conductivity of most composite solid electrolytes can only reach 10 -5 S / cm, and its flame retardancy and air stability are also poor. Summary of the invention

[0008] The purpose of the present invention is to overcome the problems existing in the prior art and to provide an inorganic superionic conductor material and a preparation method and application thereof.

[0009] In order to achieve the above-mentioned object, the first aspect of the present invention provides an inorganic superionic conductor material, wherein the inorganic superionic conductor material comprises apatite and doping ions doped in the apatite;

[0010] Wherein, the doping ions include metal cations and non-metal anions;

[0011] The inorganic superionic conductor material has a flake shape.

[0012] The second aspect of the present invention provides a method for preparing the inorganic superionic conductor material according to the first aspect, wherein the method is a solid phase sintering method, comprising the following steps:

[0013] (1) mixing hydroxyapatite powder, metal cation salt powder and a dispersant to obtain a precursor powder, and performing a solid phase reaction sintering treatment;

[0014] (2) grinding the powder after sintering in step (1), and then soaking it in water;

[0015] (3) centrifuging, washing and drying the product after soaking in step (2);

[0016] (4) Adding a non-metallic anion salt to the product obtained in step (3) for mixing, and then centrifuging, washing, and drying to obtain the inorganic superionic conductor material.

[0017] The third aspect of the present invention provides an inorganic superionic conductor material prepared by the preparation method described in the second aspect.

[0018] The fourth aspect of the present invention provides the use of the inorganic superionic conductor material described in the first aspect or the third aspect in the preparation of lithium batteries and other secondary batteries.

[0019] The fifth aspect of the present invention provides an inorganic solid electrolyte membrane made from the inorganic superionic conductor material described in the first aspect or the third aspect.

[0020] The sixth aspect of the present invention provides a method for preparing the inorganic solid electrolyte membrane described in the fifth aspect, wherein the method comprises: mixing and grinding the inorganic superionic conductor material with an acetonitrile solution of polyethylene oxide, and pressing the mixture into tablets after evaporating the acetonitrile to obtain a clay-like inorganic solid electrolyte membrane.

[0021] The seventh aspect of the present invention provides a composite solid electrolyte membrane made from the inorganic superionic conductor material described in the first aspect or the third aspect.

[0022] An eighth aspect of the present invention provides a lithium battery comprising the inorganic solid electrolyte membrane described in the fifth aspect or the composite solid electrolyte membrane described in the seventh aspect.

[0023] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0024] (1) The inorganic superionic conductor material provided by the present invention is in the form of a sheet, which can be better processed for secondary processing to prepare solid electrolyte materials in various forms such as ceramic sheets, clays, and composite materials. At the same time, the sheet-like hydroxyapatite has higher mechanical strength, more stable properties, and flame retardant properties.

[0025] (2) The inorganic superionic conductor material of the present invention can obtain higher ionic conductivity or mechanical strength when prepared into an inorganic solid electrolyte; and can have higher ionic conductivity and stability when prepared into a composite solid electrolyte.

[0026] (3) The symmetrical battery prepared from the inorganic superionic conductor material described in the present invention can obtain a longer cycle time and a lower overpotential; the prepared full battery has a high capacity retention rate, a high reversible specific capacity and excellent rate performance.

[0027] (4) The solid-phase sintering method provided by the present invention can synthesize inorganic superionic conductor materials in large quantities, and the doping amounts of metal cations and non-metallic anions can be adjusted separately to increase the doping amount of metal cations; materials with different microscopic morphologies can be obtained to meet different uses, and are suitable for large-scale industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a scanning electron microscope image of the inorganic superionic conductor material prepared in Preparation Example 1 of the present invention;

[0029] Figure 2 The XRD pattern of the inorganic superionic conductor material prepared in Example 1 of the present invention;

[0030] Figure 3 This is a scanning electron microscope image of the inorganic superionic conductor material prepared in Comparative Example 2 of the present invention;

[0031] Figure 4 This is a macroscopic photograph of a ceramic sheet prepared in Application Example 3 of the present invention;

[0032] Figure 5 The cycle performance diagram of a symmetrical battery assembled with the composite solid electrolyte membrane prepared in Application Example 1 of the present invention;

[0033] Figure 6 The charge and discharge curve diagram of a full battery assembled with the composite solid electrolyte membrane prepared in Application Example 1 of the present invention;

[0034] Figure 7 This is a rate performance diagram of a full battery assembled with the composite solid electrolyte membrane prepared in Application Example 1 of the present invention;

[0035] Figure 8 This is an electrochemical window diagram of an iron-lithium battery assembled with the composite solid electrolyte membrane prepared in Application Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0037] A first aspect of the present invention provides an inorganic superionic conductor material, characterized in that the inorganic superionic conductor material comprises apatite and doping ions doped in the apatite;

[0038] Wherein, the doping ions include hydroxide ions, metal cations and non-metal anions;

[0039] The inorganic superionic conductor material has a flake shape.

[0040] In the present invention, the inorganic superionic conductor material has a flaky morphology, and the flaky hydroxyapatite can be better processed for secondary processing to prepare solid electrolyte materials in various forms such as ceramic sheets, clays, and composite materials. At the same time, the flaky hydroxyapatite has higher mechanical strength and more stable properties.

[0041] In some embodiments of the present invention, the apatite contains hydroxide ions. The present invention can use hydroxyapatite as a raw material.

[0042] In some embodiments of the present invention, the length of the inorganic superionic conductor material is 1-20 μm, preferably 1-5 μm, or 2-10 μm, or 3-10 μm, or 8-10 μm.

[0043] In some embodiments of the present invention, the thickness of the inorganic superionic conductor material is 300 nm-2 μm, preferably 400 nm-1.2 μm, and more preferably 400-600 nm, or 1 μm.

[0044] In some embodiments of the present invention, the metal cation is selected from at least one of lithium ion, sodium ion, potassium ion, magnesium ion, zinc ion, chromium ion, aluminum ion, barium ion, chromium ion, lead ion and mercury ion, preferably lithium ion.

[0045] In some embodiments of the present invention, the non-metallic anion is selected from at least one of fluoride ion, chloride ion and bromide ion, preferably fluoride ion.

[0046] In some embodiments of the present invention, the doping amount of metal cations in the inorganic superionic conductor material is 1-8wt.%, preferably 1.9-7.68wt.%, or 4.43-5.37wt.%, or 5.21wt.%. Taking lithium ions as an example, the more lithium ions are doped, the more lithium ion channels there are in the material, and the corresponding ion conductivity will also increase, but excessive ion replacement will destroy the original crystal structure of the material, resulting in changes in its melting point / mechanical strength and other parameters, making it more difficult to process.

[0047] In some embodiments of the present invention, the doping amount of non-metallic anions in the inorganic superionic conductor material is 1-10wt.%, preferably 5-10wt.%, or 6-7wt.%. In the present invention, excessive or insufficient doping of non-metallic cations may also lead to problems such as too low ionic mechanical strength or too low conductivity.

[0048] The second aspect of the present invention provides a method for preparing the inorganic superionic conductor material according to the first aspect, wherein the method is a solid phase sintering method, comprising the following steps:

[0049] (1) mixing hydroxyapatite powder, metal cation salt powder and an optional dispersant to obtain a precursor powder, and performing a solid phase reaction sintering treatment;

[0050] (2) grinding the powder after sintering in step (1), and then soaking it in water;

[0051] (3) centrifuging, washing and drying the product after soaking in step (2);

[0052] (4) Adding a non-metallic anion salt to the product obtained in step (3) for mixing, and then centrifuging, washing, and drying to obtain the inorganic superionic conductor material.

[0053] The solid-phase sintering method described in the present invention dopes metal cations and non-metal anions into hydroxyapatite in two steps, and can accurately control the amount of doped metal cations and non-metal anions to obtain materials with different microscopic morphologies for different purposes, such as inorganic solid electrolytes or composite solid electrolytes.

[0054] In addition, the inorganic superionic conductor material prepared by the solid phase sintering method of the present invention has a higher metal cation doping amount.

[0055] The present invention can not only synthesize hydroxyapatite independently, but also extract hydroxyapatite from bones or directly use commercial hydroxyapatite products.

[0056] In some embodiments of the present invention, the metal cation salt powder in step (1) is selected from at least one of lithium carbonate, lithium nitrate, lithium sulfate, sodium carbonate, sodium sulfate, sodium nitrate, potassium carbonate, magnesium sulfate, zinc sulfate, strontium sulfate and barium carbonate, preferably lithium carbonate.

[0057] In some embodiments of the present invention, the dispersant is selected from at least one of stearic acid, sodium oleate, glutamic acid and alanine, preferably stearic acid.

[0058] In some embodiments of the present invention, the mass ratio of the hydroxyapatite powder to the metal cation salt powder is 10:0.4-8, preferably 10:2.5-4.3.

[0059] In some embodiments of the present invention, the mass ratio of the hydroxyapatite powder to the dispersant is 10:0.6-0.7.

[0060] In some embodiments of the present invention, the mixing time in step (1) is 10 min-1 h, preferably 20-30 min.

[0061] In some embodiments of the present invention, the sintering treatment in step (1) is one of muffle furnace sintering, hot pressing sintering, cold pressing sintering, microwave sintering, liquid phase sintering, and spark plasma SPS sintering, preferably muffle furnace sintering or hot pressing sintering.

[0062] In some embodiments of the present invention, the sintering temperature is 600-1200°C, preferably 800-4000°C, and more preferably 800°C or 1000°C.

[0063] In some embodiments of the present invention, the heating rate is 2-10°C / min, preferably 5°C / min.

[0064] In some embodiments of the present invention, the sintering time is 1-6 hours, preferably 2 hours.

[0065] In some embodiments of the present invention, the sintering atmosphere is one of air, oxygen, nitrogen and argon, preferably air.

[0066] In some embodiments of the present invention, the soaking time in step (2) is 8-24 hours, preferably 12 hours.

[0067] In some embodiments of the present invention, the drying conditions in step (3) include: a drying temperature of 20-80° C., preferably 60° C.; and a drying time of 6-24 h, preferably 24 h.

[0068] In some embodiments of the present invention, the non-metallic anion salt in step (4) is selected from at least one of sodium fluoride, sodium chloride, sodium bromide, potassium chloride, potassium fluoride, potassium bromide, ammonium chloride, ammonium fluoride and ammonium bromide, preferably sodium fluoride.

[0069] In some embodiments of the present invention, the mass ratio of the product obtained in step (3) to the non-metallic anion salt is 2:5-30, preferably 2:10-20.

[0070] In some embodiments of the present invention, the mixing time in step (4) is 4-24 hours, preferably 8-12 hours; the mixing temperature is 20-80°C, preferably 60°C.

[0071] In some embodiments of the present invention, the drying conditions include: a temperature of 20-100° C., preferably 40-80° C.; and a time of 4-24 h, preferably 12-16 h.

[0072] The third aspect of the present invention provides an inorganic superionic conductor material prepared by the preparation method described in the second aspect.

[0073] The fourth aspect of the present invention provides the use of the inorganic superionic conductor material described in the first aspect or the third aspect in the preparation of lithium batteries and other secondary batteries.

[0074] In some embodiments of the present invention, the inorganic superionic conductor material is used in the preparation of inorganic solid electrolytes, composite solid electrolytes, positive and negative electrode materials, separators and electrolytes.

[0075] The inorganic superionic conductor material obtained by the present invention can be directly used as an inorganic solid electrolyte, or can be added as an inorganic active filler into a polymer matrix for use as a composite solid electrolyte, added into positive and negative electrodes as a lithium-conducting active substance, as an electrolyte additive and a diaphragm, etc., and can be applied to various components of a battery to improve battery performance.

[0076] The fifth aspect of the present invention provides an inorganic solid electrolyte membrane made from the inorganic superionic conductor material described in the first aspect or the third aspect.

[0077] In some embodiments of the present invention, the inorganic solid electrolyte membrane is a ceramic sheet or a clay-like inorganic solid electrolyte membrane.

[0078] In some embodiments of the present invention, the inorganic solid electrolyte membrane is obtained by hot pressing and sintering the inorganic superionic conductor material into a sheet to obtain a ceramic sheet. After hot pressing and sintering, the inorganic superionic conductor material can obtain a ceramic sheet with extremely high strength, high ionic conductivity and relative density.

[0079] The sixth aspect of the present invention provides a method for preparing the inorganic solid electrolyte membrane described in the fifth aspect, wherein the method comprises: mixing and grinding the inorganic superionic conductor material with an acetonitrile solution of polyethylene oxide, and pressing the mixture into tablets after evaporating the acetonitrile to obtain a clay-like inorganic solid electrolyte membrane.

[0080] The method solves the problem of stratification and uneven distribution of inorganic fillers in polymers by wet-grinding inorganic superionic conductor materials with a small amount of polymer (polyethylene oxide). In addition, the clay prepared by this method can be arbitrarily plastic and can be prepared into solid electrolyte membranes of any shape for application in different scenarios.

[0081] In some embodiments of the present invention, the mass ratio of the inorganic superionic conductor material to polyethylene oxide is 3-9:1, preferably 4:1.

[0082] The seventh aspect of the present invention provides a composite solid electrolyte membrane made of the inorganic superionic conductor material described in the first aspect or the third aspect, which has higher ion conductivity, and the symmetrical battery prepared therefrom has a longer cycle time and a lower overpotential.

[0083] In some embodiments of the present invention, the composite solid electrolyte membrane is prepared by mixing the inorganic superionic conductor material with an acetonitrile solution of polyethylene oxide and then drying the mixture.

[0084] In some embodiments of the present invention, the mass ratio of the inorganic superionic conductor material to polyethylene oxide is 1:3-9, preferably 1:4.

[0085] An eighth aspect of the present invention provides a lithium battery comprising the inorganic solid electrolyte membrane described in the fifth aspect or the composite solid electrolyte membrane described in the seventh aspect.

[0086] The present invention will be described in detail below through examples.

[0087] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0088] Preparation Example 1

[0089] Weigh 1.4 g of commercial nano-needle hydroxyapatite, 0.6 g of lithium carbonate and 0.1 g of stearic acid and grind them in a mortar for 20 min; put the evenly mixed sample into a tubular furnace, and heat it to 800 ° C at a heating rate of 5 ° C / min in an air atmosphere and keep it for 2 h. After cooling the reaction product, grind it into powder in a mortar, wash it with water and then disperse it in water; add 2 g of sodium fluoride and 200 ml of water to 0.4 g of the product, stir at 60 ° C for 6 h, wash it with water, centrifuge it, and dry it for 12 h to obtain an inorganic superionic conductor material.

[0090] The scanning electron microscope image is as follows Figure 1 As shown, it is a regularly shaped flake structure with a length of 1-5 μm and a thickness of 400-600 nm.

[0091] Its XRD pattern is as follows Figure 2 As shown, it can be seen that the material contains hydroxyapatite.

[0092] ICP test shows that the doping amount of lithium ions in the inorganic superionic conductor material is 7.68wt.%, and XPS test shows that the doping amount of fluorine ions is about 7wt.%.

[0093] Preparation Example 2

[0094] The operating conditions were the same as those in Preparation Example 1, except that lithium carbonate was used instead of lithium sulfate.

[0095] Similar to Example 1, the material is a regular flake material with a length of 1-5 μm and a thickness of 400-600 nm.

[0096] ICP test shows that the doping amount of lithium ions in the inorganic superionic conductor material is 5.37wt.%; XPS test shows that the doping amount of fluorine ions is about 7wt.%.

[0097] Preparation Example 3

[0098] Weigh 20 g of commercial nano-needle hydroxyapatite, 5 g of lithium carbonate and 1.25 g of stearic acid and grind them in a mortar for 20 min; put the evenly mixed sample into a tubular furnace, and heat it to 1000 ° C at a heating rate of 5 ° C / min in an air atmosphere and keep it for 2 h. After cooling the reaction product, grind it into powder in a mortar, wash it with water and then disperse it in water; add 2 g of sodium fluoride and 200 ml of water to 0.4 g of the product, stir at 60 ° C for 6 h, wash it with water, centrifuge it, and dry it for 12 h to obtain an inorganic superionic conductor material.

[0099] The material is a regular sheet material with a length of 3-10 μm and a thickness of about 1 μm. It is larger than the sheet in Preparation Example 1 and is suitable for use as an inorganic solid electrolyte membrane.

[0100] ICP test shows that the doping amount of lithium ions in the inorganic superionic conductor material is 5.21wt.%, and XPS test shows that the doping amount of fluorine ions is about 6wt.%.

[0101] Preparation Example 4

[0102] The operating conditions were the same as those in Preparation Example 3, except that lithium carbonate was used instead of lithium sulfate.

[0103] Similar to Example 3, the material is a regular sheet material with a length of 3-10 μm and a thickness of about 1.2 μm.

[0104] ICP test shows that the doping amount of lithium ions in the inorganic superionic conductor material is 4.43wt.%; XPS test shows that the doping amount of fluorine ions is about 6wt.%.

[0105] Preparation Example 5

[0106] Weigh 1.4 g of commercial nano-needle hydroxyapatite, 0.6 g of lithium carbonate and 0.1 g of stearic acid and grind them in a mortar for 20 min; put the evenly mixed sample into a mold, and hot-press and sinter for 30 min at a pressure of 10 MPa and a temperature of 800°C. After cooling the reaction product, grind it into powder in a mortar, wash it with water and then disperse it in water; add 2 g of sodium fluoride and 200 ml of water to 0.4 g of the product, stir it at 60°C for 6 h, wash it with water, centrifuge it, and dry it for 12 h to obtain an inorganic superionic conductor material.

[0107] The material is a regular sheet material with a length of 8-10 μm and a thickness of 1.2 μm. Compared with the sheet in Preparation Example 4, it is larger and suitable for use as an inorganic solid electrolyte membrane.

[0108] ICP test shows that the doping amount of lithium ions in the inorganic superionic conductor material is 1.9wt.%, and XPS test shows that the doping amount of fluorine ions is about 5wt.%.

[0109] Comparative Example 1

[0110] The operating conditions were the same as those in Example 1, except that lithium carbonate and stearic acid were not added to the hydroxyapatite precursor powder, and sodium fluoride was not added for stirring after sintering.

[0111] Comparative Example 2

[0112] The inorganic superionic conductor material prepared in Example 5 of CN 116969432A is used as Comparative Example 2.

[0113] The scanning electron microscope image is as follows Figure 3 The material is a fibrous material with a very high aspect ratio, a width of 40-80nm, and an aspect ratio of more than 1000.

[0114] ICP test shows that the doping amount of lithium ions in the inorganic superionic conductor material is 2.2wt.%, and XPS test shows that the doping amount of fluorine ions is about 3wt.%.

[0115] The comparison of the lithium ion doping amounts of Preparation Example 1 and Comparative Example 2 shows that the method of the present invention can dope more lithium ions into the final material.

[0116] Application Example 1

[0117] 1 g of the inorganic superionic conductor material obtained in Preparation Example 1 was uniformly dispersed in an acetonitrile solution containing 4 g of polyethylene oxide, and vacuum dried to obtain a composite solid electrolyte membrane.

[0118] Application Example 2

[0119] 1 g of the inorganic superionic conductor material obtained in Preparation Example 2 was uniformly dispersed in an acetonitrile solution containing 4 g of polyethylene oxide, and the mixture was vacuum dried to obtain a composite solid electrolyte membrane.

[0120] Application Example 3

[0121] The inorganic superionic conductor material obtained in Preparation Example 3 was hot-pressed and sintered at 80 MPa and 1200°C for 30 min to obtain a ceramic sheet, which was directly used as an inorganic solid electrolyte membrane. Figure 4 shown.

[0122] Application Example 4

[0123] 0.4 g of the inorganic superionic conductor material obtained in Preparation Example 3 is mixed and ground with an acetonitrile solution containing 0.1 g of polyethylene oxide, and after the acetonitrile evaporates, the mixture is pressed into tablets to obtain a clay-like inorganic solid electrolyte membrane.

[0124] Application Example 5

[0125] 0.4 g of the inorganic superionic conductor material obtained in Preparation Example 4 is mixed and ground with an acetonitrile solution containing 0.1 g of polyethylene oxide, and after the acetonitrile evaporates, the mixture is pressed into tablets to obtain a clay-like inorganic solid electrolyte membrane.

[0126] Application Example 6

[0127] 0.4 g of the inorganic superionic conductor material obtained in Preparation Example 5 is mixed and ground with an acetonitrile solution containing 0.1 g of polyethylene oxide, and after the acetonitrile evaporates, the mixture is pressed into tablets to obtain a clay-like inorganic solid electrolyte membrane.

[0128] Application Comparative Example 1

[0129] 1 g of the material obtained in Comparative Example 1 was uniformly dispersed in an acetonitrile solution containing 4 g of polyethylene oxide, the solution was dropped onto a polytetrafluoroethylene disc, and vacuum dried to obtain a composite solid electrolyte membrane.

[0130] Application Comparative Example 2

[0131] The inorganic superionic conductor material obtained in Comparative Example 2 was dispersed in water, and an inorganic solid electrolyte membrane was prepared by vacuum filtration.

[0132] Application Comparative Example 3

[0133] 1 g of the inorganic superionic conductor material obtained in Comparative Example 2 was uniformly dispersed in an acetonitrile solution containing 4 g of polyethylene oxide, and the mixture was vacuum dried to obtain a composite solid electrolyte membrane.

[0134] Test Example 1

[0135] Ionic conductivity test: The solid electrolyte membrane was polished smooth, gold-sprayed on both sides, sandwiched between two stainless steel gaskets, and connected to an electrochemical workstation for impedance testing at a frequency of 1MHz-0.1Hz.

[0136] Mechanical properties (tensile strength) test: The tensile speed is 500 mm / min. The sample is cut into dumbbell-shaped splines, clamped between fixtures, and the thickness, width and length of the spline working area are input to perform a tensile strength test.

[0137] Electrochemical performance test: assemble symmetrical cells and full cells for testing and analysis. The entire process of assembling the battery must be carried out in a glove box filled with argon. The symmetrical cell assembly process is: place the negative electrode shell, lithium sheet, solid electrolyte membrane, lithium sheet, and positive electrode shell in sequence, put them into a packaging machine and pressurize them to 50MPa; the full cell assembly process is: place the negative electrode shell, lithium sheet, solid electrolyte membrane, lithium iron phosphate, and positive electrode shell in sequence, put them into a packaging machine and pressurize them to 50MPa.

[0138] Symmetrical battery test: at 0.1 mA cm -2 At a current density of , charge for 1 hour, discharge for 1 hour, and repeat the charge and discharge cycle.

[0139] Rate performance test: The full battery is subjected to constant current charge and discharge test analysis under step current density. The test conditions are: voltage range 2.5-4.2V, step current density of 0.1C, 0.2C, 0.3C, 0.4C, 0.5C, 1.0C.

[0140] Reversible specific capacity and cycle performance test: The full battery is subjected to constant current charge and discharge test analysis. The test conditions are: voltage range 2.5-4.2V, current density 0.5C.

[0141] The results are shown in Tables 1 and 2.

[0142] Table 1

[0143]

[0144] Among them, “-” means that they are not comparable.

[0145] It can be seen from the results in Table 1 that the sheet-like inorganic superionic conductor material prepared in the present invention has excellent mechanical properties and electrochemical properties. Figure 5 This is a cycle performance diagram of a symmetrical battery assembled with the composite solid electrolyte membrane prepared in Application Example 1 of the present invention.

[0146] According to the comparison between application examples 1 and 2 and application comparison examples 1 and 3, it can be seen that the composite solid electrolyte membrane prepared from the inorganic superionic conductor material and polyethylene oxide of the present invention has good mechanical strength and high ionic conductivity. At the same time, the close contact between the polymer and the electrode enables its symmetrical battery to have extremely long cycle time and low overpotential.

[0147] Application Example 3 shows that the ceramic sheet prepared by hot pressing has a very high relative density (about 95%), making its cycle time much longer than that of traditional inorganic ceramic solid electrolytes. The ceramic sheet has extremely high ionic conductivity, so that a very low overpotential can be obtained when assembled into a symmetrical battery.

[0148] Comparison between Application Examples 4, 5, and 6 and Application Comparative Example 2 shows that the inorganic superionic conductor material of the present invention mixed with a small amount of polyethylene oxide can obtain an inorganic clay-like solid electrolyte membrane with extremely high mechanical strength, and there is also good interface contact between the electrodes, so that it has a longer cycle time and a very low overpotential.

[0149] Table 2

[0150]

[0151] As can be seen from Table 2, the inorganic or composite solid electrolyte membrane prepared by the present invention has a very good capacity retention rate in the full battery, all above 75%, and also has a very good rate performance, and the capacity will not drop significantly at high current density, and the capacity will recover after returning to a low current density. The reversible specific capacity is generally high.

[0152] The capacity of the composite solid electrolyte membrane prepared by using ordinary hydroxyapatite in Comparative Example 1 drops to 0 after 100 cycles, and the capacity loss is also very obvious at high current density.

[0153] Although the inorganic solid electrolyte membrane made of fibrous inorganic superionic conductor material in Comparative Example 2 has a good capacity retention rate at a fixed current density, its capacity performance will have a large capacity attenuation at a high current density.

[0154] The composite solid electrolyte membrane in Comparative Example 3 is inferior to those in Examples 1-6 in terms of cycle performance and rate performance.

[0155] Figure 6 This is a charge and discharge curve diagram of a full battery assembled with the composite solid electrolyte membrane prepared in Application Example 1 of the present invention. Figure 7 This is a rate performance diagram of a full battery assembled with the composite solid electrolyte membrane prepared in Application Example 1 of the present invention.

[0156] Test Example 2

[0157] (1) Chemical stability test:

[0158] The composite solid electrolyte membrane prepared in Example 1 was assembled into an iron-lithium battery for electrochemical window test. The iron-lithium battery assembly process is: placing the negative electrode shell, lithium sheet, solid electrolyte membrane, stainless steel gasket, and positive electrode shell in sequence, and putting them into a packaging machine and pressurizing them to 50 MPa.

[0159] Linear sweep voltammetry (LSV) test analysis was performed on the lithium iron battery. The test conditions were: voltage range 0-6V, scan rate 1mV s -1 .

[0160] Depend on Figure 8 It can be seen that there is no obvious change in the internal current of the battery within the range of 0.2-5.2V, indicating that it can work normally within this potential range and no oxidation or reduction reaction will occur.

[0161] (2) Air thermal stability test:

[0162] The inorganic superionic conductor material obtained in Preparation Example 1 was placed in an air environment for 90 days, and then a composite solid electrolyte membrane was prepared according to the method described in Application Example 1. The ionic conductivity of the composite solid electrolyte membrane was 2.1×10 -4 S / cm, with no noticeable loss in performance.

[0163] The processing temperature of the inorganic superionic conductor material prepared by the present invention is about 1000° C., and the sintering atmosphere is air. The material does not decompose, which proves that it has significant air thermal stability.

[0164] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An inorganic superionic conductor material, characterized in that: The inorganic superionic conductor material comprises apatite and doping ions doped in the apatite; Wherein, the doping ions include metal cations and non-metal anions; The inorganic superionic conductor material has a flake shape.

2. The inorganic superionic conductor material according to claim 1, wherein The apatite contains hydroxide ions; Preferably, the length of the inorganic superionic conductor material is 1-20 μm, preferably 1-5 μm, or 2-10 μm, or 3-10 μm, or 8-10 μm; Preferably, the thickness of the inorganic superionic conductor material is 300 nm-2 μm, preferably 400 nm-1.2 μm, further preferably 400-600 nm, or 1 μm; Preferably, the metal cation is selected from at least one of lithium ion, sodium ion, potassium ion, magnesium ion, zinc ion, chromium ion, aluminum ion, barium ion, chromium ion, lead ion and mercury ion, preferably lithium ion; Preferably, the non-metallic anion is selected from at least one of fluoride ion, chloride ion and bromide ion, preferably fluoride ion; Preferably, the doping amount of metal cations in the inorganic superionic conductor material is 1-8wt.%, preferably 1.9-7.68wt.%, or 4.43-5.37wt.%, or 5.21wt.%; Preferably, the doping amount of the non-metallic anion in the inorganic superionic conductor material is 1-10 wt.%, preferably 5-10 wt.%, or 6-7 wt.%.

3. A method for preparing an inorganic superionic conductor material according to claim 1 or 2, characterized in that: The method is a solid phase sintering method, comprising the following steps: (1) mixing hydroxyapatite powder, metal cation salt powder and an optional dispersant to obtain a precursor powder, and performing a solid phase reaction sintering treatment; (2) grinding the powder after sintering in step (1), and then soaking it in water; (3) centrifuging, washing and drying the product after soaking in step (2); (4) Adding a non-metallic anion salt to the product obtained in step (3) for mixing, and then centrifuging, washing, and drying to obtain the inorganic superionic conductor material.

4. The method according to claim 3, wherein: The metal cation salt powder in step (1) is selected from at least one of lithium carbonate, lithium nitrate, lithium sulfate, sodium carbonate, sodium sulfate, sodium nitrate, potassium carbonate, magnesium sulfate, zinc sulfate, strontium sulfate and barium carbonate, preferably lithium carbonate; Preferably, the dispersant is selected from at least one of stearic acid, sodium oleate, glutamic acid and alanine, preferably stearic acid; Preferably, the mass ratio of the hydroxyapatite powder to the metal cation salt powder is 10:0.4-8, preferably 10:2.5-4.3; Preferably, the mass ratio of the hydroxyapatite powder to the dispersant is 10:0.6-0.7; Preferably, the mixing time in step (1) is 10 min-1 h, preferably 20-30 min; Preferably, the sintering treatment in step (1) is one of muffle furnace sintering, hot pressing sintering, cold pressing sintering, microwave sintering, liquid phase sintering, and spark plasma SPS sintering, preferably muffle furnace sintering or hot pressing sintering; Preferably, the sintering temperature is 600-1200°C, preferably 800-4000°C, and more preferably 800°C or 1000°C; Preferably, the heating rate is 2-10°C / min, preferably 5°C / min; Preferably, the sintering time is 1-6h, preferably 2h; Preferably, the sintering atmosphere is one of air, oxygen, nitrogen and argon, preferably air; Preferably, the soaking time in step (2) is 8-24 hours, preferably 12 hours; Preferably, the drying conditions in step (3) include: a drying temperature of 20-80° C., preferably 60° C.; a drying time of 6-24 h, preferably 24 h; Preferably, the non-metallic anion salt in step (4) is at least one selected from sodium fluoride, sodium chloride, sodium bromide, potassium chloride, potassium fluoride, potassium bromide, ammonium chloride, ammonium fluoride and ammonium bromide, preferably sodium fluoride; Preferably, the mass ratio of the product obtained in step (3) to the non-metallic anion salt is 2:5-30, preferably 2:10-20; Preferably, the mixing time in step (4) is 4-24 hours, preferably 8-12 hours; the mixing temperature is 20-80°C, preferably 60°C; Preferably, the drying conditions include: a temperature of 20-100° C., preferably 40-80° C.; and a drying time of 4-24 h, preferably 12-16 h.

5. An inorganic superionic conductor material obtained according to the preparation method of claim 3 or 4.

6. Use of the inorganic superionic conductor material according to any one of claims 1-2 and 5 in the preparation of lithium batteries and other secondary batteries; Preferably, the inorganic superionic conductor material is used in the preparation of inorganic solid electrolytes, composite solid electrolytes, positive and negative electrode materials, separators and electrolytes.

7. An inorganic solid electrolyte membrane made from the inorganic superionic conductor material according to any one of claims 1 to 2 and 5; Preferably, the inorganic solid electrolyte membrane is a ceramic sheet or a clay-like inorganic solid electrolyte membrane.

8. A method for preparing an inorganic solid electrolyte membrane according to claim 7, characterized in that: The method comprises: mixing and grinding the inorganic superionic conductor material with an acetonitrile solution of polyethylene oxide, and pressing the acetonitrile into tablets after evaporation to obtain a clay-like inorganic solid electrolyte membrane; Preferably, the mass ratio of the inorganic superionic conductor material to polyethylene oxide is 3-9:1, preferably 4:

1.

9. A composite solid electrolyte membrane made of the inorganic superionic conductor material according to any one of claims 1 to 2 and 5; Preferably, the composite solid electrolyte membrane is prepared by mixing the inorganic superionic conductor material with an acetonitrile solution of polyethylene oxide and then drying; Preferably, the mass ratio of the inorganic superionic conductor material to polyethylene oxide is 1:3-9, preferably 1:

4. 10 . A lithium battery comprising the inorganic solid electrolyte membrane according to claim 7 or the composite solid electrolyte membrane according to claim 9 .

Citation Information

Patent Citations

  • Polyhydroxy nano-material composite solid polymer electrolyte

    CN113851703A

  • Inorganic super-ion conductor material, preparation method and application thereof, inorganic solid electrolyte membrane and lithium battery

    CN116969432A

  • Separator, electrode group, secondary battery, battery pack, vehicle, and stationary power supply

    EP3792993A1