Efficient and environment-friendly method for preparing wooden activated carbon and application
Through enzymatic reaction of enzymatic lysis and low-concentration phosphoric acid in a nitrogen-hydrogen atmosphere, combined with alkaline buffer solution and solid composite salt, the pollution and complexity of wood activated carbon preparation in the prior art is solved, and efficient and environmentally friendly activated carbon is achieved. Preparation and excellent adsorption properties, suitable for flue gas treatment and water treatment.
Patent Information
- Application Number
- CN202411048418.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The use of metal salts and solvents in the existing wood activated carbon preparation process leads to industrial pollution, and the process is complex and does not conform to the concept of green environmental protection, making it difficult to achieve low-pollution and efficient resource utilization of agricultural and forestry waste.
After pretreatment of wood waste, the thermal reaction of enzymatic lysis and low-concentration phosphoric acid in a nitrogen-hydrogen atmosphere is adopted, combined with the medium-temperature heat treatment of alkaline buffer solution and solid composite salt to form a high activation energy activated carbon precursor, and High-performance activated carbon is obtained by extrusion molding.
It has achieved efficient and environmentally friendly preparation of high-performance activated carbon, which has improved its microporous structure and adsorption properties, which are suitable for flue gas treatment and water treatment, and has significantly improved the pollutant removal rate.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the field of environmentally friendly material preparation, and in particular to a method for preparing wood activated carbon with high efficiency and environmental protection and its application. Background Art
[0002] As economic, social, energy, and environmental issues become increasingly prominent, the preparation of agricultural and forestry waste materials into functional porous carbon materials through environmentally friendly processes has attracted great attention from researchers in various countries. Wood activated carbon has the characteristics of developed internal pore structure, large specific surface area, and strong adsorption capacity. Its unique and developed microporous structure and excellent selective adsorption characteristics are widely used in industry, agriculture, national defense, and people's daily life. Its application direction and application field are very wide.
[0003] my country has proposed: Strengthen the resource utilization of agricultural and forestry wastes, encourage the use of small firewood and three forestry residues (logging residues, timber residues, and processing residues) according to local conditions to promote the resource utilization of agricultural product processing by-products. The wood activated carbon industry is a typical resource comprehensive utilization industry, supported by national industrial support, tax incentives and other aspects. Therefore, the project has a wide range of application prospects and can be used as an important material in environmental protection, industry and life, which helps to promote the efficient utilization of resources and environmental protection. The current preparation process of activated carbon generally involves the use of metal salts and solvents, which does not conform to the concept of green environmental protection and is prone to industrial pollution. In addition, the preparation process is complicated and also consumes energy. Therefore, while utilizing agricultural and forestry wastes as resources, it is of certain research significance to achieve low-pollution and efficient preparation of wood activated carbon. Summary of the invention
[0004] In view of the above problems, the object of the present invention is to provide a method and application for preparing wood activated carbon in an efficient and environmentally friendly manner.
[0005] The technical contents of the present invention are as follows:
[0006] The present invention provides a method for preparing wood activated carbon in an efficient and environmentally friendly manner, comprising the following steps:
[0007] 1) Pre-treating wood waste to remove impurities to obtain wood particles, immersing them in an alkaline buffer solution containing 4-8wt% carbodiimide after activation, heating them with microwaves, standing them, and filtering them; the activation is to enzymatically hydrolyze the wood particles with an enzyme solution, spray low-concentration phosphoric acid until the liquid content of the wood particles is 10%-20%, and then conduct a thermal reaction in a nitrogen-hydrogen atmosphere;
[0008] The pretreatment is to crush the wood waste through a 50-100 mesh sieve;
[0009] The enzyme solution is prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in a mass ratio of 11-15:3-5:3-5 in water at a concentration of 0.05-0.1 g / L, and the mass concentration of phosphoric acid is 10-20%;
[0010] The enzyme solution uses hydroxylase and cellulase for synergistic decomposition, and the generated hydrogen peroxide can promote the decomposition of cellulose.
[0011] The ratio of nitrogen to hydrogen in the thermal reaction is (6:4) to (4:1), the temperature of the thermal reaction is 100-150° C., and the time of the thermal reaction is 40-60 min;
[0012] The alkaline buffer solution is a sodium hydrogen phosphate aqueous solution with a pH of 7-8;
[0013] The microwave heating temperature is 70-80°C, the time is 20-30min, and the standing time is 10-20min;
[0014] 2) mixing the treated wood particles with a solid composite salt in a mass ratio of 11-14:3-5, and performing a medium-temperature heat treatment under an inert atmosphere to obtain an activated carbon precursor;
[0015] The solid composite salt is composed of hydroxyapatite and sodium sulfate in a mass ratio of 3:2-5;
[0016] The medium temperature heat treatment is performed at a temperature of 250-350°C and a time of 15-25 minutes;
[0017] In the medium-temperature heat treatment, the treated wood particles have carboxyl groups with high activation energy, which can form amino groups with solid salts, and the acid radical ions modify the activated carbon to improve its stability.
[0018] 3) Mixing the activated carbon precursor with deionized water at a solid-liquid ratio of 1:10-15 g / mL, extruding and then drying in a drying oven to obtain activated carbon.
[0019] The present invention provides activated carbon prepared by the above method, with a particle size of 0.1-0.3 mm;
[0020] The present invention also provides applications of activated carbon in areas not limited to flue gas treatment and water treatment.
[0021] Beneficial effects of the present invention: The present invention provides a method for preparing highly efficient and environmentally friendly wood activated carbon, which utilizes agricultural and forestry wastes, crushes and sieves the wood waste to refine it, and then uses low-concentration phosphoric acid to perform a thermal reaction in a nitrogen-hydrogen atmosphere after enzymatic hydrolysis, thereby increasing the degree of reaction between wood cellulose and phosphoric acid, and the thermal reaction in a nitrogen-hydrogen atmosphere can play a synergistic oxidation role with phosphoric acid, and then the activated wood particles are neutralized by an alkaline buffer solution to further perform an aromatic condensation, thereby increasing the aromatization degree of the activated carbon, thereby improving its microporous structure, and then mixing and heat-treating it with a solid composite salt, and then wet-extruding it to obtain an activated carbon with a high molding rate, large production capacity and good quality;
[0022] The present invention also provides the application of the prepared activated carbon. The prepared activated carbon has good adsorption performance and can be applied to the fields of flue gas treatment, wastewater utilization, etc. It can effectively adsorb pollutants and has a high removal rate of pollutants. DETAILED DESCRIPTION
[0023] The present invention is further described in detail below through specific implementation cases. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of protection of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art are all within the scope of the claims attached to this application.
[0024] Unless otherwise specified, all raw materials and reagents of the present invention are raw materials and reagents from the conventional market.
[0025] Example 1
[0026] A method for preparing wood activated carbon in an efficient and environmentally friendly manner comprises the following steps:
[0027] 1) The collected waste wood from wood processing is crushed and pre-treated by passing through an 80-mesh sieve to remove impurities to obtain wood particles, and the wood particles are enzymatically hydrolyzed by using an enzyme solution prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in water at a mass ratio of 13:4:4 at a concentration of 0.08 g / L, and then phosphoric acid with a mass concentration of 15% is sprayed until the liquid content of the wood particles is 15%, and then the wood particles are activated by heat reaction at a temperature of 130° C. for 50 minutes in a nitrogen-hydrogen atmosphere with a ratio of nitrogen to hydrogen of 10:4, and then immersed in a sodium hydrogen phosphate aqueous solution with a pH of 7 containing 5 wt % carbodiimide and microwave-heated at a temperature of 75° C. for 25 minutes, left to stand for 15 minutes, and filtered;
[0028] 2) mixing the treated wood particles with a solid composite salt composed of hydroxyapatite and sodium sulfate in a mass ratio of 12:4 and heat-treating them at 300° C. for 20 min under an inert atmosphere to obtain an activated carbon precursor;
[0029] 3) The activated carbon precursor was mixed with deionized water at a solid-liquid ratio of 1:13 g / mL, and the mixture was extruded and dried in a drying oven to obtain activated carbon.
[0030] The BET specific surface area distribution of activated carbon was determined to be 2136.3 m 2 / g,2093m 2 / g.
[0031] Example 2
[0032] A method for preparing wood activated carbon in an efficient and environmentally friendly manner comprises the following steps:
[0033] 1) The collected waste wood materials from wood processing are crushed and pre-treated by passing through a 50-mesh sieve to remove impurities to obtain wood particles, and the wood particles are enzymatically hydrolyzed by using an enzyme solution prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in water at a mass ratio of 11:3:3 at a concentration of 0.05 g / L, and then sprayed with phosphoric acid at a mass concentration of 10% until the liquid content of the wood particles is 10%, and then activated by heat reaction for 40 minutes at a temperature of 100° C. in a nitrogen-hydrogen atmosphere with a ratio of nitrogen to hydrogen of 6:4, and then immersed in a sodium hydrogen phosphate aqueous solution with a pH of 7 containing 4 wt % carbodiimide and microwave-heated at a temperature of 70° C. for 20 minutes, allowed to stand for 10 minutes, and filtered;
[0034] 2) mixing the treated wood particles with a solid composite salt composed of hydroxyapatite and sodium sulfate in a mass ratio of 3:2 at a mass ratio of 11:3, and heat-treating the mixture at a temperature of 250° C. for 15 minutes under an inert atmosphere to obtain an activated carbon precursor;
[0035] The activated carbon precursor was mixed with deionized water at a solid-liquid ratio of 1:10 g / mL, extruded and then dried in a drying oven to obtain activated carbon.
[0036] The BET specific surface area distribution of activated carbon was determined to be 1880.3 m 2 / g,2040m 2 / g.
[0037] Example 3
[0038] A method for preparing wood activated carbon in an efficient and environmentally friendly manner comprises the following steps:
[0039] 1) The collected waste wood from wood processing is crushed and pre-treated by passing through a 100-mesh sieve to remove impurities to obtain wood particles, and the wood particles are enzymatically hydrolyzed by using an enzyme solution prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in water at a mass ratio of 15:5:5 at a concentration of 0.1 g / L, and then sprayed with phosphoric acid at a mass concentration of 20% until the liquid content of the wood particles is 20%, and then in a nitrogen-hydrogen atmosphere, the ratio of nitrogen to hydrogen is 4:1, the temperature is 150° C., and then the wood particles are activated by thermal reaction for 60 minutes, and then immersed in a sodium hydrogen phosphate aqueous solution with a pH of 8 containing 8wt% carbodiimide, and microwave-heated at a temperature of 80° C. for 30 minutes, allowed to stand for 20 minutes, and filtered;
[0040] 2) mixing the treated wood particles with a solid composite salt composed of hydroxyapatite and sodium sulfate in a mass ratio of 14:5 and heat-treating them at 350° C. for 25 min under an inert atmosphere to obtain an activated carbon precursor;
[0041] The activated carbon precursor was mixed with deionized water at a solid-liquid ratio of 1:15 g / mL, extruded and then dried in a drying oven to obtain activated carbon.
[0042] The BET specific surface area distribution of activated carbon was determined to be 1902.3 m 2 / g,2058m 2 / g.
[0043] Example 4
[0044] A method for preparing wood activated carbon in an efficient and environmentally friendly manner comprises the following steps:
[0045] 1) The collected waste wood from wood processing is crushed and pre-treated by passing through a 60-mesh sieve to remove impurities to obtain wood particles, and the wood particles are enzymatically hydrolyzed by using an enzyme solution prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in water at a mass ratio of 12:3:3 at a concentration of 0.06 g / L, and then sprayed with phosphoric acid at a mass concentration of 12% until the liquid content of the wood particles is 12%, and then in a nitrogen-hydrogen atmosphere, the ratio of nitrogen to hydrogen is 7:4, the temperature is 110° C., and then the wood particles are activated by thermal reaction for 45 minutes, and then immersed in a sodium hydrogen phosphate aqueous solution with a pH of 7 containing 6 wt % carbodiimide, and microwave-heated at a temperature of 75° C. for 25 minutes, and allowed to stand for 10 minutes, and filtered;
[0046] 2) mixing the treated wood particles with a solid composite salt composed of hydroxyapatite and sodium sulfate in a mass ratio of 3:2-5 at a mass ratio of 12:3, and heat-treating the mixture for 18 minutes at a temperature of 250-350° C. under an inert atmosphere to obtain an activated carbon precursor;
[0047] The activated carbon precursor was mixed with deionized water at a solid-liquid ratio of 1:12 g / mL, extruded and then dried in a drying oven to obtain activated carbon.
[0048] The BET specific surface area distribution of activated carbon was determined to be 2013m 2 / g,1986m 2 / g.
[0049] Example 5
[0050] A method for preparing wood activated carbon in an efficient and environmentally friendly manner comprises the following steps:
[0051] 1) The collected waste wood from wood processing is crushed and pre-treated by passing through a 90-mesh sieve to remove impurities to obtain wood particles, and the wood particles are enzymatically hydrolyzed by using an enzyme solution prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in water at a mass ratio of 15:5:3 at a concentration of 0.09 g / L, and then sprayed with phosphoric acid at a mass concentration of 19% until the liquid content of the wood particles is 19%, and then in a nitrogen-hydrogen atmosphere, the ratio of nitrogen to hydrogen is 15:4, the temperature is 140° C., and then the wood particles are activated by thermal reaction for 55 minutes, and then immersed in a sodium hydrogen phosphate aqueous solution with a pH of 8 containing 5wt% carbodiimide, and microwave-heated at a temperature of 80° C. for 20 minutes, and allowed to stand for 15 minutes, and filtered;
[0052] 2) mixing the treated wood particles with a solid composite salt composed of hydroxyapatite and sodium sulfate in a mass ratio of 14:5 and heat-treating them at 350° C. for 15 min under an inert atmosphere to obtain an activated carbon precursor;
[0053] The activated carbon precursor was mixed with deionized water at a solid-liquid ratio of 1:12 g / mL, extruded and then dried in a drying oven to obtain activated carbon.
[0054] The BET specific surface area distribution of activated carbon was determined to be 2045.3 m 2 / g,2028m 2 / g.
[0055] Example 6
[0056] A method for preparing wood activated carbon in an efficient and environmentally friendly manner comprises the following steps:
[0057] 1) The collected waste wood from wood processing is crushed and pre-treated by passing through an 80-mesh sieve to remove impurities to obtain wood particles, and the wood particles are enzymatically hydrolyzed by using an enzyme solution prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in water at a mass ratio of 134:4 at a concentration of 0.07 g / L, and then sprayed with phosphoric acid at a mass concentration of 17% until the liquid content of the wood particles is 17%, and then in a nitrogen-hydrogen atmosphere, the ratio of nitrogen to hydrogen is 13:4, the temperature is 135° C., and then the wood particles are activated by thermal reaction for 60 minutes, and then immersed in a sodium hydrogen phosphate aqueous solution with a pH of 7 containing 8wt% carbodiimide, and microwave-heated at a temperature of 70° C. for 30 minutes, allowed to stand for 20 minutes, and filtered;
[0058] 2) mixing the treated wood particles with a solid composite salt composed of hydroxyapatite and sodium sulfate in a mass ratio of 14:3 and heat-treating them at 250° C. for 30 min under an inert atmosphere to obtain an activated carbon precursor;
[0059] The activated carbon precursor was mixed with deionized water at a solid-liquid ratio of 1:11 g / mL, extruded and then dried in a drying oven to obtain activated carbon.
[0060] The BET specific surface area distribution of activated carbon was determined to be 1915.6 m 2 / g,1899.1m 2 / g.
[0061] Example 7
[0062] A method for preparing wood activated carbon in an efficient and environmentally friendly manner comprises the following steps:
[0063] 1) crushing wood waste to pass through a 90-mesh sieve for pretreatment, removing impurities to obtain wood particles, enzymolyzing the wood particles with an enzyme solution prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in water at a mass ratio of 11:3:5 at a concentration of 0.09 g / L, spraying phosphoric acid with a mass concentration of 18% until the liquid content of the wood particles is 10%, and then performing a thermal reaction at a temperature of 130° C. for 50 minutes in a nitrogen-hydrogen atmosphere with a ratio of nitrogen to hydrogen of 3:1 for activation, and then immersing in a sodium hydrogen phosphate aqueous solution with a pH of 7 containing 4 wt % carbodiimide at a temperature of 80° C. for microwave heating for 25 minutes, standing for 20 minutes, and filtering;
[0064] 2) mixing the treated wood particles with a solid composite salt composed of hydroxyapatite and sodium sulfate in a mass ratio of 14:5 and heat-treating them at 260° C. for 18 min under an inert atmosphere to obtain an activated carbon precursor;
[0065] The activated carbon precursor was mixed with deionized water at a solid-liquid ratio of 1:14 g / mL, extruded and then dried in a drying oven to obtain activated carbon.
[0066] The BET specific surface area distribution of activated carbon was determined to be 1967.3 m 2 / g,1905.7m 2 / g.
[0067] Example 8
[0068] A method for preparing wood activated carbon in an efficient and environmentally friendly manner comprises the following steps:
[0069] 1) The wood waste is crushed and passed through a 100-mesh sieve for pretreatment, and impurities are removed to obtain wood particles. The wood particles are enzymatically hydrolyzed using an enzyme solution prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in water at a mass ratio of 15:4:3 at a concentration of 0.1 g / L, and then phosphoric acid with a mass concentration of 12% is sprayed until the liquid content of the wood particles is 12%, and then the wood particles are activated by thermal reaction at a temperature of 150° C. for 45 minutes in a nitrogen-hydrogen atmosphere with a ratio of nitrogen to hydrogen of 5:2, and then immersed in a sodium hydrogen phosphate aqueous solution with a pH of 8 containing 7 wt % carbodiimide and microwave-heated at a temperature of 75° C. for 30 minutes, left to stand for 18 minutes, and filtered;
[0070] 2) mixing the treated wood particles with a solid composite salt composed of hydroxyapatite and sodium sulfate in a mass ratio of 11:3 and heat-treating them at 310° C. for 20 min under an inert atmosphere to obtain an activated carbon precursor;
[0071] The activated carbon precursor was mixed with deionized water at a solid-liquid ratio of 1:15 g / mL, extruded and then dried in a drying oven to obtain activated carbon.
[0072] The BET specific surface area distribution of activated carbon was determined to be 1909.1 m 2 / g,1893.5m 2 / g.
[0073] Comparative Example 1
[0074] The difference between Comparative Example 1 and Example 1 is that, in step 1 of Comparative Example 1, no enzymatic hydrolysis is performed, and the other steps remain unchanged;
[0075] The BET specific surface area distribution of activated carbon was determined to be 1402.6 m 2 / g,1524.0m 2 / g.
[0076] Comparative Example 2
[0077] The difference between Comparative Example 2 and Example 1 is that in step 1 of Comparative Example 2, the alkaline buffer solution is not used for immersion, and the activated wood particles are filtered 4 times with deionized water, and the other parts remain unchanged;
[0078] The BET specific surface area distribution of activated carbon was determined to be 1399.1 m 2 / g, 1374.3m 2 / g.
[0079] Comparative Example 3
[0080] The difference between Comparative Example 3 and Example 3 is that in step 2 of Comparative Example 3, the solid composite salt is not mixed, and the other parts remain unchanged;
[0081] The BET specific surface area distribution of activated carbon was determined to be 1457.7 m 2 / g,1398.5m 2 / g.
[0082] 1. The production results of activated carbon of Examples 1-8 are shown in Table 1.
[0083] Table 1 Forming rate and yield of activated carbon
[0084]
[0085] As can be seen from Table 1, the method of the present invention for preparing activated carbon has the characteristics of high yield, good formability, high efficiency and environmental protection.
[0086] 2. The toluene adsorption capacity of activated carbon is shown in Table 2.
[0087] Table 2 Organic matter adsorption capacity of activated carbon
[0088]
[0089] It can be seen from Table 2 that the activated carbon prepared by the present invention can effectively adsorb organic matter.
[0090] In the method provided by the present invention, weak alkali and weak acid solutions are used for treatment in the early stage, which reduces the corrosion pollution caused by the strong acid used in the prior art. In the early stage, the wood waste is treated by enzymatic hydrolysis combined with low-concentration phosphoric acid modification, the wood raw materials are modified and activated, and then neutralized and condensed, which can effectively improve the comprehensive performance of activated carbon. In the later stage, hydroxyl salts and sulfates are mixed to improve the structural performance, and high-performance activated carbon can be prepared efficiently and environmentally friendly.
Claims
1. A method for preparing wood activated carbon in an efficient and environmentally friendly manner, characterized in that: The following steps are involved: 1) pre-treating the wood waste to remove impurities to obtain wood particles, activating the wood particles, immersing the particles in an alkaline buffer solution containing 4-8 wt% carbodiimide, heating the particles by microwave, and then allowing the particles to stand and filter; The activation is to enzymatically hydrolyze the wood particles with an enzyme solution, then spray low-concentration phosphoric acid until the liquid content of the wood particles is 10%-20%, and then perform a thermal reaction in a nitrogen-hydrogen atmosphere; 2) mixing the treated wood particles with a solid composite salt in a mass ratio of 11-14:3-5, and performing a medium-temperature heat treatment under an inert atmosphere to obtain an activated carbon precursor; 3) Mixing the activated carbon precursor with deionized water at a solid-liquid ratio of 1:10-15 g / mL, extruding and then drying in a drying oven to obtain activated carbon.
2. The method for preparing wood activated carbon in an efficient and environmentally friendly manner according to claim 1, characterized in that: The pretreatment in step 1) is to crush the wood waste through a 50-100 mesh sieve.
3. The method for preparing wood activated carbon in an efficient and environmentally friendly manner according to claim 1, characterized in that: Step 1) The enzyme solution is prepared by dispersing cellulase, xylanase and cellobiose dehydrogenase in a mass ratio of 11-15:3-5:3-5 in water at a concentration of 0.05-0.1 g / L; The mass concentration of the phosphoric acid is 10-20%.
4. The method for preparing wood activated carbon in an efficient and environmentally friendly manner according to claim 1, characterized in that: In step 1), the ratio of nitrogen to hydrogen in the thermal reaction is (6:4) to (4:1), the temperature of the thermal reaction is 100-150° C., and the time of the thermal reaction is 40-60 min.
5. The method for preparing wood activated carbon in an efficient and environmentally friendly manner according to claim 1, characterized in that: Step 1) The alkaline buffer solution is a sodium hydrogen phosphate aqueous solution with a pH of 7-8.
6. The method for preparing wood activated carbon in an efficient and environmentally friendly manner according to claim 1, characterized in that: Step 1) The microwave heating temperature is 70-80°C, the time is 20-30 minutes, and the standing time is 10-20 minutes.
7. The method for preparing wood activated carbon in an efficient and environmentally friendly manner according to claim 1, characterized in that: Step 2) The solid composite salt is composed of hydroxyapatite and sodium sulfate in a mass ratio of 3:2-5.
8. The method for preparing wood activated carbon in an efficient and environmentally friendly manner according to claim 1, characterized in that: Step 2) The medium temperature heat treatment is performed at a temperature of 250-350° C. for 15-25 minutes.
9. An activated carbon prepared by the method according to any one of claims 1 to 8, characterized in that: Its particle size is 0.1-0.3mm.
10. Application of the activated carbon according to claim 9 in flue gas treatment and water treatment.
Citation Information
Patent Citations
Manufacturing technology for low-sulfur activated carbon
CN103408006A
Method for producing active carbon
JP2016160130A