Optical adhesive, optical adhesive film, preparation method and flexible display device

The optical adhesive, designed with specific components and electric field effects, solves the problems of poor adhesion and peelability of OCA optical adhesive film in foldable display devices, enabling easy replacement and efficient maintenance, adapting to the bending requirements of foldable displays, and improving the reliability and service life of flexible display devices.

CN118978882APending Publication Date: 2024-11-19BOE TECHNOLOGY GROUP CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411287993.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing OCA optical adhesive films have poor adhesion and peelability in foldable display devices, making it difficult to meet the requirements of high-precision electronic products, and replacement is also difficult.

Method used

The optical adhesive formulation employs specific components and proportions, including isooctyl acrylate, isobornyl acrylate, polystyrene sulfonate, acrylamide, and 3,4-ethylenedioxythiophene. Through the electric field effect, the adhesive's tackiness is significantly reduced or lost after energization. Combined with the difference in release force of the release film, easy replacement is achieved.

Benefits of technology

Optical adhesive simplifies the replacement process after being powered on, improves production efficiency and the reliability of display devices, adapts to the dynamic bending of folding displays, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978882A_ABST
    Figure CN118978882A_ABST
Patent Text Reader

Abstract

The invention relates to the field of optical cement, and particularly provides optical cement, an optical cement film, a preparation method and a flexible display device. The viscidity of the optical adhesive after being electrified is smaller than that of the optical adhesive before being electrified. The optical adhesive disclosed by the invention is prepared from the following raw material components in parts by mass: 30 to 80 parts of 2-ethylhexyl acrylate, 5 to 30 parts of isobornyl acrylate, 1 to 10 parts of polystyrene sulfonate, 0.05 to 10 parts of acrylamide, 1 to 10 parts of 3, 4-ethylenedioxythiophene and 0.01 to 5 parts of a photoinitiator. The optical cement has a unique characteristic that the viscosity of the optical cement can be obviously reduced after the optical cement is electrified. By utilizing the characteristic, the maintenance cost of the flexible display device can be greatly reduced because the replacement process of the cover plate becomes simpler, more convenient and quicker. In addition, by means of the design, the service life of the device can be effectively prolonged, and it is ensured that a user obtains more lasting experience in the using process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of optical adhesives, and specifically provides an optical adhesive, an optical adhesive film, a preparation method and a flexible display device. Background Art

[0002] With the continuous advancement and innovation of science and technology, foldable screen displays have gradually become a development trend that cannot be ignored in modern society. Many well-known brands have invested a lot of resources to actively promote and develop foldable screen technology. In order to achieve the folding function, these foldable display products usually use thinner materials, but this also brings the problem of easy damage and scratches. In order to extend the service life of the product and improve the user experience, OCA (optically clear adhesive) is particularly important and plays a huge role in this field.

[0003] OCA optical film, or optically clear adhesive, is a substrate-free double-sided laminating tape made of OCA optical adhesive material. This film is known for its colorless and transparent properties, high light transmittance and excellent adhesive strength. OCA optical film can be used in a variety of different application scenarios due to its different thickness. It is mainly used in devices such as electronic paper, projection screens, displays, lenses and touch screens to bond transparent optical components. This film not only provides a stable bonding effect, but also maintains the transparency and clarity of optical components, thereby ensuring that the optical performance of the device is not affected. As a special adhesive, OCA can effectively protect the screen surface and reduce damage to the screen caused by external friction and impact. It not only improves the durability of the screen, but also maintains the clarity and touch sensitivity of the screen.

[0004] The OCA adhesive optical film formed by the existing OCA optical adhesive has the problems of poor adhesion and peelability, is not easy to replace, and is difficult to meet the use requirements of high-end electronic products, especially folding display devices. Summary of the invention

[0005] In order to overcome the above defects, the present invention proposes an optical adhesive, an optical adhesive film, a preparation method and a flexible display device. The optical adhesive can not only play a good protective role, but also has the characteristic of being easy to replace.

[0006] In a first aspect, the present invention provides an optical adhesive, wherein the viscosity of the optical adhesive after power is supplied is less than the viscosity before power is supplied.

[0007] Furthermore, the raw materials include the following components by mass:

[0008] 30-80 parts of isooctyl acrylate, 5-30 parts of isobornyl acrylate, 1-10 parts of polystyrene sulfonate, 0.05-10 parts of acrylamide, 1-10 parts of 3,4-ethylenedioxythiophene and 0.01-5 parts of photoinitiator.

[0009] Furthermore, the photoinitiator includes: one or both of azobisisobutyronitrile and 2-hydroxy-2-methyl-1-phenyl-1-propanone.

[0010] Furthermore, the raw materials include the following components by mass:

[0011] 50-80 parts of isooctyl acrylate, 10-20 parts of isobornyl acrylate, 1-5 parts of polystyrene sulfonate, 1-7 parts of acrylamide, 1-5 parts of 3,4-ethylenedioxythiophene and 0.01-1 part of photoinitiator.

[0012] Furthermore, the raw materials include the following components by mass:

[0013] 76 parts of isooctyl acrylate, 17 parts of isobornyl acrylate, 3.5 parts of polystyrene sulfonate, 1 part of acrylamide, 2.5 parts of 3,4-ethylenedioxythiophene and 0.05 parts of azobisisobutyronitrile as a photoinitiator.

[0014] Furthermore, the optical adhesive loses its adhesion after being energized at 0.5-2V.

[0015] In a second aspect, the present invention provides a method for preparing an optical adhesive, comprising the following steps:

[0016] Weigh isooctyl acrylate, isobornyl acrylate, polystyrene sulfonate, acrylamide, 3,4-ethylenedioxythiophene and a photoinitiator according to preset weight parts, and mix them evenly in a reactor, wherein the preset weight parts are 30-80 parts of isooctyl acrylate, 5-30 parts of isobornyl acrylate, 1-10 parts of polystyrene sulfonate, 0.05-10 parts of acrylamide, 1-10 parts of 3,4-ethylenedioxythiophene and 0.01-5 parts of the photoinitiator;

[0017] After replacing the air in the reactor with an inert gas, the reaction is carried out at a preset temperature until the viscosity of the product in the reactor reaches 1800-2300 cP.

[0018] Furthermore, the preset temperature is 80-120°C.

[0019] Furthermore, the inert gas includes nitrogen.

[0020] Furthermore, it also includes:

[0021] The product in the reactor after the reaction is baked.

[0022] Furthermore, the baking temperature is 30-60°C.

[0023] Furthermore, the photoinitiator includes: one or both of azobisisobutyronitrile and 2-hydroxy-2-methyl-1-phenyl-1-propanone.

[0024] In a third aspect, the present invention provides an optical adhesive film, comprising:

[0025] An optical adhesive layer, wherein the optical adhesive layer comprises at least one layer of the optical adhesive described in the first aspect;

[0026] A first release film is attached to one side of the optical adhesive;

[0027] A second release film is attached to the other side of the optical adhesive; wherein the first release film and the second release film sandwich the optical adhesive layer in the middle;

[0028] The release force of the first release film is greater than the release force of the second release film.

[0029] Furthermore, the first release film includes a release film substrate and a release agent layer coated on the surface of the release film substrate.

[0030] In a fourth aspect, the present invention provides a method for preparing an optical adhesive film, comprising:

[0031] Coating an optical adhesive layer on the first release film, wherein the optical adhesive layer comprises at least one layer of the optical adhesive described in the first aspect, and UV curing is performed after each layer of the optical adhesive is coated;

[0032] A second release film is covered on the optical adhesive layer; wherein the release force of the first release film is greater than the release force of the second release film.

[0033] Furthermore, the UV energy of the UV curing is 13000-15000 mJ / cm 2 , time is 1-8s.

[0034] Furthermore, the method further comprises:

[0035] After covering the second release film, thermal curing is performed.

[0036] Furthermore, the thermal curing temperature is 120-150° C. and the time is 8-12 hours.

[0037] In a fifth aspect, the present invention provides a flexible display device, comprising a stacked display assembly, an optical adhesive layer and a cover plate; wherein the optical adhesive layer comprises at least one layer of the optical adhesive described in the first aspect;

[0038] There is at least one cover plate, and adjacent cover plates and / or the cover plate and the display assembly are bonded together via the optical adhesive layer, wherein a conductive layer is further provided on the bonding interface of the optical adhesive layer.

[0039] Furthermore, the conductive layer is made of one of ITO and metal wire.

[0040] Furthermore, the conductive layer is a patterned ITO structure.

[0041] Furthermore, the metal wire comprises nano silver wire.

[0042] Furthermore, the cover plate is made of polyethylene terephthalate, polyimide, thermoplastic polyurethane elastomer rubber or ultra-thin glass.

[0043] Furthermore, the cover plate is a polarizer.

[0044] The above one or more technical solutions of the present invention have at least one or more of the following beneficial effects:

[0045] In the technical solution for implementing the present invention, the novel optical adhesive proposed by the present invention has two significant characteristics, making it particularly suitable for folding display screens. First, it has bending characteristics suitable for folding display screens, and can bend accordingly with the bending of the folding display screen. The optical adhesive film of the present invention can well adapt to the dynamic bending of the screen and the static bending in high temperature and high humidity environments. Therefore, this novel optical adhesive can be widely used in the growing flexible display market, providing strong support for the further development of folding screen technology.

[0046] Another unique feature of the optical adhesive of the present invention is that when powered on, its viscosity will be significantly reduced, or even lose its viscosity. This feature gives optical adhesive a great advantage in practical applications. Specifically, the characteristic that the viscosity of optical adhesive decreases after power is applied can greatly simplify the maintenance process, making the replacement of optical adhesive easier and faster. By powering the optical adhesive at a specific voltage, it can be completely removed without leaving any residual adhesive. In this way, the maintenance cost will be reduced accordingly, because it is no longer necessary to spend a lot of time and energy on complicated disassembly and installation processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The disclosure of the present invention will become more easily understood with reference to the accompanying drawings. It is easy for those skilled in the art to understand that these drawings are only for illustrative purposes and are not intended to limit the scope of protection of the present invention. In addition, similar numbers in the figures are used to represent similar components, among which:

[0048] Figure 1 is a schematic flow chart of main steps of a method for preparing an optical adhesive according to an embodiment of the present invention;

[0049] Figure 2 is a schematic structural diagram of an optical adhesive film including a layer of optical adhesive according to an embodiment of the present invention;

[0050] Figure 3 is a schematic structural diagram of an optical adhesive film including two layers of optical adhesive according to an embodiment of the present invention;

[0051] Figure 4 is a schematic diagram of the overall structure of a flexible display device according to an embodiment of the present invention;

[0052] Figure 5 is a schematic diagram of the shape of a bending area when a foldable display device is folded inward according to an embodiment of the present invention;

[0053] Figure 6 1 is a schematic diagram of the morphology of a bending area when a foldable display device is folded outward according to an embodiment of the present invention.

[0054] Reference numerals list :

[0055] 1: optical glue; 1-1: first layer of optical glue; 1-2: second layer of optical glue; 2: first release film; 3: second release film; 4: bending zone when the screen is folded inward; 5: bending zone when the screen is folded outward; 6 display assembly; 7-1 first cover plate; 7-2 second cover plate; 7-3 third cover plate. DETAILED DESCRIPTION

[0056] Some embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0057] The present invention provides an optical adhesive, wherein the viscosity of the optical adhesive after power is supplied is smaller than the viscosity before power is supplied.

[0058] The unique feature of this optical adhesive is that it can reduce adhesion through the electric field effect. Specifically, when this optical adhesive is energized, an electric field will be formed. This electric field will exert a force on the adherends in the optical adhesive, thereby effectively reducing the adsorption force between these adherends and the adhered material. Due to the existence of the electric field effect, the adherends in the optical adhesive will be affected by a repulsive force, causing them to disperse on the surface of the adhered material, thereby reducing the contact area with the surface of the adhered material. The dispersion of the adherends and the reduction of the contact area ultimately lead to a significant decrease in the adhesion of the optical adhesive, thereby achieving the effect of reducing viscosity.

[0059] The electrical viscosity reduction property of the optical adhesive of the present invention makes it extremely convenient in the production process. Through simple electrical control, the adhesion of the optical adhesive can be conveniently adjusted, thereby helping to improve the efficiency and quality of the production process. For example, on an automated production line, when the optical adhesive needs to be transported and processed, the electrical viscosity reduction property can effectively prevent the optical adhesive from sticking or interfering with the production process during the transport process, thereby ensuring the smooth progress of the production process.

[0060] In addition, the optical adhesive of the present invention shows great advantages in the application of replaceable folding optically clear adhesive (OCA). By applying an electric field to the optical adhesive to control its viscosity, it can be easily disassembled and replaced. This characteristic makes the optical adhesive have significant application value in occasions that require frequent replacement or maintenance, such as folding screen mobile phones or other foldable display devices. By controlling the viscosity through the electric field, the old optical adhesive can be easily removed and the new optical adhesive can be conveniently installed, which greatly simplifies the maintenance and replacement process and improves the reliability and service life of the display device.

[0061] In one embodiment, in order to effectively achieve the effect of reducing viscosity by electrification, the present invention develops a new formula of optical adhesive, the raw materials of which include the following components by weight:

[0062] 30-80 parts of isooctyl acrylate, 5-30 parts of isobornyl acrylate, 1-10 parts of polystyrene sulfonate, 0.05-10 parts of acrylamide, 1-10 parts of 3,4-ethylenedioxythiophene and 0.01-5 parts of photoinitiator.

[0063] A brief description of each of the above components:

[0064] Isooctyl acrylate (2-EHA), molecular formula is C 11 H 20 O 2 .

[0065] Isobornyl acrylate (IBOA), molecular formula: C 13 H 20 O 2 .

[0066] Polystyrene sulfonate (PSS), molecular formula is (C 8 H 8 O 3 S) n .

[0067] Acrylamide (AM), chemical formula C 3 H 5 NO.

[0068] 3,4-ethylenedioxythiophene (EDOT), molecular formula is C6 H 6 O 2 S, also known as 3,4-ethylenedioxythiophene.

[0069] The optical adhesive raw materials of this embodiment contain transparent conductive polymers, such as 3,4-ethylenedioxythiophene (EDOT) and polystyrene sulfonate (PSS). 3,4-ethylenedioxythiophene is a conductive polymer with high conductivity and good transparency. Polystyrene sulfonate (PSS) is used in combination with 3,4-ethylenedioxythiophene (EDOT) to form an EDOT / PSS composite material. It has the characteristics of high conductivity, good light transmittance and easy processing. In addition, isooctyl acrylate is one of the main monomers, which provides a lower modulus and helps deformation. Isobornyl acrylate has a high Tg, which improves adhesion and increases the modulus. Acrylamide is a functional monomer that can provide cross-linking and curing properties.

[0070] The addition of these materials can effectively reduce the adhesion of the adhesive under the action of an external electric field. This property makes it easier to peel the adhesive under certain conditions, thus meeting the needs of certain specific application scenarios.

[0071] The present invention blends an optical adhesive with suitable hardness and softness by matching specific materials and proportions. This adhesive not only has good bonding properties, but also can show a certain flexibility when subjected to external forces. This property enables the adhesive to show excellent adaptability in operations such as bending and folding, thereby being able to meet the use requirements of flexible display devices such as folding screens. Through this unique design, it can be ensured that the optical adhesive can provide sufficient bonding force in actual applications and can be bent when needed, thereby greatly expanding its application scenarios and scope of application.

[0072] In one embodiment, the photoinitiator includes: azobisisobutyronitrile and 2-hydroxy-2-methyl

[0073] -1-phenyl-1-propanone, one or two of them. Azobisisobutyronitrile (AIBN), molecular formula C 8 H 12 N 4 2-Hydroxy-2-methyl-1-phenyl-1-propanone (HMPP or photoinitiator 1173), structural formula: C 6 H 5 COC(CH 3 ) 2 OH. The photoinitiator of this embodiment can absorb energy of a certain wavelength in the ultraviolet light region or the visible light region to generate free radicals, cations, etc., thereby initiating polymerization, cross-linking and curing of the monomers.

[0074] In one embodiment, in order to optimize the ratio of the optical adhesive, the raw materials include the following components by weight:

[0075] 50-80 parts of isooctyl acrylate, 10-20 parts of isobornyl acrylate, 1-5 parts of polystyrene sulfonate, 1-7 parts of acrylamide, 1-5 parts of 3,4-ethylenedioxythiophene and 0.01-1 part of photoinitiator.

[0076] In one embodiment, in order to further optimize the ratio of the optical adhesive, the raw materials thereof include the following components in parts by mass:

[0077] 76 parts of isooctyl acrylate, 17 parts of isobornyl acrylate, 3.5 parts of polystyrene sulfonate, 1 part of acrylamide, 2.5 parts of 3,4-ethylenedioxythiophene and 0.05 parts of azobisisobutyronitrile as a photoinitiator.

[0078] In one embodiment, when the applied voltage is in the range of 0.5 to 2 volts, the optical adhesive exhibits a property of losing adhesion. Specifically, after the optical adhesive is powered on, when the voltage value is in the range of 0.5 to 2 volts, its viscosity will be significantly reduced, or even completely lose its adhesion ability, and there will be no residual adhesive on the interface, and the optimal condition is 1V.

[0079] The present invention also provides a method for preparing an optical adhesive, which is prepared by thermal polymerization. The specific steps are as follows. Figure 1 The flowchart shown:

[0080] S1, weighing isooctyl acrylate, isobornyl acrylate, polystyrene sulfonate, acrylamide, 3,4-ethylenedioxythiophene and a photoinitiator according to preset weight parts, and mixing them evenly in a reactor.

[0081] The preset weight parts are 30-80 parts of isooctyl acrylate, 5-30 parts of isobornyl acrylate, 1-10 parts of polystyrene sulfonate, 0.05-10 parts of acrylamide, 1-10 parts of 3,4-ethylenedioxythiophene and 0.01-5 parts of photoinitiator.

[0082] These raw material components need to ensure that their mass ratio meets specific requirements before mixing. Put them into a reactor and mix them at normal temperature and pressure to ensure that they can be evenly mixed together.

[0083] S2, after replacing the air in the reactor with an inert gas, react at a preset temperature until the viscosity of the product in the reactor reaches 1800-2300 cP.

[0084] Before the reaction, the air in the reactor is replaced with an inert gas to ensure that no unnecessary side reactions occur during the reaction. After the air replacement is completed, the mixture in the reactor is heated to a preset reaction temperature and maintained at this temperature for reaction. When the reaction proceeds to a certain extent, the viscosity of the reaction product is measured to ensure that it reaches the range of 1800-2300 cP. When the viscosity of the reaction product reaches this range, it indicates that the reaction has been completed, and the heating can be stopped at this time and the subsequent processing steps can be carried out.

[0085] Through the above steps, the desired optical adhesive can be successfully prepared, and the optical adhesive has good optical properties, mechanical properties and conductive and viscosity-reducing effects.

[0086] Step S2 can also be used to implement heating and condensation in the reactor during the reaction process, so as to provide a more ideal environment for the reaction. At the same time, the condensate produced can be returned to the reactor by reflux. The reflux of this condensate not only helps to maintain the material balance in the reactor, but also reduces the loss of raw materials to a certain extent. In this way, the reaction efficiency is significantly improved, and the yield of the final product is also increased.

[0087] In one embodiment, the preset temperature is 80-120°C.

[0088] In one embodiment, the inert gas includes nitrogen.

[0089] In one embodiment, it further includes:

[0090] S3, baking the product in the reaction kettle after the reaction to further solidify it.

[0091] In one embodiment, the baking temperature is 30-60°C.

[0092] In one embodiment, the photoinitiator includes: one or both of azobisisobutyronitrile and 2-hydroxy-2-methyl-1-phenyl-1-propanone.

[0093] The present invention further provides an optical adhesive film OCA, comprising: an optical adhesive layer, a first release film 2 and a second release film 3 .

[0094] Wherein, the optical adhesive layer comprises at least one layer of the optical adhesive 1, Figure 2 A schematic diagram showing an OCA including a layer of optical adhesive is shown. Figure 3 A schematic diagram showing an OCA including two layers of optical adhesive is shown.

[0095] The first release film 2 is attached to one side of the optical adhesive.

[0096] The second release film 3 is attached to the other side of the optical adhesive. The first release film 2 and the second release film 3 sandwich the optical adhesive layer 1 in the middle.

[0097] The release force of the first release film 2 is greater than the release force of the second release film 3. The first release film 2 is generally called a heavy film, and the second release film 3 is generally called a light film.

[0098] In one embodiment, the first release film includes a release film substrate and a release agent layer coated on a surface of the release film substrate.

[0099] The present invention also provides a method for preparing an optical adhesive film, comprising:

[0100] An optical adhesive layer is coated on the first release film by using a scraper coating machine, wherein the optical adhesive layer includes at least one layer of the optical adhesive, and UV curing is performed after each layer of the optical adhesive is coated.

[0101] A second release film is covered on the optical adhesive layer; wherein the release force of the first release film is greater than the release force of the second release film.

[0102] The optical adhesive is coated and cured to have high viscosity and good peeling property, and is finally formed between release films. When in use, the optical adhesive layer can be set on the interface to be bonded by peeling off the two release films.

[0103] The present invention uniformly coats the optical adhesive on the release film and undergoes appropriate curing treatment to form a film and obtain an optical adhesive film with high viscosity and good peeling performance. Finally, the optical adhesive film is successfully formed and fixed between two release films. In actual application, the user only needs to simply peel off the two release films to easily and accurately set the optical adhesive layer on the target interface to be bonded. This method not only improves the convenience of operation, but also ensures the reliability of the optical adhesive layer during the bonding process.

[0104] In one embodiment, the UV energy of the UV curing is 13000-15000 mJ / cm 2 , time is 1-8s.

[0105] In one embodiment, the method further comprises:

[0106] After covering the second release film, thermal curing is performed.

[0107] In one embodiment, the thermal curing temperature is 120-150° C. and the time is 8-12 hours.

[0108] Through such a thermal curing process, the adhesion and peeling properties of the optical adhesive film can be further improved, thereby ensuring its reliability and stability in subsequent applications.

[0109] The present invention prepares the optical adhesive film by using the following different ratios and process parameters.

[0110] Example 1

[0111] First, weigh 76 parts of isooctyl acrylate (2-EHA), 17 parts of isobornyl acrylate (IBOA), 3.5 parts of polystyrene sulfonate (PSS), 1 part of acrylamide (AM), 2.5 parts of 3,4-ethylenedioxythiophene (EDOT) and 0.05 parts of a photoinitiator (AIBN) according to the mass ratio.

[0112] The weighed components are placed into a reaction kettle and mixed evenly.

[0113] Then, the reactor was purged with nitrogen for 5-8 minutes until the air in the reactor was exhausted.

[0114] After the purge is completed, the reactor is placed in a constant temperature environment of 80°C and the temperature is kept constant. During the reaction process, the product in the reactor is regularly extracted for viscosity testing. The purpose of the viscosity test is to monitor the progress of the reaction and ensure that the product reaches the predetermined viscosity range. When the viscosity of the product in the reactor reaches 1800-2300cP, stop heating and the reaction is over. When the viscosity of the product in the reactor is 1800-2300cP, stop heating and the reaction is over.

[0115] After the reaction was completed, the product in the reactor was taken out and baked at 40°C for 1 h.

[0116] Finally, a doctor blade coating machine was used to evenly coat the baked optical adhesive onto the surface of the release film, and then UV curing was performed with a UV energy of 14000mJ / cm 2 After coating and UV treatment, gently cover with release film and heat cure at 130°C for 10 hours.

[0117] After the heat curing is completed, the film is rolled up to complete the preparation process of the entire optical film.

[0118] Example 2

[0119] First, 80 parts of isooctyl acrylate (2-EHA), 15 parts of isobornyl acrylate (IBOA), 1 part of polystyrene sulfonate (PSS), 7 parts of acrylamide (AM), 1 part of 3,4-ethylenedioxythiophene (EDOT) and 0.01 part of a photoinitiator (photoinitiator 1173) were weighed in proportion by mass.

[0120] The weighed components are placed into a reaction kettle and mixed evenly.

[0121] Then, the reactor was purged with nitrogen for 5-8 minutes until the air in the reactor was exhausted.

[0122] After the purge is completed, the reactor is placed in a constant temperature environment of 100°C and the temperature is kept constant. During the reaction process, the product in the reactor is regularly extracted for viscosity testing. The purpose of the viscosity test is to monitor the progress of the reaction and ensure that the product reaches the predetermined viscosity range. When the viscosity of the product in the reactor reaches 1800-2300cP, stop heating and the reaction is over. When the viscosity of the product in the reactor is 1800-2300cP, stop heating and the reaction is over.

[0123] After the reaction was completed, the product in the reactor was taken out and baked at 30°C for 2h.

[0124] Finally, a doctor blade coating machine was used to evenly coat the baked optical adhesive onto the surface of the release film, and then UV curing was performed with a UV energy of 13000mJ / cm 2 After coating and UV treatment, gently cover with release film and heat cure at 120℃ for 9h.

[0125] After the heat curing is completed, the film is rolled up to complete the preparation process of the entire optical film.

[0126] Example 3

[0127] First, 50 parts of isooctyl acrylate (2-EHA), 10 parts of isobornyl acrylate (IBOA), 10 parts of polystyrene sulfonate (PSS), 10 parts of acrylamide (AM), 10 parts of 3,4-ethylenedioxythiophene (EDOT) and 1 part of photoinitiator (AIBN) were weighed according to the mass ratio.

[0128] The weighed components are placed into a reaction kettle and mixed evenly.

[0129] Then, the reactor was purged with nitrogen for 5-8 minutes until the air in the reactor was exhausted.

[0130] After the purge is completed, the reactor is placed in a constant temperature environment of 90°C and the temperature is kept constant. During the reaction process, the product in the reactor is regularly extracted for viscosity testing. The purpose of the viscosity test is to monitor the progress of the reaction and ensure that the product reaches the predetermined viscosity range. When the viscosity of the product in the reactor reaches 1800-2300cP, stop heating and the reaction is over. When the viscosity of the product in the reactor is 1800-2300cP, stop heating and the reaction is over.

[0131] After the reaction was completed, the product in the reactor was taken out and baked at 40°C for 2h.

[0132] Finally, a doctor blade coating machine was used to evenly coat the baked optical adhesive onto the surface of the release film, and then UV curing was performed with a UV energy of 15000mJ / cm 2 After coating and UV treatment, gently cover with release film and heat cure at 140℃ for 12h.

[0133] After the heat curing is completed, the film is rolled up to complete the preparation process of the entire optical film.

[0134] Example 4

[0135] First, 30 parts of isooctyl acrylate (2-EHA), 5 parts of isobornyl acrylate (IBOA), 10 parts of polystyrene sulfonate (PSS), 10 parts of acrylamide (AM), 10 parts of 3,4-ethylenedioxythiophene (EDOT) and 5 parts of a photoinitiator (AIBN) were weighed in proportion by mass.

[0136] The weighed components are placed into a reaction kettle and mixed evenly.

[0137] Then, the reactor was purged with nitrogen for 5-8 minutes until the air in the reactor was exhausted.

[0138] After the purge is completed, the reactor is placed in a constant temperature environment of 120°C and the temperature is kept constant. During the reaction process, the product in the reactor is regularly extracted for viscosity testing. The purpose of the viscosity test is to monitor the progress of the reaction and ensure that the product reaches the predetermined viscosity range. When the viscosity of the product in the reactor reaches 1800-2300cP, stop heating and the reaction is over. When the viscosity of the product in the reactor is 1800-2300cP, stop heating and the reaction is over.

[0139] After the reaction was completed, the product in the reactor was taken out and baked at 60°C for 1 h.

[0140] Finally, a doctor blade coating machine was used to evenly coat the baked optical adhesive onto the surface of the release film, and then UV curing was performed with a UV energy of 13000mJ / cm 2 After coating and UV treatment, gently cover with release film and heat cure at 150℃ for 8h.

[0141] After the heat curing is completed, the film is rolled up to complete the preparation process of the entire optical film.

[0142] Example 5

[0143] First, weigh 60 parts of isooctyl acrylate (2-EHA), 20 parts of isobornyl acrylate (IBOA), 5 parts of polystyrene sulfonate (PSS), 10 parts of acrylamide (AM), 5 parts of 3,4-ethylenedioxythiophene (EDOT) and 0.2 parts of a photoinitiator (photoinitiator 1173) according to the mass ratio.

[0144] The weighed components are placed into a reaction kettle and mixed evenly.

[0145] Then, the reactor was purged with nitrogen for 5-8 minutes until the air in the reactor was exhausted.

[0146] After the purge is completed, the reactor is placed in a constant temperature environment of 110°C and the temperature is kept constant. During the reaction process, the product in the reactor is regularly extracted for viscosity testing. The purpose of the viscosity test is to monitor the progress of the reaction and ensure that the product reaches the predetermined viscosity range. When the viscosity of the product in the reactor reaches 1800-2300cP, stop heating and the reaction is over. When the viscosity of the product in the reactor is 1800-2300cP, stop heating and the reaction is over.

[0147] After the reaction was completed, the product in the reactor was taken out and baked at 40°C for 2h.

[0148] Finally, a doctor blade coating machine was used to evenly coat the baked optical adhesive onto the surface of the release film, and then UV curing was performed with a UV energy of 13000mJ / cm 2 After coating and UV treatment, gently cover with release film and heat cure at 120℃ for 10h.

[0149] After the heat curing is completed, the film is rolled up to complete the preparation process of the entire optical film.

[0150] Example 6

[0151] First, weigh 80 parts of isooctyl acrylate (2-EHA), 30 parts of isobornyl acrylate (IBOA), 1 part of polystyrene sulfonate (PSS), 10 parts of acrylamide (AM), 1 part of 3,4-ethylenedioxythiophene (EDOT) and 0.1 part of photoinitiator (0.05 parts each of photoinitiator 1173 and photoinitiator AIBN) according to the mass ratio.

[0152] The weighed components are placed into a reaction kettle and mixed evenly.

[0153] Then, the reactor was purged with nitrogen for 5-8 minutes until the air in the reactor was exhausted.

[0154] After the purge is completed, the reactor is placed in a constant temperature environment of 110°C and the temperature is kept constant. During the reaction process, the product in the reactor is regularly extracted for viscosity testing. The purpose of the viscosity test is to monitor the progress of the reaction and ensure that the product reaches the predetermined viscosity range. When the viscosity of the product in the reactor reaches 1800-2300cP, stop heating and the reaction is over. When the viscosity of the product in the reactor is 1800-2300cP, stop heating and the reaction is over.

[0155] After the reaction was completed, the product in the reactor was taken out and baked at 40°C for 2h.

[0156] Finally, a doctor blade coating machine was used to evenly coat the baked optical adhesive onto the surface of the release film, and then UV curing was performed with a UV energy of 13000mJ / cm 2 After coating and UV treatment, gently cover with release film and heat cure at 120℃ for 10h.

[0157] After the heat curing is completed, the film is rolled up to complete the preparation process of the entire optical film.

[0158] Comparative Example 1

[0159] The only difference between Comparative Example 1 and Example 1 is that: by mass, 79 parts of isooctyl acrylate (2-EHA), 20 parts of isobornyl acrylate (IBOA), 0 parts of polystyrene sulfonate (PSS), 1 part of acrylamide (AM), 0 parts of 3,4-ethylenedioxythiophene (EDOT) and 0.05 parts of photoinitiator (AIBN) were weighed.

[0160] Comparative Example 2

[0161] The only difference between Comparative Example 2 and Example 1 is that: 84 parts of isooctyl acrylate (2-EHA), 7.5 parts of isobornyl acrylate (IBOA), 0 parts of polystyrene sulfonate (PSS), 1 part of acrylamide (AM), 7.5 parts of 3,4-ethylenedioxythiophene (EDOT) and 0.05 parts of photoinitiator (AIBN) were weighed in proportion by mass.

[0162] Comparative Example 3

[0163] The only difference between Comparative Example 3 and Example 1 is that: by mass ratio, 76 parts of isooctyl acrylate (2-EHA), 17 parts of isobornyl acrylate (IBOA), 7 parts of polystyrene sulfonate (PSS), 1 part of acrylamide (AM), 0 parts of 3,4-ethylenedioxythiophene (EDOT) and 0.05 parts of photoinitiator (AIBN) were weighed.

[0164] Comparative Example 4

[0165] The only difference between Comparative Example 4 and Example 1 is that: 84.55 parts of isooctyl acrylate (2-EHA), 10 parts of isobornyl acrylate (IBOA), 4.45 parts of polystyrene sulfonate (PSS), 1 part of acrylamide (AM), 0 parts of 3,4-ethylenedioxythiophene (EDOT) and 0.08 parts of photoinitiator (AIBN) were weighed in proportion by mass.

[0166] Comparative Example 5

[0167] The only difference between Comparative Example 5 and Example 1 is that: by mass, 60 parts of isooctyl acrylate (2-EHA), 22 parts of isobornyl acrylate (IBOA), 17 parts of polystyrene sulfonate (PSS), 1 part of acrylamide (AM), 0 parts of 3,4-ethylenedioxythiophene (EDOT) and 0.08 parts of photoinitiator (AIBN) were weighed.

[0168] Comparative Example 6

[0169] The only difference between Comparative Example 6 and Example 1 is that: by mass ratio, 54 parts of isooctyl acrylate (2-EHA), 5 parts of isobornyl acrylate (IBOA), 0 parts of polystyrene sulfonate (PSS), 1 part of acrylamide (AM), 40 parts of 3,4-ethylenedioxythiophene (EDOT) and 0.05 parts of photoinitiator (AIBN) were weighed.

[0170] Comparative Example 7

[0171] The only difference between Comparative Example 7 and Example 1 is that: 20 parts of isooctyl acrylate (2-EHA), 21 parts of isobornyl acrylate (IBOA), 0 parts of polystyrene sulfonate (PSS), 1 part of acrylamide (AM), 58 parts of 3,4-ethylenedioxythiophene (EDOT) and 0.05 parts of photoinitiator (AIBN) are weighed in proportion by mass.

[0172] The optical adhesive films prepared in Examples 1-6 of the present invention and Comparative Examples 1-7 were tested, and the test results are shown in Table 1 and Table 2, respectively.

[0173] The test method of the peeling force of PET is: peeling is performed at a peeling rate of 300 nm / min according to the conventional peeling force test method.

[0174] The test method of the peeling force UTG is: peeling is performed at a peeling rate of 300 nm / min according to the conventional peeling force test method.

[0175] Using Anton Paar's MCR302 test equipment, the G' and Tg points at 25°C, 60°C were measured simultaneously. The test conditions were: 1HZ frequency; normal force 0.5N; temperature range: -50°C to 120°C.

[0176] Recovery (%) was calculated using Anton Paar MCR302 testing equipment, and the test conditions were: fixed stress 10 KPa, hold for 10 min, unload for 10 min. Sample size: diameter 8 nm, thickness 0.6 nm.

[0177] Table 1 Experimental test results of Examples 1-6

[0178]

[0179]

[0180] In Table 1, the optical adhesive film prepared by the present invention, after being attached to the folding display screen, can meet the requirement of peeling force ≥ 4N / inch, ensuring that separation will not occur at the folding optical display interface. In addition, the storage modulus of the optical adhesive film is 25-50kpa at 25°C and greater than 15kpa at 60°C, which indicates that it has good mechanical properties under different temperature conditions. At the same time, the Recovery value of the film at different temperatures is greater than 85%, which means that it has excellent rebound performance, can maintain structural integrity during the bending process, and avoid the problem of cohesive failure. It is also important to emphasize that after power is turned on, the optical adhesive film can be easily removed without leaving any residual adhesive, thereby ensuring convenience and cleanliness during use.

[0181] Table 2 Experimental test results of comparative examples 1-7

[0182]

[0183]

[0184] In Table 2, it can be seen that transparent conductive polymers EDOT and EDOT must coexist in the optical adhesive system, and a specific ratio needs to be maintained between them. In addition, other components must also be mixed according to the specific ratio specified in the present invention, otherwise it will be difficult to achieve good mechanical properties, post-conductive debonding, and bending effects at the same time. Although both EDOT and PSS have the property of post-conductive polymerization, this does not mean that other components with similar properties can be added or increased at will in the hope of achieving the effect of conductive debonding or conductive debonding. For example, under the ratio of comparative example 5, PSS exists alone and has a large content, and the entire system cannot even form an optical adhesive, but presents a gel form. Therefore, the energized debonding optical adhesive of the present invention is under specific components and ratios, combined with a preparation process that can effectively polymerize these components and solidify them into a film, and finally forms the optical adhesive of the present invention that can achieve the above-mentioned performance, which is used in flexible display devices.

[0185] Next, the application of the optical adhesive layer of the present invention in a flexible display device is described.

[0186] The present invention also provides a flexible display device, referring to Figure 4 , comprising a stacked display assembly 6, an optical adhesive layer and a cover plate 7; wherein the optical adhesive layer comprises at least one layer of the optical adhesive 1;

[0187] There is at least one cover plate, and adjacent cover plates and / or the cover plate and the display assembly are bonded together via the optical adhesive layer, wherein a conductive layer is further provided on the bonding interface of the optical adhesive layer.

[0188] In one embodiment, the conductive layer is made of one of ITO and metal wire.

[0189] In one embodiment, the conductive layer is a patterned ITO structure.

[0190] In one embodiment, the metal wire comprises nanosilver wire.

[0191] In one embodiment, the cover plate is made of polyethylene terephthalate, polyimide, thermoplastic polyurethane elastomer rubber or ultra-thin glass.

[0192] In one embodiment, the thickness of the ultra-thin glass is less than 1.2 mm.

[0193] In one embodiment, the cover plate is a polarizer.

[0194] In one embodiment, the display component includes an organic light-emitting layer and a driving backplane layer.

[0195] In one embodiment, the organic light-emitting layer includes an OLED light-emitting layer.

[0196] In one embodiment, the driving backplane layer includes a BKT layer and a supporting material layer which are stacked.

[0197] In one embodiment, when optical adhesive is required to be used to bond the display panel (organic light-emitting layer) and the cover plate, the method for forming the conductive layer includes:

[0198] A first ITO layer is formed on the display panel.

[0199] The first ITO layer is patterned to form a first ITO structure.

[0200] A second ITO layer is formed on the cover plate.

[0201] The second ITO layer is patterned to form a second ITO structure.

[0202] In order to facilitate storage and process flow, a protective film can be respectively covered on the other surface of the cover plate and the surface of the second ITO structure, which can be removed when in use.

[0203] Take the optical adhesive film, and adhere the optical adhesive layer after removing the second release film and the first release film to the first ITO structure of the display panel.

[0204] Then, a cover plate with a second ITO structure is placed on the optical adhesive layer, and the second ITO structure is arranged on the surface of the optical adhesive layer, so that adhesive for bonding and a conductive layer at the bonding interface are formed between the cover plate and the panel. After power is turned on, the cover plate and the display panel are separated due to the loss of adhesion of the optical adhesive.

[0205] In the current field of display technology, the material selection of folding display modules is an important research direction. In order to achieve the folding function, the current mainstream material selection includes ultra-thin glass and polymer materials, which are used as cover plates of folding display modules. Since these materials must have the characteristics of being able to withstand folding, they are usually designed to be very thin. However, this thinness also brings a significant disadvantage, that is, the material is easily damaged, scratched and broken. This fragility leads to the need for frequent replacement of the surface cover and its protective film to ensure that the display module can work properly and maintain the integrity of its appearance.

[0206] In order to solve this problem, the present invention proposes a new type of optical adhesive - folding OCA (Optically Clear Adhesive). This optical adhesive has two significant characteristics, making it particularly suitable for folding display screens. First, it has a bending property suitable for folding display screens and can bend accordingly with the bending of the folding display screen. Taking the OLED folding display screen as an example, refer to Figure 5 As shown, when the screen is folded inward, a water drop shape is formed in the bending area; refer to Figure 6 When the screen is folded outward, the bending area forms a U shape. The optical adhesive film of the present invention can well adapt to the dynamic bending of the screen and the static bending in a high temperature and high humidity environment. Therefore, this new optical adhesive can be widely used in the growing folding screen display market, providing strong support for the further development of folding screen technology.

[0207] Another unique feature of the optical adhesive of the present invention is that when powered on, its viscosity will be significantly reduced, or even lose its viscosity. This feature gives optical adhesive a great advantage in practical applications. Specifically, the characteristic that the viscosity of optical adhesive decreases after power is applied can greatly simplify the maintenance process, making the replacement of optical adhesive easier and faster. By powering the optical adhesive at a specific voltage, it can be completely removed without leaving any residual adhesive. In this way, the maintenance cost will be reduced accordingly, because it is no longer necessary to spend a lot of time and energy on complicated disassembly and installation processes.

[0208] In addition, this design not only performs well during the repair process, but also effectively extends the service life of related components. Since the optical glue becomes less sticky after power is turned on, the components can be adjusted and maintained more flexibly during use, ensuring that users have a more lasting and stable experience during use. The superiority of this design is not only reflected in the convenience of repair, but also in the reliability of long-term use, providing users with double protection.

[0209] It should be pointed out that although the various steps in the above embodiments are described in a specific order, those skilled in the art can understand that in order to achieve the effects of the present invention, different steps do not have to be performed in such an order. They can be performed simultaneously (in parallel) or in other orders. These changes are within the scope of protection of the present invention.

[0210] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. An optical adhesive, characterized in that: The viscosity of the optical adhesive after power is supplied is less than that before power is supplied.

2. The optical adhesive according to claim 1, characterized in that: The raw materials include the following components by mass: 30-80 parts of isooctyl acrylate, 5-30 parts of isobornyl acrylate, 1-10 parts of polystyrene sulfonate, 0.05-10 parts of acrylamide, 1-10 parts of 3,4-ethylenedioxythiophene and 0.01-5 parts of photoinitiator.

3. The optical adhesive according to claim 2, characterized in that: The photoinitiator comprises: one or two of azobisisobutyronitrile and 2-hydroxy-2-methyl-1-phenyl-1-propanone.

4. The optical adhesive according to claim 2 or 3, characterized in that: The raw materials include the following components by mass: 50-80 parts of isooctyl acrylate, 10-20 parts of isobornyl acrylate, 1-5 parts of polystyrene sulfonate, 1-7 parts of acrylamide, 1-5 parts of 3,4-ethylenedioxythiophene and 0.01-1 part of photoinitiator.

5. The optical adhesive according to claim 4, characterized in that: The raw materials include the following components by mass: 76 parts of isooctyl acrylate, 17 parts of isobornyl acrylate, 3.5 parts of polystyrene sulfonate, 1 part of acrylamide, 2.5 parts of 3,4-ethylenedioxythiophene and 0.05 parts of azobisisobutyronitrile as a photoinitiator.

6. The optical adhesive according to claim 1, characterized in that: The optical adhesive loses its adhesion after being powered at 0.5-2V.

7. A method for preparing an optical adhesive, characterized in that: The following steps are involved: Weigh isooctyl acrylate, isobornyl acrylate, polystyrene sulfonate, acrylamide, 3,4-ethylenedioxythiophene and a photoinitiator according to preset weight parts, and mix them evenly in a reactor, wherein the preset weight parts are 30-80 parts of isooctyl acrylate, 5-30 parts of isobornyl acrylate, 1-10 parts of polystyrene sulfonate, 0.05-10 parts of acrylamide, 1-10 parts of 3,4-ethylenedioxythiophene and 0.01-5 parts of the photoinitiator; After replacing the air in the reactor with an inert gas, the reaction is carried out at a preset temperature until the viscosity of the product in the reactor reaches 1800-2300 cP.

8. The method according to claim 7, characterized in that The preset temperature is 80-120°C.

9. The method according to claim 7, characterized in that: The inert gas includes nitrogen.

10. The method according to claim 7, characterized in that Also includes: The product in the reactor after the reaction is baked.

11. The method according to claim 10, characterized in that The baking temperature is 30-60°C.

12. The method according to claim 7, characterized in that The photoinitiator comprises: one or two of azobisisobutyronitrile and 2-hydroxy-2-methyl-1-phenyl-1-propanone.

13. An optical adhesive film, characterized in that: include: An optical adhesive layer, wherein the optical adhesive layer comprises at least one layer of the optical adhesive according to any one of claims 1 to 6; A first release film attached to one side of the optical adhesive; A second release film is attached to the other side of the optical adhesive; wherein the first release film and the second release film sandwich the optical adhesive layer in the middle; The release force of the first release film is greater than the release force of the second release film.

14. The adhesive film according to claim 13, characterized in that: The first release film includes a release film substrate and a release agent layer coated on the surface of the release film substrate.

15. A method for preparing an optical adhesive film, characterized in that: include: Coating an optical adhesive layer on the first release film, wherein the optical adhesive layer comprises at least one layer of the optical adhesive according to any one of claims 1 to 6, and UV curing is performed after each layer of the optical adhesive is coated; A second release film is covered on the optical adhesive layer; wherein the release force of the first release film is greater than the release force of the second release film.

16. The adhesive film according to claim 15, characterized in that: The UV energy of the UV curing is 13000-15000 mJ / cm 2 , time is 1-8s.

17. The adhesive film according to claim 15, characterized in that: The method further comprises: After covering the second release film, thermal curing is performed.

18. The adhesive film according to claim 17, characterized in that: The thermal curing temperature is 120-150° C. and the time is 8-12 hours.

19. A flexible display device, characterized in that: The invention comprises a display component, an optical adhesive layer and a cover plate which are stacked; wherein the optical adhesive layer comprises at least one layer of the optical adhesive according to any one of claims 1 to 6; There is at least one cover plate, and adjacent cover plates and / or the cover plate and the display assembly are bonded together via the optical adhesive layer, wherein a conductive layer is further provided on the bonding interface of the optical adhesive layer.

20. The device according to claim 19, characterized in that The conductive layer is made of one of ITO and metal wire.

21. The device according to claim 20, characterized in that The conductive layer is a patterned ITO structure.

22. The device according to claim 20, characterized in that The metal wires include nano silver wires.

23. The device according to claim 19, characterized in that The cover plate is made of polyethylene terephthalate, polyimide, thermoplastic polyurethane elastomer rubber or ultra-thin glass.

24. The device according to claim 19, characterized in that The cover plate is a polarizer.

Citation Information

Cited By

  • Adhesive tape capable of losing adhesive force after being electrified as well as preparation method and application of adhesive tape

    CN119799193A

  • Adhesive tape that loses adhesion after being powered on, preparation method thereof, and application thereof

    CN119799193B