Method for combined extraction of ferroniobium from Bayan Obo rare earth tailings

Through the method of strengthening the leaching of sulfuric acid calcination-fluorosaline second stage and pickling-hydrogen peroxide precipitation reaction, the problems of low extraction efficiency and environmental pollution in Baiyun Obo rare earth tailings are solved, and efficient ferroniobium combination is achieved Extraction improves recycling efficiency and reduces costs.

CN118979161AActive Publication Date: 2024-11-19CHINA UNIV OF MINING & TECH

Patent Information

Application Number
CN202411056505.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

In the prior art, the efficiency of extracting niobium from Baiyun Obo rare earth tailings is low, and the use of high concentration of hydrofluoric acid leads to environmental pollution and equipment corrosion, and other metals cannot be effectively recovered, resulting in low recycling benefits.

Method used

The two-stage leaching method of enhanced sulfuric acid calcination-fluorine salt was used to combine pickling and hydrogen peroxide precipitation reaction to achieve the joint extraction of niobium in Baiyun Obo rare earth tailings, avoid the use of hydrofluoric acid, and improve the extraction rate of niobium and iron. .

Benefits of technology

Improve the extraction efficiency and recycling efficiency of niobium and iron, reduce environmental pollution, and realize efficient joint extraction of niobium in Baiyun Obo rare earth tailings. The niobium leaching rate can reach 82%, the iron extraction rate can reach 45%, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979161A_ABST
    Figure CN118979161A_ABST
Patent Text Reader

Abstract

The invention relates to a method for combined extraction of ferroniobium from Bayan Obo rare earth tailings, belongs to the technical field of mineral recovery metallurgy, and solves at least one of the problems of low recovery benefit, environmental pollution caused by hydrofluoric acid and low niobium extraction efficiency in the prior art. The method comprises the following steps: carrying out acid pickling on the Bayan Obo rare earth tailings, and filtering to obtain an acid pickling solution and filter residues; drying the filter residue, mixing with ammonium sulfate and concentrated sulfuric acid, roasting, and primarily leaching niobium; the mixture obtained after primary leaching is mixed with villiaumite and water, niobium is leached for the second time, solid-liquid separation is conducted, niobium is extracted from obtained filtrate, and raffinate and extraction liquid containing niobium ions are obtained; mixing the pickling solution and the raffinate, adjusting the pH value to 3-4.5, then adding a hydrogen peroxide solution, and carrying out precipitation reaction to form Fe (OH) 3 precipitate; by means of the method, joint extraction of niobium and iron in the Bayan Obo rare earth tailings can be achieved, hydrofluoric acid is avoided, and the leaching rate of niobium is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral recovery metallurgy, and in particular to a method for jointly extracting ferroniobium from Bayan Obo rare earth tailings. Background Art

[0002] The Bayan Obo rare earth tailings are the products of Baotou Iron and Steel Mine after iron selection, rare earth selection and mixed flotation, and are the raw materials for the production of niobium concentrate. The mineral composition of Bayan Obo rare earth tailings is complex, mainly magnetite, pyrite, dolomite, fluorite and quartz, and contains a wide variety of niobium minerals and niobium minerals. Among them, the iron oxide content is 28.464%, the magnesium oxide content is 5.573%, and the calcium oxide content is 13.398%. Excessive iron, magnesium and calcium content affects the extraction of niobium. The niobium oxide content is 0.10%, which exceeds the boundary grade of niobium oxide by 0.05%. The increasing rare earth tailings are piled up in the tailings pond, with low utilization value, occupying land and polluting the environment. Excessive tailings may also cause the tailings pond to burst, which is very dangerous. The problem of reasonable recycling of tailings remains to be solved.

[0003] The prior art only has methods for extracting and recovering niobium from the Bayan Obo rare earth ore, but no methods for recovering and treating the Bayan Obo rare earth tailings. When the prior method for extracting niobium from the Bayan Obo rare earth ore is used to extract niobium from the Bayan Obo rare earth tailings, the niobium extraction efficiency is low. In addition, the prior art uses a mixed leaching of high-concentration hydrofluoric acid and sulfuric acid. During the leaching process, hydrofluoric acid is easily volatile when heated, which pollutes the environment and harms human health. Hydrofluoric acid is easily corroded by equipment, which increases the cost of extracting niobium. In addition, the prior method can only extract niobium, but does not recover other metals, and the recovery efficiency is low. Summary of the invention

[0004] In view of the above analysis, the present invention aims to provide a method for the combined extraction of niobium iron from the Bayan Obo rare earth tailings to solve at least one of the following problems existing in the existing methods: (1) only niobium can be extracted, and other metals are not recovered, resulting in low recovery efficiency; (2) hydrofluoric acid pollutes the environment, harms human health and corrodes equipment; (3) the efficiency of niobium extraction is low.

[0005] The present invention provides a method for jointly extracting ferroniobium from Bayan Obo rare earth tailings, the method comprising:

[0006] Step (1): pickling the Bayan Obo rare earth tailings, filtering them, and obtaining a pickling solution and filter residue;

[0007] Step (2): drying the filter residue, mixing it with ammonium sulfate and concentrated sulfuric acid, roasting it, and leaching niobium for the first time; mixing the mixture after the first leaching with fluoride salt and water, leaching niobium for the second time, separating the solid and liquid, extracting niobium from the obtained filtrate, and obtaining a raffinate and an extract containing niobium ions;

[0008] Step (3): The pickling liquid and the raffinate are mixed, the pH is adjusted to 3-4.5, and then a hydrogen peroxide solution is added to perform a precipitation reaction to form a Fe(OH)3 precipitate.

[0009] Preferably, in step (1), dilute hydrochloric acid is used for pickling.

[0010] Preferably, the concentration of the dilute hydrochloric acid is 2-2.5 mol / L.

[0011] Preferably, the ratio of the volume of the dilute hydrochloric acid to the mass of the low-grade niobium-containing ore is 5-10:1.

[0012] Preferably, the pickling temperature is 60-90°C.

[0013] Preferably, the pickling time is 1-1.5h.

[0014] Preferably, in step (3), adjusting the pH to 3-4.5 comprises: first adding 5-7 mol / L NaOH solution to adjust the pH to 2-2.5, and then adding 1-2 mol / L Na2CO3 solution to adjust the pH to 3-4.5.

[0015] Preferably, in step (3), the mass concentration of the hydrogen peroxide solution is 25-30%.

[0016] Preferably, the volume ratio of the mixed solution of the pickling liquid and the raffinate to the hydrogen peroxide solution is 20:1-5.

[0017] Preferably, in step (3), the temperature of the precipitation reaction is 50-80°C.

[0018] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0019] 1. The method of the present invention extracts niobium from the Bayan Obo rare earth tailings by ammonium sulfate-enhanced sulfuric acid roasting-fluoride salt two-stage leaching, and extracts iron by precipitation reaction of the pickling solution and the raffinate, thereby realizing the combined extraction of niobium and iron from the Bayan Obo rare earth tailings (the niobium leaching rate of the preferred implementation method can reach 82%, and the iron extraction rate can reach 45%), with high recovery efficiency.

[0020] 2. The present invention adopts the method of ammonium sulfate enhanced sulfuric acid roasting-fluoride salt two-stage leaching to effectively improve the niobium extraction efficiency in Bayan Obo rare earth tailings. Sulfuric acid roasting destroys the mineral structure and releases niobium elements. Ammonium sulfate enhanced sulfuric acid roasting makes fluoride ions and niobium easily complex to form NbF6 - and NbOF5 2-, so that niobium ions enter the leaching solution, the leaching rate of niobium (also called extraction rate) is increased, thereby improving the efficiency of niobium extraction; and the present invention does not use hydrofluoric acid, reducing environmental pollution and the harm caused by hydrofluoric acid.

[0021] 3. In the Bayan Obo rare earth tailings of the present invention, the content of niobium is low and the content of silicon oxide is high. The niobium in silicon oxide cannot be leached out by sulfuric acid leaching in the existing method, and the existing hydrofluoric acid leaching will pollute the environment. In the present invention, fluoride ions are added during the water leaching process. On the one hand, the fluoride ions destroy silicates in the acidic solution and release the niobium contained in the silicates. On the other hand, the fluoride ions are easily complexed with niobium to form NbF6 - and NbO5 2- , so that niobium ions enter the leaching solution, and the leaching rate of niobium is increased. The reason why fluoride salt is not added in step (1) is that fluoride salt reacts easily with strong acid (concentrated sulfuric acid) to generate hydrofluoric acid, which volatilizes under high temperature conditions, which not only fails to destroy the silicate mineral structure, but also causes environmental pollution.

[0022] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0024] Figure 1 The present invention is a flow chart of the method for jointly extracting ferroniobium from Bayan Obo rare earth tailings. DETAILED DESCRIPTION

[0025] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0026] The present invention provides a method for jointly extracting ferroniobium from Bayan Obo rare earth tailings, such as Figure 1 As shown, the method includes:

[0027] Step (1): pickling the Bayan Obo rare earth tailings, filtering them, and obtaining a pickling solution and filter residue;

[0028] Step (2): drying the filter residue, mixing it with ammonium sulfate and concentrated sulfuric acid, roasting it, and leaching niobium for the first time; mixing the mixture after the first leaching with fluoride salt and water, leaching niobium for the second time, separating the solid and liquid, extracting niobium from the obtained filtrate, and obtaining a raffinate and an extract containing niobium ions;

[0029] Step (3): The pickling liquid and the raffinate are mixed, the pH is adjusted to 3-4.5, and then a hydrogen peroxide solution is added to perform a precipitation reaction to form a Fe(OH)3 precipitate.

[0030] Compared with the prior art, the method of the present invention extracts niobium from the Bayan Obo rare earth tailings by ammonium sulfate-enhanced sulfuric acid roasting-fluoride salt two-stage leaching, and extracts iron by precipitation reaction of the pickling solution and the raffinate, thereby realizing the combined extraction of niobium and iron from the Bayan Obo rare earth tailings with high recovery efficiency.

[0031] Exemplarily, the mass content of niobium oxide in the Bayan Obo rare earth tailings is less than 0.12%.

[0032] It should be noted that the Bayan Obo rare earth tailings are the products of Baotou Iron and Steel Mine after iron and rare earth selection and mixed flotation. Its components include fluorite, quartz, magnetite and dolomite. The specific chemical composition is shown in Table 1 below.

[0033] The method of the present invention is applicable to the Baiyunebo rare earth tailings. In the Baiyunebo rare earth tailings, the niobium content is low and the silicon oxide content is high. The niobium in the silicon oxide cannot be leached only by sulfuric acid leaching in the existing method, and the existing hydrofluoric acid leaching will pollute the environment. The present invention adds fluoride ions during the water leaching process. On the one hand, the fluoride ions destroy silicates and release niobium contained in silicates. On the other hand, the fluoride ions are easily complexed with niobium to form NbF6 - and NbOF5 2- , so that niobium ions enter the leaching solution and increase the niobium leaching rate.

[0034] In order to initially extract iron from the tailings, and to avoid the generation of insoluble sulfates during the ammonium sulfate-sulfuric acid roasting process, and to avoid the violent reaction of sulfuric acid and carbonates, and the danger of overflowing the pot, the present invention firstly pickles the Bayan Obo rare earth tailings to remove carbonate impurities in the Bayan Obo rare earth tailings, improve the subsequent niobium leaching efficiency, and initially leach iron into a dilute hydrochloric acid solution. The carbonate impurities include carbonate forms of iron, calcium, magnesium, aluminum and other ions.

[0035] Illustratively, in step (1), the pickling is performed using dilute hydrochloric acid.

[0036] Exemplarily, the concentration of the dilute hydrochloric acid is 2-2.5 mol / L.

[0037] Exemplarily, the ratio of the volume of the dilute hydrochloric acid to the mass of the Bayan Obo rare earth tailings is 5-10 mL: 1 g.

[0038] Exemplarily, the pickling temperature is 60-90° C. If the pickling temperature is too low, the iron extraction rate is low, and if the pickling temperature is too high, niobium will enter the pickling solution, affecting the final leaching rate of niobium.

[0039] Exemplarily, the pickling time is 1-1.5h.

[0040] Specifically, before the Bayan Obo rare earth tailings are acid-washed, the Bayan Obo rare earth tailings are first sieved through an 80-mesh sieve to remove leaves, small stones and other debris in the Bayan Obo rare earth tailings, and then the sieved material is dried at 100-120° C. for 4-5 hours.

[0041] The method of the present invention is applicable to the Baiyunebo rare earth tailings. In the Baiyunebo rare earth tailings, the niobium content is low and the silicon oxide content is high. The niobium in the silicon oxide cannot be leached only by sulfuric acid leaching in the existing method, and the existing hydrofluoric acid leaching will pollute the environment. The present invention adds fluoride ions during the water leaching process. On the one hand, the fluoride ions destroy silicates and release niobium contained in silicates. On the other hand, the fluoride ions are easily complexed with niobium to form NbF6 - and NbOF5 2- , so that niobium ions enter the leaching solution and increase the niobium leaching rate.

[0042] Exemplarily, in step (2), the ratio of the mass of the Bayan Obo rare earth tailings to the mass of ammonium sulfate and the volume of concentrated sulfuric acid is 1 g: 0.15-0.4 g: 1-1.5 mL.

[0043] For example, in step (2), ammonium sulfate is first added to the Bayan Obo rare earth tailings, and after the Bayan Obo rare earth tailings and ammonium sulfate are mixed, concentrated sulfuric acid is added and mixed evenly. This can promote the consistency of the mineral reaction degree and improve the leaching rate of niobium.

[0044] Illustratively, in step (2), the temperature of the initial leaching is 260-300°C, such as 270°C, 280°C, or 290°C.

[0045] Exemplarily, in step (2), the initial leaching time is 2.0-2.5 h, such as 2.1 h, 2.2 h, 2.3 h, 2.4 h.

[0046] Exemplarily, after the initial leaching is completed, the sample is taken out and cooled to room temperature.

[0047] Exemplarily, in step (2), the mass ratio of the Bayan Obo rare earth tailings to the fluoride salt is 1:0.15-0.25. If there is too much fluoride salt, sodium fluoride will be wasted and too many fluoride ions will be produced, which are difficult to handle. If there is too little fluoride salt, the niobium extraction rate will be reduced and niobium cannot be fully extracted.

[0048] In the present invention, in step (2), fluoride ions destroy silicates in an acidic solution, thereby releasing niobium contained in the silicates.

[0049] For example, in step (2), after the mixture after the initial leaching is mixed with fluoride salt and water, the pH of the mixture is adjusted to 1.5-1.8, for example, pH 1.5, 1.6, 1.7, 1.8. If the pH value is too low, hydrofluoric acid is easily formed; if the pH value is too high, the leaching rate of niobium is affected.

[0050] Specifically, fluoride salt is first added to the mixture after the primary leaching, water is added after mixing evenly, and then a pH adjuster is added to adjust the pH of the solution.

[0051] Illustratively, the pH of the mixture is adjusted using dilute sulfuric acid and / or sodium hydroxide.

[0052] Exemplarily, in step (2), the ratio of the mass of Bayan Obo rare earth tailings to the volume of water is 1 g: 20-30 mL.

[0053] Illustratively, in step (2), the temperature of the secondary leaching is 60-80°C, such as 60°C, 65°C, 70°C, 75°C.

[0054] Exemplarily, in step (2), the secondary leaching time is 1-2 hours.

[0055] Illustratively, in step (2), stirring is performed during the secondary leaching process at a stirring speed of 300-500 r / min.

[0056] Illustratively, in step (2), the fluoride salt is sodium fluoride.

[0057] Illustratively, in step (2), extracting niobium from the obtained filtrate comprises: fixing the volume of the filtrate to 500 mL, concentrating the fixed niobium solution by 50 times, placing the concentrate and MIBK into a separatory funnel, shaking and then standing until an organic phase and an aqueous phase are stably separated in the separatory funnel, and separating the organic phase; back-extracting niobium from the organic phase, taking the organic phase and 0.5 mol / L sulfuric acid and placing them into a separatory funnel, shaking the separatory funnel, and extracting the aqueous phase after the aqueous phase and the organic phase are completely separated, and the aqueous phase is obtained. The aqueous phase is a niobium-containing solution.

[0058] Exemplarily, the volume ratio of the concentrate to MIBK is 1:1-2.

[0059] Exemplarily, the volume ratio of the organic phase to sulfuric acid is 1:4-5.

[0060] Illustratively, in step (3), adjusting the pH to 3-4.5 comprises: first adding 5-7 mol / L NaOH solution to adjust the pH to 2-2.5, and then adding 1-2 mol / L Na2CO3 solution to adjust the pH to 3-4.5.

[0061] Exemplarily, in step (3), the role of hydrogen peroxide is to convert Fe 2+ Oxidized to Fe 3+ , the mass concentration of the hydrogen peroxide solution is 25-30%.

[0062] Exemplarily, the volume ratio of the mixed solution of the pickling liquid and the raffinate to the hydrogen peroxide solution is 20:1-5.

[0063] For example, in step (3), the temperature of the precipitation reaction is 50-80° C. Too low or too high a temperature will affect the precipitation rate of iron.

[0064] Exemplarily, step (3) includes placing the precipitate in a muffle furnace and calcining it at 600-700° C. for 1-2 hours in order to remove water from the precipitate.

[0065] The method for combined extraction of ferroniobium from Bayan Obo rare earth tailings of the present invention is further illustrated below by means of specific examples.

[0066] The main components of the Bayan Obo rare earth tailings in the following examples and comparative examples are shown in Table 1.

[0067] Table 1

[0068] Components <![CDATA[Na2O]]> MgO <![CDATA[Al2O3]]> <![CDATA[SiO2]]> CaO <![CDATA[TiO2]]> MnO <![CDATA[Fe2O3]]> <![CDATA[Nb2O5]]> Wt.% 2.28 5.57 1.74 19.17 13.40 0.78 1.40 28.50 0.10

[0069] Example 1

[0070] This embodiment provides a method for jointly extracting ferroniobium from Bayan Obo rare earth tailings, the method comprising:

[0071] (1) Pretreatment: The Bayan Obo rare earth tailings were screened through an 80-mesh sieve to remove leaves, small stones and other debris from the Bayan Obo rare earth tailings, and the screened material was placed in a tray and dried at 100°C for 4 hours.

[0072] (2) Hydrochloric acid pickling: Take the Bayan Obo rare earth tailings and put them into a round-bottom flask. Add 2 mol / L hydrochloric acid at a liquid-to-solid ratio of 7:1. After connecting the round-bottom flask to a condensation reflux device, place it in a water bath at a temperature of 70°C. The rotor speed is 400 r / min and the pickling time is 1.2 h.

[0073] (3) Filtration and separation: Use a vacuum filter to separate the filtrate and filter residue after pickling, dry the filter residue at 100°C for 1 hour, and retain the pickling liquid.

[0074] The removal rates of iron, magnesium, calcium and aluminum in the Bayan Obo rare earth tailings after pickling were detected and calculated by XRF, and they were 29.51%, 64.76%, 66.85% and 49.09% respectively. The recovery rate of niobium was 86.84%, which refers to the ratio of the remaining niobium in the tailings after pickling to the niobium in the tailings before pickling.

[0075] (4) Ammonium sulfate-enhanced sulfuric acid roasting and primary leaching: 2 g of tailings after acid washing are placed in a glass quartz crucible, and 0.6 g of ammonium sulfate and 2.5 mL of 98% concentrated sulfuric acid are added (the ratio of the mass of tailings to the mass of ammonium sulfate and the volume of concentrated sulfuric acid is 1:0.3:1.25). The tailings are first mixed with ammonium sulfate and then with concentrated sulfuric acid. The glass quartz crucible is placed in a muffle furnace at 290°C and roasted for 2 hours. After the roasting is completed, the quartz glass crucible is taken out and cooled to room temperature.

[0076] (5) Secondary leaching of fluoride salt: Add 0.3 g of sodium fluoride (the mass ratio of tailings to sodium fluoride is 1:0.15) to the glass quartz crucible in step (4), add 50 mL of deionized water (the volume of water to the mass of tailings is 25:1), adjust the pH to 1.7, and place the glass quartz crucible in a constant temperature water bath. The water immersion temperature is 80°C, the leaching time is 1 hour, and the rotor speed is 400 r / min.

[0077] (6) Filtration and separation: Use a vacuum filter to separate the filtrate and residue after leaching.

[0078] Detection of niobium extraction rate: The niobium content in the filtrate after the secondary leaching was detected by ICP-MS and the niobium leaching rate (extraction rate) was calculated to be 82%. The leaching rate is the ratio of the niobium content in the filtrate after the secondary leaching to the niobium content in the tailings before the primary leaching.

[0079] (7) Extraction of niobium: The filtrate was fixed to 500 mL, and the niobium solution was concentrated 50 times. The concentrated solution and MIBK (volume ratio of 1:1) were placed in a separatory funnel. The separatory funnel was shaken for 3 minutes. After the shaking, the separatory funnel was left to stand until the organic phase (extract solution) and the aqueous phase (raffinate) were stably separated in the separatory funnel to separate the organic phase. The niobium in the organic phase was extracted by back-extracting the organic phase and the organic phase and 0.5 mol / L sulfuric acid were placed in a separatory funnel in a volume ratio of 1:4. The separatory funnel was shaken for 5 minutes until the aqueous phase and the organic phase were completely separated. The aqueous phase was extracted and the niobium content was detected.

[0080] The niobium in the solution was extracted with MIBK, and the extraction rate reached 87.2%. The niobium was stripped with 0.5 mol / L sulfuric acid solution, and the dissolution rate of niobium was almost 100%.

[0081] (8) mixing the pickling solution and the raffinate, adding 5 mol / L NaOH solution to the mixed solution to adjust the pH value of the mixed solution to 2, and then adding 1 mol / L Na2CO3 to adjust the pH value of the mixed solution to 3;

[0082] Add 25% H2O2 solution to the mixed solution, the volume ratio of the mixed solution of pickling solution and raffinate to hydrogen peroxide solution is 20:3, and Fe 2+ Oxidized to Fe 3+ , forming Fe(OH)3 precipitate, separating the precipitate from the filtrate with a vacuum filter, and recovering the precipitate. The precipitate was placed in a muffle furnace and calcined at 600℃ for 1h.

[0083] The iron extraction rate is 45%, and the iron extraction rate is the ratio of the iron content in the product after iron extraction roasting to the iron content in the tailings before acid washing.

[0084] Example 2

[0085] This example provides the effect of the amount of ammonium sulfate added on the niobium extraction rate, and adopts a method for jointly extracting niobium iron from Bayan Obo rare earth tailings similar to Example 1, except that the amount of ammonium sulfate added is 0.1g, 0.2g, 0.4g, 0.5g, 0.6g, 0.7g, and 0.8g, respectively.

[0086] Table 2

[0087] The amount of ammonium sulfate 0.1g 0.2g 0.4g 0.5g 0.6g 0.7g 0.8g Niobium leaching rate 70% 71% 78% 78% 78% 76% 78%

[0088] It can be seen from the data in Table 2 and Example 1 that when the amount of ammonium sulfate added is 0.3-0.8 g (that is, the mass ratio of tailings to ammonium sulfate is 1:0.15-0.4), the leaching rate is maintained above 76%.

[0089] Example 3

[0090] This example provides the effect of the amount of concentrated sulfuric acid added on the niobium extraction rate, and adopts a method similar to Example 1 for the combined extraction of ferroniobium from the Bayan Obo rare earth tailings, except that the solid-liquid ratio (g / mL) of the tailings to the concentrated sulfuric acid is 1:0.25, 1:0.5, 1:0.75, 1:1, and 1:1.5, respectively. The results are shown in Table 3.

[0091] Table 3

[0092]

[0093] It can be seen from the data in Table 3 and Example 1 that when the solid-liquid ratio of tailings to concentrated sulfuric acid is 1:1-1.5, the final leaching rate of niobium can reach more than 78%.

[0094] Example 4

[0095] This example provides the effect of roasting temperature on niobium extraction rate, using a method similar to Example 1 for combined extraction of niobium iron from Bayan Obo rare earth tailings, except that the roasting temperatures are 200°C, 230°C, 260°C, 280°C, 300°C, and 320°C, respectively. The results are shown in Table 4.

[0096] Table 4

[0097] Calcination temperature 200℃ 230℃ 260℃ 280℃ 300℃ 320℃ Niobium leaching rate 67% 64% 71% 82% 82% 29%

[0098] It can be seen from the data in Table 4 and Example 1 that when the roasting temperature is between 260 and 300°C, the niobium extraction rate reaches more than 70%, and when the roasting temperature is between 260 and 300°C, the niobium extraction rate reaches more than 71%.

[0099] Example 5

[0100] This example provides the effect of roasting time on niobium extraction rate, using a method similar to Example 1 for combined extraction of ferroniobium from Bayan Obo rare earth tailings, except that the roasting times are 0.5h, 1.0h, 1.5h, and 2.5h, respectively. The results are shown in Table 5.

[0101] Table 5

[0102] Roasting time 0.5h 1.0h 1.5h 2.5h Niobium leaching rate 73% 72% 76% 82%

[0103] It can be seen from the data in Table 5 and Example 1 that when the roasting time exceeds 2 h, the niobium extraction rate remains substantially unchanged. Therefore, the preferred roasting time of the present invention is 2-2.5 h.

[0104] Example 6

[0105] This example provides the effect of the amount of sodium fluoride added during the water leaching process on the niobium extraction rate. A method similar to Example 1 is used to jointly extract ferroniobium from the Bayan Obo rare earth tailings, except that the amount of sodium fluoride added is 0.1 g, 0.2 g, 0.4 g, and 0.5 g, respectively. The results are shown in Table 6.

[0106] Table 6

[0107] Sodium fluoride dosage 0.1g 0.2g 0.4g 0.5g Niobium leaching rate 13% 31% 82% 82%

[0108] It can be seen from the data in Table 6 and Example 1 that for 2 g of tailings, the niobium leaching rate is highest when the amount of sodium fluoride used is above 0.3 g, and the niobium leaching rate remains basically unchanged when the amount of sodium fluoride used exceeds 0.3 g.

[0109] Example 7

[0110] This example provides the effect of pH value on niobium extraction rate during water leaching, and adopts a method for combined extraction of niobium iron from Bayan Obo rare earth tailings similar to Example 1, except that the pH value is adjusted by dripping sodium hydroxide solution and sulfuric acid solution, and the pH value of the leaching solution is adjusted to 2.0.

[0111] The niobium leaching rate in this example is 67%.

[0112] Example 8

[0113] This example provides the effect of the secondary leaching temperature on the niobium extraction rate, and adopts a method for combined extraction of niobium iron from Bayan Obo rare earth tailings similar to that of Example 1, except that the secondary leaching temperature is 50°C.

[0114] The niobium leaching rate in this example is 68%.

[0115] Example 9

[0116] This embodiment provides the effect of the amount of dilute hydrochloric acid used on the iron extraction rate, and adopts a method for jointly extracting niobium iron from the Bayan Obo rare earth tailings similar to that of Example 1, except that in step (2), the liquid-to-solid ratio of dilute hydrochloric acid to the Bayan Obo rare earth tailings is 3:1.

[0117] The iron extraction rate in this example is 39%.

[0118] Example 10

[0119] This embodiment provides the effect of the amount of H2O2 solution on the iron extraction rate, and adopts a method similar to Example 1 for the combined extraction of niobium iron from the Bayan Obo rare earth tailings, except that the volume ratio of the mixed solution of the pickling solution and the raffinate to the hydrogen peroxide solution is 20:0.5.

[0120] The iron extraction rate in this example is 35%.

[0121] Comparative Example 1

[0122] The comparative example adopts the method of ammonium sulfate and sulfuric acid roasting + water leaching + oxalic acid leaching to extract niobium from the Bayan Obo rare earth tailings. The method is similar to the method in Example 1, except that: after the initial roasting and leaching by ammonium sulfate and concentrated sulfuric acid roasting, water is added to the mixture for water leaching, and then solid-liquid separation is performed to obtain a first filtrate and a first filter residue, the first filter residue is mixed with oxalic acid, and after the oxalic acid leaching is completed, solid-liquid separation is performed to obtain a second filtrate and a second filter residue, and the total content of niobium in the obtained first filtrate and the second filtrate is detected and the extraction rate is calculated to be 54.6%.

[0123] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for jointly extracting ferroniobium from Bayan Obo rare earth tailings, characterized in that: The method comprises: Step (1): pickling the Bayan Obo rare earth tailings, filtering them, and obtaining a pickling solution and filter residue; Step (2): drying the filter residue, mixing it with ammonium sulfate and concentrated sulfuric acid, roasting it, and leaching niobium for the first time; mixing the mixture after the first leaching with fluoride salt and water, leaching niobium for the second time, separating the solid and liquid, extracting niobium from the obtained filtrate, and obtaining a raffinate and an extract containing niobium ions; Step (3): The pickling liquid and the raffinate are mixed, the pH is adjusted to 3-4.5, and then a hydrogen peroxide solution is added to perform a precipitation reaction to form a Fe(OH)3 precipitate.

2. The method according to claim 1, characterized in that In step (1), dilute hydrochloric acid is used for pickling.

3. The method according to claim 2, characterized in that The concentration of the dilute hydrochloric acid is 2-2.5 mol / L.

4. The method according to claim 3, characterized in that The ratio of the volume of the dilute hydrochloric acid to the mass of the low-grade niobium-containing ore is 5-10:

1.

5. The method according to claim 1, characterized in that The pickling temperature is 60-90°C.

6. The method according to claim 1, characterized in that The pickling time is 1-1.5h.

7. The method according to claim 1, characterized in that In step (3), the pH value is adjusted to 3-4.5, comprising: first adding 5-7 mol / L NaOH solution to adjust the pH value to 2-2.5, and then adding 1-2 mol / L Na2CO3 solution to adjust the pH value to 3-4.

5.

8. The method according to claim 1, characterized in that In step (3), the mass concentration of the hydrogen peroxide solution is 25-30%.

9. The method according to claim 8, characterized in that In step (3), the volume ratio of the mixed solution of the pickling liquid and the raffinate to the hydrogen peroxide solution is 20:1-5.

10. The method according to claim 1, characterized in that In step (3), the temperature of the precipitation reaction is 50-80°C.

Citation Information

Patent Citations

  • Method for decomposing ore concentrate containing tantalum, niobium and rare-earth element

    CN101440429A

  • Method for extracting tantalum and niobium and producing potassium fluosilicate from tungsten smelting slag

    CN102952951A

  • Method for extracting niobium from Bayan Obo mine tailing

    CN103361495A

  • Method for using low-grade niobium concentrate to produce niobium-iron alloy and rare earth double sulfate salt

    CN104894363A

  • Method for comprehensively recovering rare earth, niobium and silicon from Baiyuneboite tailings

    CN105624396A

Cited By

  • Method for synergistically decomposing low-grade niobium ore and fluorine-containing ore

    CN120624849A

  • Method for recovering indium from indium-containing lead smoke dust

    CN120776149A

  • A method for recovering indium from indium-containing lead fumes

    CN120776149B