Positive pole piece, battery, energy storage device and electric equipment

By combining the first positive electrode material and the second positive electrode material in the positive electrode material layer of the lithium-ion battery, the distribution of spherical and rod-shaped particles and vanadium elements are used to solve the problem of balance between the positive electrode sheet duct radiance and battery capacity, and low latencies are achieved battery with high capacity performance.

CN118983395AActive Publication Date: 2024-11-19XIAMEN HITHIUM ENERGY STORAGE TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411044496.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

While increasing the capacity of lithium-ion batteries, the ductility rate of the positive electrode sheet becomes larger, resulting in the problem of difficult battery performance balance.

Method used

A positive electrode material layer is adopted, including a first positive electrode material (LiFexTiyPO4/C) and a second positive electrode material (LiFexTiyVzPO4/C), wherein spherical particles and rod-shaped particles in the second positive electrode material hinder the rolling deformation, vanadium element slows down the capacity and regulates the Material ratio and particle size distribution to reduce ductility.

Benefits of technology

While reducing the radiating rate of the positive electrode sheet, the capacity performance of the lithium-ion battery is maintained or improved, the risk of cracking at the edge of the battery is reduced, and the discharge capacity is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983395A_ABST
    Figure CN118983395A_ABST
Patent Text Reader

Abstract

The invention provides a positive pole piece, a battery, an energy storage device and electric equipment, the positive pole piece comprises a positive current collector, at least one surface of the positive current collector is provided with a positive material layer, and the positive material layer comprises a first positive material and a second positive material; the Dv50 of the first positive electrode material is 800-1000 nm, the second positive electrode material comprises spherical particles and rod-shaped particles, the Dv50 of the spherical particles is 300-500 nm, the average length of the rod-shaped particles is 2-6 [mu] m, and the second positive electrode material comprises vanadium element.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to a positive electrode sheet, a battery, an energy storage device, and an electrical device. Background Art

[0002] Lithium-ion batteries have the characteristics of high specific energy, high operating voltage, low self-discharge rate, small size and light weight. They are widely used in various fields such as energy storage, portable electronic devices and electric vehicles.

[0003] Lithium-ion batteries based on lithium iron phosphate (LiFePO4) cathode materials offer the advantages of high safety and stability. With the increasing demand for battery capacity in energy storage scenarios, smaller LiFePO4 particle sizes are currently being used. However, this leads to increased elongation of the positive electrode sheet during rolling. However, simply increasing the particle size of the LiFePO4 material decreases battery capacity. Balancing battery capacity performance while reducing the elongation of the positive electrode sheet has become a pressing technical challenge. Summary of the Invention

[0004] In order to solve the above technical problems, the present application discloses a positive electrode sheet, a battery, an energy storage device and an electrical equipment, which balance the capacity performance of the battery while reducing the elongation of the positive electrode sheet.

[0005] In the first aspect, the present application provides a positive electrode plate, including a positive electrode current collector, at least one side of the positive electrode current collector having a positive electrode material layer, the positive electrode material layer including a first positive electrode material and a second positive electrode material; the Dv50 of the first positive electrode material is 800nm~1000nm, the second positive electrode material includes spherical particles and rod-shaped particles, the Dv50 of the spherical particles is 300nm~500nm, the average length of the rod-shaped particles is 2μm~6μm, and the second positive electrode material includes vanadium.

[0006] In some embodiments of the present application, based on the mass of the positive electrode material layer, the mass percentage of the first positive electrode material is 90% to 93%, and the mass percentage of the second positive electrode material is 2% to 5%.

[0007] In some embodiments of the present application, the first cathode material has a chemical formula of LiFe x Ti y PO4 / C, where x+y=1 and 0 <y≤0.03。

[0008] In some embodiments of the present application, the second cathode material has a chemical formula of LiFe x Ti y V zPO4 / C, where x+y+Z=1 and 0 <y≤0.03,0<z≤0.03。

[0009] In some embodiments of the present application, the elongation of the positive electrode sheet is 0.8% to 2.3%.

[0010] In some embodiments of the present application, the button cell containing the positive electrode sheet has a 0.5C discharge capacity of 140 mAh / g to 150 mAh / g, and a 1C discharge capacity of 128 mAh / g to 137 mAh / g.

[0011] In some embodiments of the present application, the compacted density of the mixture of the first positive electrode material and the second positive electrode material is 2.3 g / cm 3 ~2.5g / cm 3 .

[0012] In some embodiments of the present application, the positive electrode plate further includes a conductive agent and a binder. Based on the mass of the positive electrode material layer, the mass percentage of the conductive agent is 1% to 3%, and the mass percentage of the binder is 1% to 3%.

[0013] In a second aspect, the present application provides a battery comprising the positive electrode sheet described in the first aspect.

[0014] In a third aspect, the present application provides an energy storage device comprising a housing and at least one battery as described in the second aspect, wherein the battery is housed in the housing.

[0015] In a fourth aspect, the present application provides an electrical device comprising the energy storage device described in the third aspect, wherein the energy storage device supplies power to the electrical device.

[0016] Compared with the prior art, this application has at least the following beneficial effects:

[0017] The present application provides a positive electrode sheet, a battery, an energy storage device, and an electrical device, wherein the positive electrode sheet includes a positive electrode current collector, at least one side of the positive electrode current collector has a positive electrode material layer, and the positive electrode material layer includes a first positive electrode material and a second positive electrode material; the Dv50 of the first positive electrode material is 800nm ​​to 1000nm; the second positive electrode material includes spherical particles and rod-shaped particles, the Dv50 of the spherical particles is 300nm to 500nm, the average length of the rod-shaped particles is 2μm to 6μm, and the second positive electrode material includes vanadium. The positive electrode sheet of the present application includes the above-mentioned first positive electrode material and the second positive electrode material, wherein the first positive electrode material is mainly used to provide capacity; in the second positive electrode material, the rod-shaped particles can hinder particle displacement and deformation during rolling, thereby reducing the elongation of the positive electrode sheet; the spherical particles have a smaller particle size and are used to fill the gaps in the first positive electrode material to further increase the capacity, and the vanadium in the second positive electrode material can slow down the decline in capacity. Under the joint action of the first positive electrode material and the second positive electrode material, the capacity performance of the battery can be balanced while reducing the elongation of the positive electrode sheet. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0019] Figure 1 A schematic structural diagram of a household energy storage system according to an embodiment of the present application;

[0020] Figure 2 A schematic structural diagram of an energy storage system according to an embodiment of the present application;

[0021] Figure 3 Schematic diagram of the positive electrode elongation test;

[0022] Figure 4 This is a scanning electron microscope (SEM) image of the first cathode material prepared in Example 1;

[0023] Figure 5 This is a SEM image of the second positive electrode material prepared in Example 1;

[0024] Figure 6 This is a cross-sectional SEM image of the positive electrode sheet of Example 1.

[0025] Explanation of the accompanying drawings: 1-energy storage device, 2-electric energy conversion device, 3-first user load, 4-second user load, 10-positive electrode current collector, 20-positive electrode material layer, 30-roller, 400-energy storage system, 410-high-voltage cable, 420-first electric energy conversion device, 430-second electric energy conversion device. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0027] In this application, terms such as "upper," "lower," "left," "right," "front," "back," "top," "bottom," "inner," "outer," "vertical," "horizontal," "transverse," and "longitudinal" indicate positions or locations based on the positions or locations shown in the accompanying drawings. These terms are primarily intended to better describe this application and its embodiments and are not intended to limit the devices, elements, or components indicated to having a specific orientation, or to being constructed or operated in a specific orientation.

[0028] Furthermore, some of the above terms may be used to express other meanings besides indicating a position or location. For example, the term "on" may also be used to indicate a dependency or connection in certain circumstances. Those skilled in the art will understand the specific meanings of these terms in this application based on the specific circumstances.

[0029] Furthermore, the terms "installed," "disposed," "provided with," "connected," and "connected" should be interpreted broadly. For example, they can refer to fixed connections, removable connections, or integral structures; mechanical connections or electrical connections; direct connections, indirect connections through an intermediary, or internal communication between two devices, elements, or components. Those skilled in the art will understand the specific meanings of these terms in this application based on the specific circumstances.

[0030] Furthermore, the terms "first," "second," etc., are primarily used to distinguish between different devices, elements, or components (which may or may not be of the same type and configuration), and are not intended to indicate or imply the relative importance or quantity of the devices, elements, or components indicated. Unless otherwise specified, "plurality" means two or more.

[0031] It should be noted that, in the content of this application, lithium-ion batteries are used as an example of batteries to explain this application, but the batteries of this application are not limited to lithium-ion batteries.

[0032] The present application provides a positive electrode sheet, comprising a positive electrode current collector, at least one side of which comprises a positive electrode material layer, the positive electrode material layer comprising a first positive electrode material and a second positive electrode material; the first positive electrode material has a Dv50 of 800 nm to 1000 nm, the second positive electrode material comprises spherical particles and rod-shaped particles, the spherical particles have a Dv50 of 300 nm to 500 nm, the rod-shaped particles have an average length of 2 μm to 6 μm, and the second positive electrode material comprises vanadium. For example, the first positive electrode material has a Dv50 of 800 nm, 850 nm, 900 nm, or 1000 nm, the spherical particles have a Dv50 of 300 nm, 320 nm, 350 nm, or 500 nm, and the rod-shaped particles have an average length of 2 μm, 3 μm, 5 μm, or 6 μm.

[0033] In the present application, Dv50 means the particle size at which the cumulative volume of particles reaches 50% from the smallest particle size side in the volume-based particle size distribution.

[0034] The positive electrode sheet of the present application includes the aforementioned first and second positive electrode materials. The first positive electrode material primarily provides capacity; the rod-shaped particles in the second positive electrode material prevent particle displacement and deformation during rolling, thereby reducing the elongation of the positive electrode sheet; the spherical particles in the second positive electrode material have a smaller particle size and are used to fill the gaps in the first positive electrode material to further increase capacity. The vanadium element in the second positive electrode material also mitigates capacity degradation. The combined effects of the first and second positive electrode materials balance the capacity performance of the lithium-ion battery while reducing the elongation of the positive electrode sheet.

[0035] In an optional embodiment, based on the mass of the positive electrode material layer, the mass percentage of the first positive electrode material is 90% to 93%, and the mass percentage of the second positive electrode material is 2% to 5%. For example, the mass percentage of the first positive electrode material is 90%, 91%, 92% or 93%, and the mass percentage of the second positive electrode material is 2%, 3%, 4% or 5%. By regulating the content of the first positive electrode material and the second positive electrode material within the above range, the first positive electrode material is mainly used to provide capacity, which is beneficial to balancing the capacity performance of the lithium-ion battery while reducing the elongation of the positive electrode sheet, and the second positive electrode material is used to reduce the elongation of the positive electrode sheet. In this way, the capacity performance of the lithium-ion battery can be balanced while reducing the elongation of the positive electrode sheet.

[0036] In an alternative embodiment, the first cathode material has the chemical formula LiFe x Ti yPO4 / C, where x + y = 1 and 0 < y ≤ 0.03. For example, y = 0.01, 0.02 or 0.03. The first positive electrode material with the above chemical formula can provide capacity, which is beneficial to improving the capacity performance of the lithium-ion battery.

[0037] In an optional embodiment, the second positive electrode material has the chemical formula LiFe x Ti y V z PO4 / C, where x + y + Z = 1, 0 < y ≤ 0.03, and 0 < z ≤ 0.03. For example, y = 0.01, 0.02 or 0.03, and z = 0.01, 0.02 or 0.03. The second positive electrode material with the above chemical formula can form rod-shaped particles and spherical particles. The rod-shaped particles can hinder the displacement and deformation of particles during rolling, thereby reducing the elongation rate of the positive electrode sheet. The spherical particles can fill the gaps of the first positive electrode material to further improve the capacity. The vanadium element can slow down the decline of the capacity.

[0038] In an optional embodiment, the elongation rate of the positive electrode sheet is 0.8% - 2.3%. For example, the elongation rate is 0.8%, 1%, 1.5%, 2% or 2.3%. Having a smaller elongation rate is beneficial to reducing the risk of edge cracking of the positive electrode sheet.

[0039] In an optional embodiment, the 0.5C discharge capacity of the coin cell containing the positive electrode sheet is 140 mAh / g - 150 mAh / g, and the 1C discharge capacity is 128 mAh / g - 137 mAh / g. For example, the 0.5C discharge capacity is 140 mAh / g, 143 mAh / g, 145 mAh / g or 150 mAh / g, and the 1C discharge capacity is 128 mAh / g, 132 mAh / g, 135 mAh / g or 137 mAh / g. Having a higher discharge capacity is beneficial to improving the capacity performance of the lithium-ion battery.

[0040] In an optional embodiment, the tap density of the mixture of the first positive electrode material and the second positive electrode material is 2.3 g / cm 3 ~2.5 g / cm 3 , for example, the tap density is 2.3 g / cm 3 , 2.4 g / cm 3 or 2.5 g / cm 3 . By controlling the tap density of the positive electrode material layer within the above range, it is beneficial to improving the capacity performance of the lithium-ion battery.

[0041] In an optional embodiment, the positive electrode plate further includes a conductive agent and a binder. Based on the mass of the positive electrode material layer, the mass percentage of the conductive agent is 1% to 3%, and the mass percentage of the binder is 1% to 3%. For example, the mass percentage of the conductive agent is 1%, 2%, 2.5% or 3%, and the mass percentage of the binder is 1%, 2%, 2.5% or 3%. This application does not particularly limit the types of conductive agents and binders. For example, conductive agents include but are not limited to conductive carbon black, carbon nanotubes, graphene, etc., and binders include but are not limited to at least one of polyvinylidene fluoride (PVDF), fluorine-containing resins, polypropylene resins, fiber-type binders, rubber-type binders and polyimide-type binders.

[0042] In an optional embodiment, the preparation method of the first positive electrode material comprises the following steps:

[0043] Step A: According to LiFe x Ti y The iron source, phosphorus source, lithium source, carbon source and titanium source were weighed in the required stoichiometric ratio of PO4 / C (x+y=1, y≤0.03), uniformly mixed on a ball mill, and then pure water was added as a dispersant, followed by high-energy ball milling;

[0044] Step B, spray drying the material after high-energy ball milling to form a powder;

[0045] Step C: placing the powder formed after spray drying into a vacuum atmosphere sintering furnace for high-temperature calcination, and then subjecting it to ball milling and crushing to obtain the first positive electrode material.

[0046] In step A, the iron source can be selected from ferrous oxalate, ferric phosphate or ferric oxide, the phosphorus source can be selected from lithium dihydrogen phosphate or ammonium dihydrogen phosphate, the lithium source can be selected from lithium carbonate or lithium hydroxide, the carbon source can be selected from glucose, sucrose or citric acid, and the titanium source can be selected from titanium tetrachloride or titanium oxalate; the ball-to-material ratio of the high-energy ball milling is 3 to 5:1, the rotation speed is 1000 r / min to 1500 r / min, and the ball milling time is 15 h to 20 h.

[0047] In step B, the pump speed of the spray drying is 8 mL / min to 12 mL / min, the drying temperature is 180° C. to 220° C., and the powder formed is granular.

[0048] In step C, the protective atmosphere is nitrogen, the sintering temperature is 650° C. to 750° C., and the sintering time is 5 h to 10 h.

[0049] In an optional embodiment, the preparation method of the second positive electrode material comprises the following steps:

[0050] Step a: According to LiFe x Ti y Vz Weigh the iron source, phosphorus source, carbon source, titanium source and vanadium source according to the stoichiometric ratio required in PO4 / C(x + y + Z = 1, and 0 < y ≤ 0.03, 0 < z ≤ 0.03), and after mixing, obtain a mixed metal salt solution; then prepare a strong base solution as a precipitant solution and prepare ammonia water as a complexing agent solution;

[0051] Step b: Place the prepared mixed metal salt solution, complexing agent solution and precipitant solution in a reaction kettle, continuously stir, keep the pH value of the reaction liquid at 9 ± 0.5, the reaction temperature at 190°C to 200°C, and the reaction duration at 8h to 10h, and synthesize by precipitation reaction. After solid-liquid separation, washing and drying, obtain the first precursor material;

[0052] Step b': Place the prepared mixed metal salt solution, complexing agent solution and precipitant in a reaction kettle, continuously stir, keep the pH value of the reaction liquid at 9 ± 0.5, the reaction temperature at 150°C to 160°C, and the reaction duration at 5h to 7h, and synthesize by precipitation reaction. After solid-liquid separation, washing and drying, obtain the second precursor material;

[0053] Step c: Mix the prepared first precursor material and second precursor material according to a mass ratio of 8 to 10:1 to obtain a mixed precursor material;

[0054] Step d: Weigh the lithium source according to the stoichiometric ratio required in LiFe x Ti y V z PO4 / C(x + y + Z = 1, and 0 < y ≤ 0.03, 0 < z ≤ 0.03). Mix the lithium source with the mixed precursor material evenly, put it into a vacuum atmosphere sintering furnace for calcination, and obtain the second positive electrode material after crushing treatment.

[0055] In step a, the iron source can be selected from ferrous oxalate, iron sulfate or ferric chloride, the phosphorus source can be selected from phosphoric acid or ammonium dihydrogen phosphate, the carbon source can be selected from glucose, sucrose or citric acid, the titanium source can be selected from titanium tetrachloride or titanium oxalate, and the vanadium source can be selected from vanadium pentoxide; the above raw materials can be prepared into corresponding solutions first, and then the solutions containing the above raw materials are mixed to obtain a mixed metal salt solution. Among them, the molar concentration of titanium or vanadium in the mixed metal salt solution is 3mol / L to 5mol / L; the strong base solution can be a sodium hydroxide solution with a molar concentration of 0.5mol / L to 1mol / L, and the molar concentration of ammonia water is 0.5mol / L to 1.5mol / L. The solvent in the mixed metal salt solution in this application can include water and / or phosphoric acid.

[0056] In step b or b', a complexing agent may be first added to the mixed metal salt solution to adjust the pH value to 9±0.5, and then a precipitant solution may be added. As the precipitate is formed, the complexing agent may be continuously added to adjust the pH value to maintain at 9±0.5. This process is a precipitation reaction process.

[0057] In step d, the lithium source can be selected from lithium carbonate or lithium hydroxide; the protective atmosphere is nitrogen, the sintering temperature is 500° C. to 600° C., and the sintering time is 5 h to 10 h.

[0058] The present application also provides a battery, comprising the positive electrode sheet described in any of the above embodiments.

[0059] In the present application, the positive electrode material layer can be arranged on one surface in the thickness direction of the positive electrode current collector, or on both surfaces in the thickness direction of the positive electrode current collector. In the present application, the positive electrode material layer is arranged on the surface of the positive electrode current collector, that is, the positive electrode material layer can be arranged in a partial area of ​​one surface of the positive electrode current collector, or on the entire area of ​​one surface of the positive electrode current collector. In the present application, there is no special restriction on the positive electrode current collector, as long as the purpose of the present application can be achieved, for example, it can include but is not limited to aluminum foil, aluminum alloy foil or composite current collector, etc. In the present application, there is no special restriction on the thickness of the positive electrode current collector, as long as the purpose of the present application can be achieved, for example, the thickness is 4μm to 12μm. The single-sided thickness of the positive electrode material layer of the present application can be 8μm to 15μm.

[0060] The lithium-ion battery of the present application also includes a negative electrode plate. The present application has no special restrictions on the negative electrode plate, as long as the purpose of the present application can be achieved. For example, the negative electrode plate generally includes a negative electrode current collector and a negative electrode material layer. The negative electrode material layer can be arranged on one surface or two surfaces along the thickness direction of the negative electrode current collector. In the present application, the negative electrode material layer is arranged on the surface of the negative electrode current collector, that is, the negative electrode material layer can be arranged on a partial area of ​​one surface of the negative electrode current collector, or it can be arranged on the entire area of ​​one surface of the negative electrode current collector. The present application has no special restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, it can include but is not limited to copper foil, copper alloy foil, nickel foil or composite current collector, etc. In the present application, there is no special restriction on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness is 4μm to 12μm. The single-sided thickness of the negative electrode material layer of the present application can be 70μm to 200μm.

[0061] In the present application, the negative electrode material layer includes a negative electrode material, wherein the negative electrode material is not particularly limited as long as the purpose of the present application can be achieved. For example, it can include at least one of artificial graphite, natural graphite, mesophase carbon microbeads, soft carbon, hard carbon, silicon, and silicon carbon.

[0062] In the present application, the negative electrode material layer may further include a negative electrode binder. There are no particular limitations on the negative electrode binder, as long as it can achieve the purpose of the present application. For example, it may include, but is not limited to, at least one of acrylate, polyamide, polyimide, polyamideimide, polyvinylidene fluoride, styrene-butadiene rubber, sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, polyacrylonitrile, sodium carboxymethyl cellulose, and potassium carboxymethyl cellulose.

[0063] The lithium-ion battery of the present application also includes a separator. The present application does not particularly limit the separator, and those skilled in the art can select according to actual needs, as long as the purpose of the present application can be achieved. For example, the separator may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, film or composite film with a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, polypropylene porous film, polyethylene porous film, polypropylene non-woven fabric, polyethylene non-woven fabric or polypropylene-polyethylene-polypropylene porous composite film can be selected.

[0064] The battery of the present application also includes an electrolyte. The present application does not particularly limit the electrolyte, and those skilled in the art can select it according to actual needs, as long as the purpose of the present application can be achieved. For example, at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl propionate (EP), propyl propionate (PP), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), vinylene carbonate (VC), or fluoroethylene carbonate (FEC) is mixed in a certain mass ratio or volume ratio to obtain a non-aqueous organic solvent, and then a lithium salt is added to dissolve and mix evenly. The present application does not limit the type of lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt can include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, lithium bis(oxalatoborate) (LiBOB), or lithium difluoroborate. The present application has no particular limitation on the concentration of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. For example, the concentration of the lithium salt is 1.0 mol / L to 2.0 mol / L.

[0065] The battery of the present application also includes a housing. The present application does not particularly limit the housing, and those skilled in the art can select it according to actual needs, as long as it can achieve the purpose of the present application. For example, the housing may include an aluminum-plastic film.

[0066] This application does not particularly limit the preparation method of the battery. Any preparation method known in the art may be used as long as the purpose of this application can be achieved. For example, the preparation method of the battery includes, but is not limited to, the following steps: stacking the positive electrode sheet, the separator, and the negative electrode sheet in sequence, and performing winding and folding operations as needed to obtain a bare battery cell with a wound structure, placing the bare battery cell in a packaging bag, injecting an electrolyte into the packaging bag, and sealing the packaging bag to obtain a battery.

[0067] The present application also provides an energy storage device comprising a housing and at least one battery according to any of the above embodiments, the battery being housed within the housing. The energy storage device comprising such a battery exhibits excellent performance, facilitating its use. Enclosing the battery within the housing enhances its securement and protection, thereby extending the lifespan of the energy storage device. It will be appreciated that the energy storage device may comprise one or more batteries. When the energy storage device comprises multiple batteries, the multiple batteries may be connected in at least one of parallel and series connection.

[0068] The present application also provides an electrical device, including the energy storage device in the above-mentioned embodiment, which is conducive to improving the product competitiveness and performance of the electrical device. In an optional embodiment, the electrical device includes an electrical device body, and the energy storage device is used to supply power to the electrical device body. In an optional embodiment, the electrical device body includes a positive electrode and a negative electrode, the positive electrode plate of the battery in the energy storage device is used to electrically connect to the positive electrode of the electrical device body, and the negative electrode plate of the battery in the energy storage device is used to electrically connect to the negative electrode of the electrical device body to supply power to the electrical device.

[0069] The electrical equipment of the present application may include but is not limited to: containers, household energy storage systems, battery vehicles, electric vehicles, ships, spacecraft, electric toys and electric tools, etc., among which spacecraft include airplanes, rockets, space shuttles and spacecraft, etc., electric toys include fixed or mobile electric toys, specifically electric car toys, electric ship toys and electric airplane toys, etc., and electric tools include metal cutting power tools, grinding power tools, assembly power tools and railway power tools, specifically electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers.

[0070] See Figure 1 , Figure 1 This is a schematic diagram of the structure of a household energy storage system according to an embodiment of the present application. Figure 1 The implementation plan is described using the household energy storage scenario in user-side energy storage as an example. The energy storage device of this application is not limited to the household energy storage scenario.

[0071] The present application provides a household energy storage system, which includes an energy conversion device 2 (photovoltaic panels), a first user load 3 (street lights), a second user load 4 (such as air conditioners and other household appliances), and an energy storage device 1. The energy storage device 1 is a small energy storage box that can be mounted on an outdoor wall. Specifically, the photovoltaic panels can convert solar energy into electrical energy during periods of low electricity prices. The energy storage device 1 is used to store this electrical energy and supply it to street lights and household appliances for use during peak electricity prices, or to provide power during power outages / power outages.

[0072] See Figure 2 , Figure 2 This is a schematic diagram of the structure of an energy storage system 400 according to an embodiment of the present application, and this application Figure 2 The implementation plan is described using the shared energy storage scenario on the generation / distribution side as an example. The energy storage device 1 of the present application is not limited to the energy storage scenario on the generation / distribution side.

[0073] The present application provides an energy storage system 400, which includes: a high-voltage cable 410, a first electric energy conversion device 420, a second electric energy conversion device 430 and the energy storage device 1 provided in the present application. In the power generation state, the first electric energy conversion device 420 and the second electric energy conversion device 430 are used to convert other forms of energy into electric energy, which is connected to the high-voltage cable 410 and supplied to the power distribution network for use. When the power load is low and the first electric energy conversion device 420 and the second electric energy conversion device 430 generate excess power, the excess power is stored in the energy storage device 1, reducing the wind and solar power abandonment rates and improving the problem of new energy power generation and consumption. When the power load is high, the power grid issues an instruction to transmit the power stored in the energy storage device 1 in conjunction with the high-voltage cable 410 in a grid-connected mode to the power consumption side, providing peak regulation, frequency regulation, standby and other services for the power grid operation, giving full play to the peak regulation role of the power grid, promoting peak shaving and valley filling of the power grid, and alleviating the power supply pressure of the power grid.

[0074] Optionally, the first electric energy conversion device 420 and the second electric energy conversion device 430 can convert at least one of solar energy, light energy, wind energy, thermal energy, tidal energy, biomass energy and mechanical energy into electric energy.

[0075] There can be multiple energy storage devices 1, connected in series or in parallel, and supported and electrically connected using isolation plates (not shown). In this embodiment, "multiple" refers to two or more. An energy storage box may also be provided outside the energy storage device 1 to accommodate the energy storage device 1.

[0076] Optionally, the energy storage device 1 may include, but is not limited to, a battery module, a battery pack, a battery system, etc. The battery module may be a battery module formed by connecting multiple batteries of the present application in series or parallel, the battery pack may include multiple batteries of the present application, and the battery system may be a charging and discharging system including the batteries or battery pack of the present application.

[0077] The energy storage device 1 provided in the embodiments of this application may be, but is not limited to, the products listed above. It may also be in other application forms. The embodiments of this application do not impose strict restrictions on the application form of the energy storage device 1. The embodiments of this application illustrate the energy storage device 1 as a multi-core battery. When the energy storage device 1 is a single battery, the energy storage device 1 may be at least one of a cylindrical battery, a prismatic battery, and the like.

[0078] Example

[0079] Hereinafter, the embodiments of the present application will be described in more detail with reference to preparation examples, examples, and comparative examples. Various tests and evaluations were performed according to the following methods.

[0080] Example 1

[0081] <Preparation of positive electrode sheet>

[0082] <Preparation of First Positive Electrode Material>

[0083] According to LiFe 0.99 Ti 0.01 The iron source ferrous oxalate, the phosphorus source lithium dihydrogen phosphate, the lithium source lithium carbonate, the carbon source glucose and the titanium source titanium tetrachloride were weighed in the required stoichiometric ratio in PO4 / C, uniformly mixed on a ball mill, and then pure water was added as a dispersant, and then high-energy ball milling was performed; the ball-to-material ratio of the high-energy ball milling was 4:1, the rotation speed was 1300r / min, and the ball milling time was 20h; the ball-milled material was spray-dried, the spray drying pump speed was 10mL / min, and the drying temperature was 200℃ to form a powder; the powder formed after spray drying was placed in a vacuum atmosphere sintering furnace for high-temperature calcination, the protective atmosphere was nitrogen, the sintering temperature was 700℃, and the sintering time was 8h, and then the first positive electrode material was obtained after crushing. The Dv50 of the first positive electrode material is shown in Table 1.

[0084] <Preparation of Second Positive Electrode Material>

[0085] <Solution Preparation>

[0086] According to LiFe 0.98 Ti 0.01 V 0.01The stoichiometric ratio required in PO4 / C is as follows: ferrous oxalate as an iron source, phosphoric acid as a phosphorus source, glucose as a carbon source, titanium tetrachloride as a titanium source, and vanadium pentoxide as a vanadium source are weighed and mixed to obtain a mixed metal salt solution; a strong base solution is then prepared as a precipitant solution, and ammonia water is prepared as a complexing agent solution; wherein the molar concentration of titanium or vanadium in the mixed metal salt solution is 4 mol / L, the strong base solution is a sodium hydroxide solution with a molar concentration of 0.5 mol / L, and the molar concentration of the ammonia water is 1 mol / L;

[0087] <Preparation of the First Precursor Material>

[0088] The mixed metal salt solution, complexing agent solution, and precipitant solution prepared above were placed in a reaction kettle, stirred continuously, the pH value of the reaction liquid was maintained at 9, the reaction temperature was 200° C., the reaction time was 10 h, and a precipitation reaction was used for synthesis. After solid-liquid separation, washing, and drying, a first precursor material was obtained;

[0089] <Preparation of Second Precursor Material>

[0090] The mixed metal salt solution, complexing agent solution and precipitant solution prepared above were placed in a reaction kettle, stirred continuously, the pH value of the reaction liquid was maintained at 9, the reaction temperature was 160° C., the reaction time was 7 h, and the second precursor material was obtained by precipitation reaction synthesis, solid-liquid separation, washing and drying.

[0091] The prepared first precursor material and the second precursor material were mixed in a mass ratio of 9:1 to obtain a mixed precursor material; 0.98 Ti 0.01 V 0.01 The lithium source lithium carbonate was weighed in the required stoichiometric ratio in PO4 / C, and the lithium source and the mixed precursor material were evenly mixed and placed in a vacuum atmosphere sintering furnace for calcination. The protective atmosphere was nitrogen, the sintering temperature was 550°C, and the sintering time was 10 h. After crushing, the second positive electrode material was obtained. The Dv50 of the spherical particles and the average length of the rod-shaped particles in the second positive electrode material are shown in Table 1.

[0092] <Preparation of positive electrode material layer>

[0093] The first positive electrode material, the second positive electrode material, the conductive agent conductive carbon black (Super-P), and the binder PVDF are mixed in a mass ratio of 93:2:2:3, and then N-methylpyrrolidone (NMP) is added as a solvent to prepare a positive electrode slurry with a solid content of 50wt%, and stirred evenly. Then, the positive electrode slurry is evenly coated on one surface of a positive electrode collector with a thickness of 10μm, dried at 85°C, and then the above steps are repeated on the other surface of the positive electrode sheet. After rolling, a positive electrode sheet coated with a positive electrode material layer on both sides is obtained, and the thickness of the positive electrode material layer on one side is 100μm.

[0094] <Preparation of negative electrode sheet>

[0095] The negative electrode materials, artificial graphite, conductive carbon black Super-P, and sodium carboxymethyl cellulose (CMC-Na), were mixed in a mass ratio of 95:2.5:2.5. Deionized water was added to prepare a negative electrode slurry with a solid content of 60wt%, and the mixture was stirred evenly. The negative electrode slurry was evenly coated on one surface of a 10μm-thick negative electrode current collector copper foil and dried at 85°C. The above steps were then repeated on the other surface of the negative electrode sheet. After roller pressing, a negative electrode sheet with a double-sided negative electrode material layer was obtained. The negative electrode material layer thickness on each side was 70μm.

[0096] <Preparation of Electrolyte>

[0097] Ethylene carbonate (EC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1, dissolved, and thoroughly stirred, then placed at a temperature of 5°C or less for 12 hours. LiPF6 is then added and mixed thoroughly to form an electrolyte solution. The molar concentration of LiPF6 in the electrolyte solution is 1 mol / L.

[0098] <Preparation of Separator>

[0099] A polyethylene (PE) porous polymer film with a thickness of 16 μm was used as the separator.

[0100] <Assembly of lithium-ion batteries>

[0101] The prepared positive electrode sheet and negative electrode sheet are placed in a press for pressing, and then a puncher is used to cut out a circular positive electrode sheet with a diameter of 15 mm and a circular negative electrode sheet with a diameter of 18 mm respectively; then the circular positive electrode sheet, the separator and the circular negative electrode sheet are stacked in order, so that the separator is placed between the circular positive electrode sheet and the circular negative electrode sheet to play an isolating role, and then the prepared electrolyte is injected to assemble a lithium-ion battery.

[0102] Example 2

[0103] Except for the preparation of the first positive electrode material, the LiFe 0.98Ti 0.02 Except for weighing the raw materials according to the stoichiometric ratio required for PO4 / C, the rest is the same as Example 1.

[0104] Example 3

[0105] Except for the preparation of the first positive electrode material, the LiFe 0.97 Ti 0.03 Except for weighing the raw materials according to the stoichiometric ratio required for PO4 / C, the rest is the same as Example 1.

[0106] Example 4

[0107] Except for the preparation of the second positive electrode material, the LiFe 0.97 Ti 0.01 V 0.02 Except for weighing the raw materials according to the stoichiometric ratio required for PO4 / C, the rest is the same as Example 1.

[0108] Example 5

[0109] Except for the preparation of the second positive electrode material, the LiFe 0.96 Ti 0.01 V 0.03 Except for weighing the raw materials according to the stoichiometric ratio required for PO4 / C, the rest is the same as Example 1.

[0110] Example 6

[0111] Except for the preparation of the second positive electrode material, the LiFe 0.97 Ti 0.02 V 0.01 Except for weighing the raw materials according to the stoichiometric ratio required for PO4 / C, the rest is the same as Example 1.

[0112] Example 7

[0113] Except for the preparation of the second positive electrode material, the LiFe 0.96 Ti 0.03 V 0.01 Except for weighing the raw materials according to the stoichiometric ratio required for PO4 / C, the rest is the same as Example 1.

[0114] Example 8 to Example 11

[0115] Except that the reaction temperature and reaction time in <Preparation of the Second Positive Electrode Material> were adjusted according to Table 1, the rest was the same as in Example 1.

[0116] Example 12 to Example 14

[0117] Except that the contents of the first positive electrode material and the second positive electrode material in the positive electrode material layer were adjusted according to Table 2 in <Preparation of Positive Electrode Material Layer>, the rest were the same as in Example 1.

[0118] Comparative Example 1

[0119] The process is the same as that of Example 1 except that in <Preparation of Positive Electrode Material Layer>, the positive electrode material layer contains only the first positive electrode material but not the second positive electrode material.

[0120] Comparative Example 2

[0121] Except for the preparation of the second positive electrode material, the LiFe 0.98 Ti 0.01 The raw materials are weighed in the required stoichiometric ratio of PO4 / C, that is, the second positive electrode material does not contain vanadium, and the rest is the same as in Example 1.

[0122] Table 1 Relevant preparation parameters of Examples 1 to 11 and Comparative Examples 1 to 2

[0123]

[0124]

[0125] In Table 1, “ / ” indicates that there are no relevant preparation parameters.

[0126] Table 2 Preparation parameters of the positive electrode material layer of Example 1, Examples 12 to 14, and Comparative Examples 1 to 2

[0127]

[0128] Test methods and equipment:

[0129] Material particle size distribution test:

[0130] Using a laser diffraction particle size distribution meter (Malvern Mastersizer 3000), according to the particle size distribution laser diffraction method (GB / T19077-2016), the particle size distribution of the spherical particles and the rod-shaped particles in the first positive electrode material and the second positive electrode material was measured, thereby measuring the Dv50 of the first positive electrode material, the Dv50 of the spherical particles, and the average length of the rod-shaped particles.

[0131] Test on the average length of rod-shaped particles in the second positive electrode material:

[0132] 100 rod-shaped particles were randomly selected from the SEM image of the positive electrode material layer, the length of each rod-shaped particle was measured, and the average length of the 100 rod-shaped particles was calculated after statistics, which was used as the average length of the rod-shaped particles in the second positive electrode material.

[0133] Positive electrode elongation test:

[0134] like Figure 3 As shown, the positive electrode sheet includes a positive electrode current collector 10 and a double-sided positive electrode material layer 20. For each of the examples and comparative examples, points A and B are marked on the surface of the positive electrode material layer 20 before rolling. L1 is the distance between points A and B before rolling. After rolling by roller 30, the positive electrode sheet stretches along its length, extending the distance between points A and B to the distance from A' to B', which is recorded as L2. The sheet stretch ratio is calculated as S = (L2 - L1) / L1 × 100%.

[0135] Compaction density test:

[0136] Using the powder compaction tester (model LD43.305) of Shanghai Lishi Company, the first positive electrode material and the second positive electrode material were mixed to obtain a sample according to the standard method GBT 24533-2019, and then the compaction density of the sample under a pressure of 3 kN was measured.

[0137] Rate performance test:

[0138] At 25°C, the lithium ion batteries prepared in the examples and comparative examples were charged at a rate of 0.5C to 3.75V, and then discharged at a rate of 0.5C to 2.5V, and the discharge capacity at this time was recorded as 0.5C; then charged at 1C to 3.75V, and then discharged at a rate of 1C to 2.5V, and the discharge capacity at this time was recorded as 1C, in mAh / g.

[0139] Table 3 Performance data of Examples 1 to 14 and Comparative Examples 1 to 2

[0140]

[0141]

[0142] As can be seen from Example 1 and Comparative Examples 1 and 2, since Comparative Example 1 does not contain a second positive electrode material, its positive electrode sheet has a greater elongation. The positive electrode sheet of Example 1 has a lower elongation, which may be due to the rod-shaped particles in the second positive electrode material hindering particle displacement and deformation during rolling, resulting in a lower elongation. Since the second positive electrode material of Comparative Example 2 does not contain the doping element vanadium, its elongation is the same as that of Example 1, but its capacity performance is reduced. Compared with Comparative Example 1, the 0.5C discharge capacity of Example 1 only decreased by 1.2%, and the 1C discharge capacity only decreased by 2.2%, with no significant impact on capacity performance. While the elongation is the same, the capacity performance of Example 1 and Comparative Example 2 is further improved. This shows that the combined effect of the first and second positive electrode materials can reduce the elongation of the positive electrode sheet while balancing the capacity performance of the lithium-ion battery.

[0143] The content of each raw material in the first positive electrode material, the Dv50 of the first positive electrode material, etc., generally also have an impact on the performance of the positive electrode sheet. As can be seen from Examples 1 to 3, based on the positive electrode sheet comprising the first positive electrode material and the second positive electrode material of the present application, by adjusting the above-mentioned preparation parameters within the scope of the present application, it is advantageous to obtain a lithium-ion battery with low elongation and high capacity performance.

[0144] The content of each raw material in the second positive electrode material, reaction temperature, reaction time, average length of rod-shaped particles, Dv50 of spherical particles, etc. generally also have an impact on the performance of the positive electrode sheet. From Examples 4 to 11, it can be seen that, based on the positive electrode sheet comprising the first positive electrode material and the second positive electrode material of this application, by adjusting the above preparation parameters within the scope of this application, it is beneficial to obtain a lithium-ion battery with low elongation and high capacity performance.

[0145] The content of the first and second positive electrode materials in the positive electrode material layer generally also affects the performance of the positive electrode sheet. As can be seen from Examples 1 and 12 to 14, based on the positive electrode sheet comprising the first and second positive electrode materials of the present application, by regulating the above-mentioned preparation parameters within the scope of the present application, a lithium-ion battery with low elongation and high capacity performance can be obtained.

[0146] Figure 4 This is the SEM image of the first cathode material obtained in Example 1. Figure 4 It can be seen that the particles of the first cathode material are larger, the particle size distribution is relatively uniform, and the surface morphology is smooth and tends to be spherical; Figure 5 This is the SEM image of the second cathode material obtained in Example 1. Figure 5 It can be seen that it contains spherical particles and rod-shaped particles, among which the spherical particles are smaller in size; Figure 6The cross-sectional SEM image of the positive electrode material layer of Example 1 is shown in FIG. Figure 6 It can be seen that there are rod-shaped particles in the positive electrode material layer.

[0147] The above is a detailed introduction to a positive electrode plate, battery, energy storage device and electrical equipment disclosed in the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the technical solutions and core invention points of the embodiments of the present application. At the same time, for those skilled in the art, according to the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A positive electrode sheet, characterized in that: A positive electrode current collector is included, wherein at least one side of the positive electrode current collector has a positive electrode material layer, and the positive electrode material layer includes a first positive electrode material and a second positive electrode material; The Dv50 of the first positive electrode material is 800nm-1000nm, the second positive electrode material includes spherical particles and rod-shaped particles, the Dv50 of the spherical particles is 300nm-500nm, the average length of the rod-shaped particles is 2μm-6μm, and the second positive electrode material includes vanadium.

2. The positive electrode sheet according to claim 1, characterized in that: Based on the mass of the positive electrode material layer, the mass percentage of the first positive electrode material is 90% to 93%, and the mass percentage of the second positive electrode material is 2% to 5%.

3. The positive electrode sheet according to claim 1, characterized in that: The first cathode material has a chemical formula of LiFe x Ti y PO4 / C, where x+y=1 and 0 <y≤0.03。 4. The positive electrode sheet according to claim 1, characterized in that: The second positive electrode material has a chemical formula of LiFe x Ti y V z PO4 / C, where x+y+Z=1 and 0 <y≤0.03,0<z≤0.03。 5. The positive electrode sheet according to claim 1, characterized in that: The elongation rate of the positive electrode sheet is 0.8% to 2.3%.

6. The positive electrode sheet according to claim 1, characterized in that: The button cell containing the positive electrode sheet has a 0.5C discharge capacity of 140 mAh / g to 150 mAh / g, and a 1C discharge capacity of 128 mAh / g to 137 mAh / g.

7. The positive electrode sheet according to claim 1, characterized in that: The compaction density of the mixture of the first positive electrode material and the second positive electrode material is 2.3 g / cm 3 ~2.5g / cm 3 .

8. The positive electrode sheet according to claim 1, characterized in that: The positive electrode plate further includes a conductive agent and a binder. Based on the mass of the positive electrode material layer, the mass percentage of the conductive agent is 1% to 3%, and the mass percentage of the binder is 1% to 3%.

9. A battery, characterized in that: The invention comprises the positive electrode sheet as described in any one of claims 1 to 7.

10. An energy storage device, characterized in that: The invention comprises a casing and at least one battery according to claim 9, wherein the battery is accommodated in the casing.

11. An electrical device, characterized in that: It includes the energy storage device as described in claim 10, and the energy storage device supplies power to the electrical equipment.

Citation Information

Patent Citations

  • Lithium-rich manganese-based lithium-ion battery cathode material and preparation method thereof

    CN105280909A

  • Titanium-doped regenerated lithium iron phosphate cathode material and preparation method thereof, and application thereof

    CN109167119A

  • Preparation method of graphene / silicon oxide composite material and application of graphene / silicon oxide composite material to electrode material

    CN110028060A

  • Positive pole piece and preparation method and application thereof

    CN113036085A

  • Positive pole piece and preparation method thereof, secondary battery, battery module, battery pack and power utilization device

    CN115832183A

Cited By

  • Positive pole piece, battery, energy storage device and electric equipment

    CN119905516A

  • Positive electrode sheet, battery, energy storage device, and electric device

    CN119905516B

  • Positive electrode, battery, energy-storage apparatus, and electricity-consumption device

    EP4773216A1

  • Positive electrode sheets, batteries, energy storage devices, and power consumption devices

    JP2026116869A

  • Positive electrode, battery, energy-storage apparatus, and electricity-consumption device