High-temperature-resistant flame-retardant PVDF-based semi-solid electrolyte and preparation method thereof

By using PVDF-based porous membrane as a semi-solid electrolyte in lithium-ion batteries, the safety hazards and short service life of lithium-ion batteries are solved, and efficient electrochemical performance and safety performance are improved, which is suitable for industrial production.

CN118983513APending Publication Date: 2024-11-19HUAZHONG UNIV OF SCI & TECH +1
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411299801.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have problems such as safety hazards, short service life, small energy density, and difficulty in mass production, especially the thermal runaway and poor mechanical properties of traditional liquid electrolytes.

Method used

Polyvinylidene fluoride (PVDF)-based porous membrane is used as the matrix of semi-solid electrolyte, and swelling polymers, inorganic nanofillers and flame retardant particles are added to form a three-dimensional interconnected micro-nano pore structure, and the electrolyte is adsorbed to form a semi-solid electrolyte. , improve thermal stability, electrochemical performance and safety performance.

Benefits of technology

It realizes the maintenance of electrolyte morphology and physical and chemical properties at high temperatures, inhibits the growth of lithium dendrites, improves ion conductivity and battery stability, extends service life, reduces preparation costs, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983513A_ABST
    Figure CN118983513A_ABST
Patent Text Reader

Abstract

The invention relates to a high-temperature-resistant flame-retardant PVDF-based semi-solid electrolyte and a preparation method thereof, and belongs to the technical field of lithium ion batteries. Comprising a polyvinylidene fluoride-based porous membrane and an electrolyte, the polyvinylidene fluoride based porous membrane is doped with a swelling polymer, and is blended with an inorganic nano filler and flame-retardant particles; the polyvinylidene fluoride based porous membrane is provided with a three-dimensional interconnected micro-nano pore channel structure, and the three-dimensional interconnected micro-nano pore channel structure is used for adsorbing electrolyte and swelling to form the semi-solid electrolyte. The main body of the porous membrane is PVDF doped with a swelling polymer, and the porous membrane has the advantages of good thermal stability, good electrochemical stability, good ionic conductivity, small interface impedance, high mechanical strength, high porosity and the like; the porous membrane has a micro-nano pore structure, and forms a semi-solid electrolyte after adsorbing an electrolyte, so that the growth of lithium dendrites is avoided, and the lithium ion conductivity, the ion transference number, the battery stability and the safety performance are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and more specifically, relates to a high temperature resistant and flame retardant PVDF-based semi-solid electrolyte and a preparation method thereof. Background Art

[0002] Lithium-ion batteries are safe and clean, have long working hours, short working cycles, good cycle performance, high energy density, small size, and are easy to carry. They play an increasingly important role in solving environmental pollution and energy shortage problems and are widely used in precision instruments, digital products, new energy vehicles, wearable products, etc. Traditional lithium-ion batteries have great safety hazards due to the use of liquid electrolytes. They are prone to thermal runaway due to battery overcharging, internal short circuits, mechanical failures, etc., causing fires and explosions. Based on this, the existing research work includes: adding a certain amount of flame retardant to the liquid electrolyte to reduce the risk of thermal runaway and fire of the battery (such as the flame retardant applied to lithium batteries disclosed in Chinese patent application 202410310532.9), but there are still problems such as high cost and complex process of flame retardant preparation; using solid electrolyte to completely replace liquid electrolyte, which is not flammable, has certain mechanical strength and good safety performance (such as the all-solid-state lithium metal battery proposed in Chinese patent application 202111564753.1), but the interface impedance is large, the energy density is low, and it is difficult to promote and apply; using solid electrolyte to partially replace liquid electrolyte, while ensuring safety and having the advantages of high conductivity and interface contact (such as the semi-solid lithium ion battery disclosed in Chinese patent application 202111051013.8), but the mechanical properties are poor and the preparation cost is high. In addition, the existing lithium battery technology also has problems such as poor cycle life, difficulty in industrialization, and short service time. Summary of the invention

[0003] In view of the problems of safety hazards, short service life, low energy density, and difficulty in mass production in existing lithium-ion battery technology, the purpose of the present invention is to provide a high-temperature resistant and flame-retardant PVDF-based semi-solid electrolyte and a preparation method thereof. A semi-solid electrolyte includes a polyvinylidene fluoride (PVDF)-based porous membrane and a battery electrolyte. The main component of the porous membrane is PVDF, and it is blended with a swelling polymer, an inorganic nanofiller, and flame-retardant particles. The porous membrane has a three-dimensional interconnected micro-nano pore structure, which can absorb a large amount of electrolyte and swell to form a semi-solid electrolyte. The main body of the porous membrane is PVDF doped with a swelling polymer, which has the advantages of good thermal stability, good electrochemical stability, good ionic conductivity, small interface impedance, high mechanical strength, and high porosity. The porous membrane has a micro-nano pore structure, and forms a semi-solid electrolyte after adsorbing the electrolyte, which avoids the growth of lithium dendrites and reduces safety issues such as electrode corrosion and oxidative combustion caused by electrolyte leakage, thereby improving lithium ion conductivity, ion migration number, battery stability, and safety performance. In addition, the micro-nano pore structure of the porous membrane increases the solid-liquid contact area, thereby improving the wetting performance of the porous membrane to the electrolyte, improving the liquid absorption rate and liquid retention performance of the porous membrane, and facilitating the infiltration of the electrolyte.

[0004] According to a first aspect of the present invention, a high-temperature resistant and flame-retardant PVDF-based semi-solid electrolyte is provided, comprising a polyvinylidene fluoride based porous membrane and an electrolyte; the polyvinylidene fluoride based porous membrane is doped with a swellable polymer and blended with inorganic nanofillers and flame-retardant particles; the polyvinylidene fluoride based porous membrane has a three-dimensional interconnected micro-nano pore structure, and the three-dimensional interconnected micro-nano pore structure is used to adsorb the electrolyte and swell to form a semi-solid electrolyte.

[0005] Preferably, in the polyvinylidene fluoride-based porous membrane, the mass fraction of polyvinylidene fluoride is 40%-70%, the mass fraction of the swelling polymer is 1%-40%, the mass fraction of the inorganic nanofiller is 1%-15%, and the mass fraction of the flame retardant particles is 1%-15%.

[0006] Preferably, the swellable polymer is one or more of polyethylene oxide, polyethylene glycol, polyethylene glycol dimethacrylate, polymethyl methacrylate, polyvinyl alcohol, polyacrylonitrile, polyacrylamide, thermoplastic polyurethane elastomer, and polyimide.

[0007] Preferably, the inorganic nanofiller is one or more of aluminum oxide, silicon dioxide, barium titanate, cerium oxide, titanium dioxide, magnesium oxide, zinc oxide, zirconium dioxide, manganese dioxide, yttrium oxide, magnesium borate, vanadium pentoxide, aluminum hydroxide, and molybdenum disulfide, and the particle size is 10 to 1000 nm;

[0008] The flame retardant particles are one or more of decabromodiphenyl ether, tetrabromobisphenol A, tetrabromobisphenol A bis(2,3-dibromopropyl) ether (octabromoether), 1,2-bis(2,4,6-tribromophenoxy) ethane, chlorendic anhydride, hexachlorocyclopentadiene, bis(hexachlorocyclopentadiene) cyclooctane, chlorinated paraffin, 1,2-bis(tetrabromophthalimide) ethane, tetrabromophthalic anhydride, 2,4,6-tribromophenyl allyl ether, melamine polyphosphate, metal organic framework, covalent organic framework, antimony trioxide, magnesium hydroxide, aluminum hydroxide, phosphonate, phosphate, phosphite, organic phosphorus salt, phosphine oxide and phosphorus-nitrogen compound, ammonium phosphate, ammonium polyphosphate, zinc borate, melamine, melamine cyanurate, expandable graphite, and dihydroxy metal oxide, and the particle size is 10 to 1000 nm.

[0009] Preferably, the thickness of the polyvinylidene fluoride-based porous membrane is 5 to 500 μm;

[0010] The pore size range of the three-dimensional interconnected micro-nano pore structure is 0.01-5 μm.

[0011] According to another aspect of the present invention, there is provided a method for preparing any one of high temperature resistant flame retardant PVDF-based semi-solid electrolytes, comprising the following steps:

[0012] (1) melt-blending polyvinylidene fluoride, a swelling polymer, a diluent, an inorganic nanofiller and flame retardant particles, and then extruding and casting the mixture, and then stretching and cooling the mixture to obtain a polyvinylidene fluoride based cast film;

[0013] (2) extracting the polyvinylidene fluoride cast film obtained in step (1) with an extractant to remove the diluent, and drying to obtain a polyvinylidene fluoride porous film having a three-dimensional interconnected micro-nano pore structure;

[0014] (3) The porous membrane with three-dimensional interconnected micro-nano pore structure obtained in step (2) is immersed in an electrolyte, and the electrolyte enters the pore structure of the porous membrane and swells with the swellable polymer to form a gel, and is filled in the polyvinylidene fluoride solid skeleton, thereby obtaining a semi-solid electrolyte.

[0015] Preferably, in the polyvinylidene fluoride-based cast film, the mass fraction of polyvinylidene fluoride is 10%-50%, the mass fraction of swellable polymer is 1%-20%, the mass fraction of diluent is 30%-70%, the mass fraction of inorganic nanofiller is 1%-10%, and the mass fraction of flame retardant particles is 1%-10%.

[0016] Preferably, the diluent is one or more of acetyl tributyl citrate, dibutyl phthalate, dioctyl phthalate, triacetin, dioctyl adipate, dioctyl sebacate, polyethylene glycol, polybutene, polyethylene oxide, NN-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, methyl pyrrolidone, and dimethylsulfonamide.

[0017] Preferably, the equipment used for the melt blending is a blade extruder, a single-shaft eccentric rotor extruder, a double-shaft eccentric rotor extruder, a planetary rotor extruder, a single-screw extruder, a double-screw extruder, a three-screw extruder or a planetary screw extruder, and the extrusion temperature is 100-300°C.

[0018] Preferably, the cooling method in step (1) is specifically: passing the melt formed by the casting die head through one or more of a cold water bath, an ethanol bath, a wind field or a cooling roller under external traction, so that the cast film is uniformly cooled to obtain a uniform and stable polyvinylidene fluoride-based cast film;

[0019] Preferably, the temperature of the cold water bath, ethanol bath, wind field or cooling roller is set to 0-30° C., the pulling external force is 5-100N, and the pulling speed is 10-100mm / min.

[0020] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:

[0021] (1) The polyvinylidene fluoride and inorganic nanoparticles used in the present invention are both high-temperature resistant materials with good thermal stability, so that the prepared semi-solid electrolyte still maintains its original morphology and physical and chemical properties at a temperature of 150°C; polyvinylidene fluoride has high mechanical strength and good safety performance, can effectively inhibit the growth of lithium dendrites, avoid the problem of porous membrane being punctured, and can also effectively resist external stress impact; flame retardant particles are also added when preparing the semi-solid electrolyte, which can effectively avoid the problem of the semi-solid electrolyte burning due to excessive temperature and causing safety hazards, thereby providing a new solution for preparing lithium batteries with long service life, good safety performance and low cost.

[0022] (2) The porous membrane of the semi-solid electrolyte of the present invention is mainly composed of polyvinylidene fluoride and a swellable polymer, which has the advantages of good electrochemical stability, good ionic conductivity, small interface impedance, and high porosity; the swellable polymer absorbs the electrolyte and swells to form a gel, which is filled in the three-dimensional interconnected micro-nano pore structure of the porous membrane, avoiding safety problems such as electrode corrosion and oxidative combustion caused by electrolyte leakage; in addition, the micro-nano pore structure of the porous membrane increases the solid-liquid contact area, so that the wettability of the porous membrane to the electrolyte is improved, the liquid absorption rate and liquid retention performance of the porous membrane are improved, and it is conducive to the infiltration of the electrolyte. The number of cycles of the semi-solid battery of the present invention can reach more than 300 times, the lithium ion migration number can reach 0.74, and the ionic conductivity can reach 1.62mS / cm.

[0023] (3) The semi-solid electrolyte of the present invention can be processed using common melt blending equipment, is easy to realize industrial production, has low manufacturing cost, high production efficiency, and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The figures are actual photos of the polypropylene (PP) diaphragm of Comparative Example 1 and the porous membrane of the high temperature resistant and flame retardant PVDF-based semi-solid electrolyte of Example 1 at different temperatures and the test results of thermal shrinkage.

[0025] Figure 2 This is a real photo of the porous membrane of the high temperature resistant and flame retardant PVDF-based semi-solid electrolyte of Example 1.

[0026] Figure 3 This is a scanning electron microscope photograph of the porous membrane of the high temperature resistant and flame retardant PVDF-based semi-solid electrolyte of Example 1.

[0027] Figure 4 This is a flow chart for the preparation of high temperature resistant and flame retardant PVDF-based semi-solid electrolyte.

[0028] Figure 5 Schematic diagram of the preparation of high temperature resistant and flame retardant PVDF-based semi-solid electrolyte.

[0029] Figure 6 This is a photograph of the contact angle of 4 to 5 μL of electrolyte on the surface of the porous membrane of the high temperature resistant flame retardant PVDF-based semi-solid electrolyte of Example 1.

[0030] Figure 7 This is a test graph of the ionic conductivity of the semi-solid electrolyte of Example 1.

[0031] Figure 8 This is a test chart of the lithium ion migration number of the semi-solid electrolyte of Example 1.

[0032] Fig. 9This is a battery cycle test diagram of the high temperature resistant and flame retardant PVDF-based semi-solid electrolyte of Example 1.

[0033] Fig.10 This is a scanning electron microscope photograph of the porous membrane of the high temperature resistant and flame retardant PVDF-based semi-solid electrolyte of Example 2. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0035] A semi-solid electrolyte of the present invention comprises a polyvinylidene fluoride (PVDF)-based porous membrane and an electrolyte (preferably a lithium battery electrolyte), wherein the main body of the porous membrane is PVDF doped with a swelling polymer and is blended with inorganic nanofillers and flame-retardant particles; the porous membrane has a three-dimensionally interconnected micro-nano pore structure; the three-dimensionally interconnected micro-nano pore structure is used to absorb a large amount of electrolyte and swell to form a semi-solid electrolyte.

[0036] In some embodiments, the polyvinylidene fluoride (PVDF)-based porous membrane is doped with a swelling polymer, such as one or more of polyethylene oxide (PEO), polyethylene glycol (PEG), polyethylene glycol dimethacrylate (PEGDMA), polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polyacrylonitrile (PAN), hexafluoropropylene (HFP), polyacrylamide (PAM), thermoplastic polyurethane elastomer (TPU), and polyimide (PI);

[0037] In some embodiments, the inorganic nanofiller is one or more of aluminum oxide, silicon dioxide, barium titanate, cerium oxide, titanium dioxide, magnesium oxide, zinc oxide, zirconium dioxide, manganese dioxide, yttrium oxide, magnesium borate, vanadium pentoxide, aluminum hydroxide, and molybdenum disulfide, and the particle size is 10 to 1000 nm;

[0038] In some embodiments, the flame retardant particles are decabromodiphenyl ether (DBD-PO), tetrabromobisphenol A (TBB-PA), tetrabromobisphenol A bis (2,3-dibromopropyl) ether (octabromoether), 1,2-bis (2,4,6-tribromophenoxy) ethane (BTPE), chlorendic anhydride (HET), hexachlorocyclopentadiene, bis (hexachlorocyclopentadiene) cyclooctane, chlorinated paraffin, 1,2-bis (tetrabromophthalimide) ethane (BTPAE), tetrabromophthalic anhydride (TBPA), 2,4,6-tribromobenzene One or more of tributyl acrylate (TBP-AE), melamine polyphosphate (MPP), metal organic frameworks (MOFs), covalent organic frameworks (COFs), antimony trioxide, magnesium hydroxide, aluminum hydroxide, phosphonates, phosphates, phosphites, organic phosphorus salts, phosphine oxides and phosphorus-nitrogen compounds, ammonium phosphates, ammonium polyphosphate (APP), zinc borate, melamine, melamine cyanurate (MCA), expandable graphite, and dihydroxy metal oxides (LDHs), with a particle size of 10 to 1000 nm.

[0039] In some embodiments, the porous membrane has a thickness of 5 to 500 μm;

[0040] The size of the three-dimensional interconnected micro-nano pore structure is 0.01-5 μm.

[0041] The method for preparing the semi-solid electrolyte comprises the following steps:

[0042] (1) melt-blending a PVDF matrix, a swellable polymer, a diluent, an inorganic nanofiller and flame-retardant particles, and then extruding and casting the mixture, stretching the mixture, and cooling the mixture to obtain a PVDF-based cast film;

[0043] (2) extracting the PVDF-based cast membrane obtained in step (1) with an extractant to remove the diluent, and drying to obtain a PVDF-based porous membrane having a three-dimensional interconnected micro-nano pore structure;

[0044] (3) The porous membrane obtained in step (2) is immersed in an electrolyte, and the electrolyte enters the pore structure of the porous membrane and swells with part of the swellable polymer to form a gel, which is filled in the polyvinylidene fluoride solid skeleton to obtain a semi-solid electrolyte.

[0045] In some embodiments, the diluent is one or more of acetyl tributyl citrate (ATBC), dibutyl phthalate (DBP), dioctyl phthalate (DOP), glyceryl triacetate (GTA), dioctyl adipate (DOA), dioctyl sebacate (DOS), polyethylene glycol (PEG), polybutene (PB), polyethylene oxide (PEO), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), tetrahydrofuran (THF), methyl pyrrolidone (NMP), and dimethylsulfonamide (DMSO);

[0046] The equipment used for melt blending is preferably a blade extruder, a single-shaft eccentric rotor extruder, a double-shaft eccentric rotor extruder, a planetary rotor extruder, a single-screw extruder, a double-screw extruder, a three-screw extruder and a planetary screw extruder, and the extrusion temperature is 100-300°C.

[0047] The rate of the cast film is 10-50 mm / min; the content of polyvinylidene fluoride (PVDF) in the polymer cast film is 10-50%, the content of other thermoplastic polymers is 1-20%, the content of diluent is 30-70%, the content of inorganic filler is 1-10%, and the content of flame retardant particles is 1-10%.

[0048] In some embodiments, the quenching method in step (1) is specifically: passing the melt formed by the casting die head through one or more of a cold water bath, an ethanol bath, a wind field or a cooling roller under external traction, so that the cast film is uniformly cooled to obtain a uniform and stable polyvinylidene fluoride-based cast film;

[0049] In some embodiments, the temperature of the cold water bath, ethanol bath, wind field or cooling roller is set to 0-30°, the pulling force is 5-100N, and the pulling speed is 10-50mm / min.

[0050] In some embodiments, the extractant in step (2) is one or more of anhydrous ethanol, glycerol, ethylene glycol, ethyl acetate, ether, cyclohexane, and methanol, and the extraction time is 12 to 72 hours;

[0051] The drying method can be natural drying, infrared drying, microwave drying, freeze drying, the drying time is 1 to 12 hours, and the drying temperature is 30 to 100°C.

[0052] In some embodiments, the porous membrane in step (3) is infiltrated for a time of 0.1 to 12 hours at a temperature of 0 to 50°C.

[0053] The semi-solid electrolyte of the present invention can be used in the fields of new energy vehicles, electronic devices, digital products, medical devices, wearable devices, aerospace, energy storage, etc.

[0054] The following are specific comparative examples and embodiments.

[0055] Comparative Example 1

[0056] A polypropylene (PP) lithium-ion battery separator is purchased from the market.

[0057] like Figure 1 The polypropylene membrane and the PVDF-based porous membrane prepared in Example 1 were placed in different temperature environments for testing (eg Figure 1 In a), when the temperature increases from 60°C to 150°C, the volume of the PP diaphragm continues to shrink, while the PVDF-based porous membrane basically maintains its original shape. When the temperature rises to 180°C, the PP diaphragm completely melts and the volume of the porous membrane shrinks by 10% (e.g. Figure 1 As shown in b), compared with the traditional PP diaphragm, the PVDF-based porous membrane has better thermal stability.

[0058] Example 1

[0059] A semi-solid electrolyte (such as Figure 2 ), the semi-solid electrolyte porous membrane has a three-dimensional interconnected micro-nano pore structure (such as Figure 3 ), the pore size range is 30 to 1000 nm, and the thermoplastic polymers are polyvinylidene fluoride (PVDF) and polyethylene oxide (PEO).

[0060] The preparation process of the semi-solid electrolyte is as follows Figure 4 The specific preparation method is as follows (such as Figure 5 ):

[0061] (1) PVDF (content of 30%), PEO1 (content of 15%), aluminum oxide 2 (particle size of 10-1000 nm, content of 2%), flame retardant particle melamine polyphosphate (MPP) 3 (particle size of 10-1000 nm, content of 3%), and diluent acetyl tributyl citrate (ATBC) 4 (content of 50%) are melt blended and extruded through a double-shaft eccentric rotor extruder 5, and a high-temperature molten cast film is formed through a casting die 6. Under external traction (traction force of 50 N, traction rate of 50 mm / min), the cast film passes through a cooling roller 7 (roller speed of 50 mm / min, circulating water temperature of 0-30° C.), so that the cast film is uniformly cooled to obtain a uniform and stable solid polymer cast film 8;

[0062] (2) extracting the polymer cast film obtained in step (1) with anhydrous ethanol 9 for 48 hours to remove ATBC, and drying it with an infrared drying device 10 for 5 hours (temperature is 70° C.) to obtain a porous film 11 having a three-dimensional interconnected micro-nano pore structure;

[0063] (3) The porous membrane 11 obtained in step (2) is immersed in a lithium battery electrolyte 12 for 5 hours (immersion temperature is 25° C.) to obtain a semi-solid electrolyte 13.

[0064] Among them, it should be noted that:

[0065] The density, height, diameter and three-dimensional interconnected micro-nano pore structure size of spherulites are determined as follows:

[0066] With the help of scanning electron microscope, the surface of the prepared semi-solid electrolyte porous membrane was observed, and the original photos were directly observed and obtained, and the density of spherulites was obtained by counting. With the help of mapping software, the height, diameter and micro-nano pore size of spherulites in different regions were measured, and the data were statistically analyzed and the average value was obtained, and finally the variation range of spherulite diameter, height and micro-nano pore structure diameter was obtained. Spread out a single layer of inorganic nanofiller and place it under the scanning electron microscope lens, directly observe and obtain the original photos, and measure the particle size.

[0067] like Figure 6 , which is a photograph of the wetting state of 4-5 μL electrolyte on the surface of the porous membrane of the present invention. It can be seen that the micro-nano pore structure on the surface of the product can improve the wettability of the porous membrane to the liquid, increase the solid-liquid contact area, thereby presenting a smaller contact angle, and improving the liquid absorption rate and liquid retention rate of the porous membrane.

[0068] like Figure 7 The prepared porous membrane has a high ionic conductivity, reaching a maximum of 1.62mS / cm.

[0069] like Figure 8 The lithium ion migration number of the porous membrane was detected using an electrochemical workstation. The prepared porous membrane had a high lithium ion migration number, reaching a maximum of 0.74, which is conducive to ion conduction.

[0070] like Fig. 9 , the porous membrane is immersed in the electrolyte. The porous membrane can be quickly infiltrated by the electrolyte. The rich porous structure can well absorb the electrolyte to form a semi-solid electrolyte, and the liquid absorption rate can reach up to 370%. After the cycle test, the lithium-ion battery assembled with the prepared semi-solid electrolyte has been cycled more than 300 times at a charge and discharge rate of 1C, and is still continuing to cycle. The average coulomb efficiency is greater than 96%, which has good cycle performance.

[0071] Example 2

[0072] The semi-solid electrolyte prepared in Example 2 and Example 1 ( Fig.10 ) are different in that:

[0073] The mass percentages of polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), diluent acetyl tributyl citrate (ATBC), flame retardant particle melamine polyphosphate (MPP), and aluminum oxide in step (1) are 30%, 20%, 45%, 2%, and 3%, and the remaining preparation steps are the same as those in Example 1.

[0074] Example 3

[0075] The difference between the semi-solid electrolyte prepared in Example 3 and Example 1 is that:

[0076] The diluent in step (1) is dibutyl phthalate (DBP), wherein the mass percentages of polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), diluent dibutyl phthalate (DBP), flame retardant particle melamine polyphosphate (MPP), and aluminum oxide are 30%, 20%, 45%, 2%, and 3%, and the remaining preparation steps are the same as those in Example 1.

[0077] Example 4

[0078] The difference between the semi-solid electrolyte prepared in Example 4 and Example 1 is that:

[0079] The inorganic nanoparticles in step (1) are silicon dioxide (particle size is 10 to 500 nm), and the remaining preparation steps are the same as those in Example 1.

[0080] Example 5

[0081] The difference between the semi-solid electrolyte prepared in Example 5 and Example 1 is that:

[0082] The swellable polymer in step (1) is polyethylene glycol (PEG), and the remaining preparation steps are the same as those in Example 1.

[0083] Example 6

[0084] The difference between the semi-solid electrolyte prepared in Example 6 and Example 1 is that:

[0085] The flame retardant in step (1) is melamine cyanurate (MCA) (particle size is 50-500 nm), and the remaining preparation steps are the same as those in Example 1.

[0086]

[0087] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high temperature resistant flame retardant PVDF-based semi-solid electrolyte, characterized in that: It comprises a polyvinylidene fluoride based porous membrane and an electrolyte; the polyvinylidene fluoride based porous membrane is doped with a swellable polymer and blended with inorganic nanofillers and flame retardant particles; the polyvinylidene fluoride based porous membrane has a three-dimensional interconnected micro-nano pore structure, and the three-dimensional interconnected micro-nano pore structure is used to adsorb the electrolyte and swell to form a semi-solid electrolyte.

2. The high temperature resistant flame retardant PVDF-based semi-solid electrolyte according to claim 1, characterized in that: In the polyvinylidene fluoride based porous membrane, the mass fraction of polyvinylidene fluoride is 40%-70%, the mass fraction of swelling polymer is 1%-40%, the mass fraction of inorganic nano filler is 1%-15%, and the mass fraction of flame retardant particles is 1%-15%.

3. The high temperature resistant flame retardant PVDF-based semi-solid electrolyte according to claim 1, characterized in that: The swellable polymer is one or more of polyethylene oxide, polyethylene glycol, polyethylene glycol dimethacrylate, polymethyl methacrylate, polyvinyl alcohol, polyacrylonitrile, polyacrylamide, thermoplastic polyurethane elastomer, and polyimide.

4. The high temperature resistant flame retardant PVDF-based semi-solid electrolyte according to claim 1, characterized in that: The inorganic nanofiller is one or more of aluminum oxide, silicon dioxide, barium titanate, cerium oxide, titanium dioxide, magnesium oxide, zinc oxide, zirconium dioxide, manganese dioxide, yttrium oxide, magnesium borate, vanadium pentoxide, aluminum hydroxide, and molybdenum disulfide, and the particle size is 10 to 1000 nm; The flame retardant particles are one or more of decabromodiphenyl ether, tetrabromobisphenol A, tetrabromobisphenol A bis(2,3-dibromopropyl) ether (octabromoether), 1,2-bis(2,4,6-tribromophenoxy) ethane, chlorendic anhydride, hexachlorocyclopentadiene, bis(hexachlorocyclopentadiene) cyclooctane, chlorinated paraffin, 1,2-bis(tetrabromophthalimide) ethane, tetrabromophthalic anhydride, 2,4,6-tribromophenyl allyl ether, melamine polyphosphate, metal organic framework, covalent organic framework, antimony trioxide, magnesium hydroxide, aluminum hydroxide, phosphonate, phosphate, phosphite, organic phosphorus salt, phosphine oxide and phosphorus-nitrogen compound, ammonium phosphate, ammonium polyphosphate, zinc borate, melamine, melamine cyanurate, expandable graphite, and dihydroxy metal oxide, and the particle size is 10 to 1000 nm.

5. The high temperature resistant flame retardant PVDF-based semi-solid electrolyte according to claim 1, characterized in that: The thickness of the polyvinylidene fluoride based porous membrane is 5 to 500 μm; The pore size range of the three-dimensional interconnected micro-nano pore structure is 0.01-5 μm.

6. The method for preparing a high temperature resistant flame retardant PVDF-based semi-solid electrolyte according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) melt-blending polyvinylidene fluoride, a swelling polymer, a diluent, an inorganic nanofiller and flame retardant particles, and then extruding and casting the mixture, and then stretching and cooling the mixture to obtain a polyvinylidene fluoride based cast film; (2) extracting the polyvinylidene fluoride cast film obtained in step (1) with an extractant to remove the diluent, and drying to obtain a polyvinylidene fluoride porous film having a three-dimensional interconnected micro-nano pore structure; (3) The porous membrane with three-dimensional interconnected micro-nano pore structure obtained in step (2) is immersed in an electrolyte, and the electrolyte enters the pore structure of the porous membrane and swells with the swellable polymer to form a gel, and is filled in the polyvinylidene fluoride solid skeleton, thereby obtaining a semi-solid electrolyte.

7. The preparation method according to claim 6, characterized in that: In the polyvinylidene fluoride based cast film, the mass fraction of polyvinylidene fluoride is 10%-50%, the mass fraction of swelling polymer is 1%-20%, the mass fraction of diluent is 30%-70%, the mass fraction of inorganic nanofiller is 1%-10%, and the mass fraction of flame retardant particles is 1%-10%.

8. The preparation method according to claim 6, characterized in that: The diluent is one or more of acetyl tributyl citrate, dibutyl phthalate, dioctyl phthalate, triacetin, dioctyl adipate, dioctyl sebacate, polyethylene glycol, polybutene, polyethylene oxide, NN-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, methyl pyrrolidone, and dimethylsulfonamide.

9. The preparation method according to claim 6, characterized in that: The equipment used for the melt blending is a blade extruder, a single-shaft eccentric rotor extruder, a double-shaft eccentric rotor extruder, a planetary rotor extruder, a single-screw extruder, a double-screw extruder, a three-screw extruder or a planetary screw extruder, and the extrusion temperature is 100-300°C.

10. The preparation method according to claim 6, characterized in that: The cooling method in step (1) is specifically: passing the melt formed by the casting die head through one or more of a cold water bath, an ethanol bath, a wind field or a cooling roller under external traction, so that the cast film is uniformly cooled to obtain a uniform and stable polyvinylidene fluoride based cast film; Preferably, the temperature of the cold water bath, ethanol bath, wind field or cooling roller is set to 0-30° C., the pulling external force is 5-100N, and the pulling speed is 10-100mm / min.

Citation Information

Cited By

  • Low-temperature polymer lithium battery and preparation method thereof

    CN119764546A

  • PVDF / APP nano-microsphere flame-retardant composite membrane as well as preparation method and application thereof

    CN119955134A

  • Semi-solid electrolyte precursor solution, semi-solid electrolyte, preparation method of semi-solid electrolyte precursor solution and semi-solid electrolyte, and lithium ion battery

    CN121237990A

  • Preparation method of phosphorus-containing PVDF battery diaphragm

    CN122338347A