Organic memristor based on thiophene viologen and preparation method thereof
By using the combination of thiophene violet essence functional layer and organic functional layer in organic memristors, the problem of restricted application of violet essence molecules in memristors is solved, the rectification function of organic memristors is realized, and its application is expanded scope.
Patent Information
- Application Number
- CN202411058509.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
Due to the low conjugation degree, wide band gap and unstable radical state, the purple sperm molecules are limited in their application in memristors. The existing organic memristors do not have the rectification function, resulting in limited application range.
The thiophene violet essence functional layer solution is dissolved from thiophene violet essence compound and polyvinylidene fluoride-co-hexafluoropropylene in N-methylpyrrolidone, and the thiophene violet essence functional layer is prepared by specific reaction and spin coating steps, and with The organic functional layer is combined to form a composite functional layer of thiophene violet essence, which is used to prepare an organic memristor.
It improves the stability of purple-spice radicals and electron transfer speed, gives organic memristor rectification function, expands its application range, and solves the problem that existing organic memristors do not have rectification function.
Smart Images

Figure CN118984594A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic memristor protection, and in particular relates to an organic memristor based on thiophene viologen and a preparation method thereof. Background Art
[0002] Memristors are considered to be the most promising new electronic components to solve computing power problems, break through the limitations of "Moore's Law", and realize storage-computing integrated architecture. The working principle of organic memristors is based on the migration and redistribution of charge carriers in organic materials. By applying voltage or current, the charge distribution inside the organic material can be changed, thereby changing the resistance value.
[0003] Viologen (i.e. 4,4′-bipyridine) and its derivatives are a class of organic small molecules with versatility and application potential. Due to their excellent electronic conductivity and stable redox properties, their research and application in electrochemistry, materials science and biomedicine are constantly expanding, making them one of the ideal choices for these applications. Viologen compounds have two resistance states in the process of gaining and losing electrons, namely the high resistance state of the divalent cation state and the low resistance state of the reduced state or cation radical state. Ordinary viologen molecules are greatly limited in the application of memristors due to their low degree of conjugation and wide band gap.
[0004] The existing functional layer preparation method uses spin coating of organic solutions. The advantage of organic materials is that the molecular structure is highly adjustable and can be regulated according to the use requirements, and can even increase the functionality that inorganic materials do not have. At the same time, the organic functional layer can be used in flexible devices and can work even when bent or stretched. Organic materials have low power consumption and do not have heating problems; however, the organic molecule synthesis process is complex and the yield is low; the stability and cycle performance are poor; the effect is not good in the application of memristors, etc., and the obtained memristors do not have rectification functions.
[0005] Therefore, the application of viologen molecules in memristors is limited due to their low degree of conjugation and wide band gap. In addition, existing organic memristors cannot further expand their application scope because they do not have rectification function. Summary of the invention
[0006] In view of the technical status that the application of viologen molecules in memristors is limited by their low degree of conjugation, wide band gap, unstable free radical state and reduced state, and the existing organic memristors do not have a rectification function, which limits their application scope, the first object of the present invention is to provide an organic memristor based on thiophene viologen, and the second object of the present invention is to provide a method for preparing an organic memristor based on thiophene viologen.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The present invention provides a thiophene viologen functional layer solution, wherein the solute of the solution is a thiophene viologen compound and polyvinylidene fluoride-co-hexafluoropropylene, and the solvent is N-methylpyrrolidone. The structural formula of the thiophene viologen compound is as follows:
[0009]
[0010] The mass ratio of the thiophene viologen compound to polyvinylidene fluoride-co-hexafluoropropylene is 1 to 2:1.
[0011] The preparation method of the thiophene viologen functional layer solution is specifically obtained by the following steps:
[0012] (1) under argon protection, adding 4-pyridylboronic acid pinacol ester, 2,5-dibromothiophene, (triphenylphosphine) palladium, and sodium carbonate to a mixed solvent for reaction, cooling to room temperature after the reaction, and removing the solvent under reduced pressure to obtain a concentrated solution;
[0013] (2) extracting the concentrated solution from step (1) with chloroform, adding concentrated hydrochloric acid to the organic phase for precipitation, dissolving the precipitate in water, adjusting the pH value to 8-9, and precipitating compound 1;
[0014]
[0015] (3) dissolving the compound 1 obtained in step (2) in dichloromethane, adding methyl trifluoromethanesulfonate to precipitate, eluting and drying the precipitate to obtain the thiophene viologen compound 2;
[0016]
[0017] (4) Dissolving the compound 2 obtained in step (2) and polyvinylidene fluoride-co-hexafluoropropylene in N-methylpyrrolidone to obtain a thiophene viologen functional layer solution.
[0018] The present invention provides a thiophene viologen functional layer solution, wherein in the step (1), the molar ratio of 4-pyridylboronic acid pinacol ester, (triphenylphosphine) palladium and sodium carbonate is 110-130:1:290-310, the mixed solvent is toluene, 2,5-dibromothiophene and water in a volume ratio of 45-55:1-2:10-20, the reaction temperature is 80-100°C, and the reaction time is 42-56h.
[0019] The present invention provides a thiophene violet composite functional layer, the composite functional layer comprises a thiophene violet functional layer and an organic functional layer, the thiophene violet functional layer is located on the organic functional layer, the thiophene violet functional layer is obtained by spin coating and annealing the thiophene violet functional layer solution, and the organic functional layer is obtained by spin coating and annealing the poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) organic functional layer solution.
[0020] Application of the above-mentioned thiophene viologen functional layer solution in the preparation of organic memristor.
[0021] Application of the above-mentioned thiophene viologen composite functional layer in the preparation of organic memristor.
[0022] Furthermore, the present invention provides an organic memristor based on a thiophene viologen composite functional layer, comprising a substrate, a lower electrode, the above-mentioned thiophene viologen composite functional layer, and an upper electrode, wherein the lower electrode is deposited on the substrate, the thiophene viologen composite functional layer is formed on the lower electrode, and the upper electrode is deposited on the thiophene viologen composite functional layer.
[0023] The invention discloses an organic memristor based on thiophene viologen, wherein the lower electrode is ITO.
[0024] The present invention discloses an organic memristor based on thiophene viologen, wherein the upper electrode is Ag.
[0025] At the same time, the present invention provides a method for preparing an organic memristor based on a thiophene viologen composite functional layer, comprising the following steps:
[0026] S1: preparing thiophene viologen functional layer solution;
[0027] S2: After ultrasonic treatment of the substrate, it was air-dried with a nitrogen air gun;
[0028] S3: depositing a lower electrode on the substrate in step S2 by thermal evaporation;
[0029] S4: spin coating the poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) solution on the lower electrode in step S3, and annealing to form an organic functional layer;
[0030] S5: Continue to spin-coat the thiophene violet functional layer solution on the organic functional layer of step S4, and anneal to form a thiophene violet functional layer;
[0031] S6: thermally evaporate an upper electrode on the thiophene viologen functional layer of step S5 to obtain an organic memristor based on the thiophene viologen composite functional layer.
[0032] In the preparation method of the organic memristor based on the thiophene viologen composite functional layer of the present invention, in step S3 and step S6, the deposition thickness of the upper electrode and the lower electrode are both 90-110 nm.
[0033] In the preparation method of the organic memristor based on the thiophene viologen composite functional layer of the present invention, the poly 3,4-ethylenedioxythiophene-polystyrene sulfonic acid solution in step S4 is prepared by Clevios TM PH 1000 with 0.02% FS-30 fluorosurfactant was obtained by mixing and stirring for 1 hour.
[0034] In the preparation method of the organic memristor based on the thiophene viologen composite functional layer of the present invention, in the step S4 and the step S5, the spin coating speed is 1500-2500 rpm, the spin coating time is 40-50s, the annealing temperature is 110-130°C, and the annealing time is 20-40min.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The thiophene viologen functional layer solution provided by the present invention improves the stability of the viologen free radical and the electron transfer speed and stabilizes the molecular structure by introducing a thiophene heterocycle. The thiophene viologen functional layer solution obtained from the modified thiophene viologen compound is used to prepare an organic memristor functional layer. The obtained memristor has a rectifying function, which solves the technical problems that the application of viologen in memristors is limited due to its low degree of conjugation, wide band gap, unstable free radical state and reduced state.
[0037] (2) The thiophene violet composite functional layer provided by the present invention comprises an organic functional layer and a thiophene violet functional layer. The physical bonding effect between the organic functional layer and the thiophene violet functional layer is good, and a uniform thin film structure is formed. The annealing forms a flat interface between the layers, and the double-layer structure retains the overall light transmittance of the device. The organic functional layer is an excellent hole transfer material. The thiophene violet composite functional layer is used to prepare an organic memristor, which has a rectification function and expands its application range. This solves the problem that the organic memristor obtained by the existing preparation method does not have a rectification function and has a limited application range. At the same time, it is of great significance for the application of violet in memristors. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Shown is a schematic structural diagram of the thiophene viologen organic memristor of the present invention.
[0039] Figure 2 Shown is a schematic diagram of the specific structure of the thiophene viologen organic memristor of the present invention.
[0040] Figure 3 Shown are current-voltage relationship curves of organic memristors with different functional layers, wherein A is the thiophene viologen organic memristor of the present invention, and B is the organic memristor with an unmodified viologen molecule functional layer.
[0041] Figure 4 It shows the rectification performance curves of organic memristors with different functional layers, wherein A is the thiophene viologen organic memristor of the present invention, and B is the organic memristor with unmodified viologen molecule functional layer.
[0042] Figure 5 Shown is a cross-sectional SEM image of the thiophene viologen organic memristor of the present invention.
[0043] Figure 6 Shown is a real picture of the thiophene viologen organic memristor of the present invention. DETAILED DESCRIPTION
[0044] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0045] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0046] The present invention provides an organic memristor based on thiophene viologen, which has a vertical structure, and comprises a substrate, a lower electrode, a thiophene viologen composite functional layer, and an upper electrode in order from bottom to top. The thiophene viologen composite functional layer comprises a thiophene viologen functional layer and an organic functional layer. The thiophene viologen functional layer is located on the organic functional layer. The thiophene viologen functional layer is obtained by spin coating and annealing a thiophene viologen functional layer solution. The organic functional layer is obtained by spin coating and annealing a poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid organic functional layer solution. For a specific structure, see the attached Figure 1-2 shown.
[0047] Wherein, the lower electrode is ITO; the upper electrode is Ag.
[0048] Example 1: Preparation of organic memristor based on thiophene viologen composite functional layer
[0049] 1. Preparation of Thiophene Viologen Compounds
[0050] 4-Pyridylboronic acid pinacol ester (6.36 g, 31 mmol), tetrakis(triphenylphosphine)palladium(0) (286 mg, 0.248 mmol) and sodium carbonate (7.95 g, 75 mmol) were added to a 250 mL pressure tube; toluene (50 mL), 2,5-dibromothiophene (1.40 mL, d=2.15 g / mL, 3 g, 12.4 mmol) and 15 mL of water were added under argon atmosphere, and the suspension was stirred at 90 ° C for 48 hours; after cooling to room temperature, toluene was removed under reduced pressure; extraction was performed three times with chloroform. ; then, concentrated hydrochloric acid (about 2 mL) was added to the organic phase to precipitate the product from the solution; the precipitate was collected by filtration and then dissolved in water; subsequently, an aqueous solution of NaOH (15 M) was added dropwise to the aqueous phase until the pH value was about 8-9, and a yellow solid compound 1 (1.83 g, 7.68 mmol, 61.9%) was precipitated; finally, compound 1 was dissolved in dichloromethane, and methyl trifluoromethanesulfonate (4.923 g, 30 mmol) was added, the precipitate was taken, eluted and dried to obtain the thiophene viologen compound 2, and the reaction formula is as follows:
[0051]
[0052] 2. Preparation of Thiophene Viologen Functional Layer Solution
[0053] The thiophene viologen compound obtained in Experiment 1 and poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-co-HFP) were mixed in a mass ratio of 1:1 and dissolved using N-methylpyrrolidone (NMP) solution. The concentration of the thiophene viologen compound in the thiophene viologen functional layer solution was 20 mg / mL.
[0054] 3. Preparation of organic memristor based on thiophene viologen composite functional layer
[0055] (1) Cut the glass substrate into 3 cm × 3 cm square pieces and soak them in deionized water, anhydrous ethanol, acetone, anhydrous ethanol, and deionized water and perform ultrasonic treatment for 15 min each. Then air-dry the cleaned glass pieces with a N2 air gun.
[0056] (2) A 100 nm thick ITO was deposited on a glass substrate using thermal evaporation as the lower electrode.
[0057] (3) Spin coating a poly (3,4-ethylenedioxythiophene)-poly (styrene sulfonic acid) (PEDOT:PSS) solution on the lower electrode at a speed of 2000 rpm for 45 seconds and annealing at 120° C. for 30 minutes to form an organic functional layer. The poly (3,4-ethylenedioxythiophene)-poly (styrene sulfonic acid) solution was prepared by Clevios TM PH 1000 with 0.02% FS-30 fluorosurfactant was obtained by mixing and stirring for 1 hour.
[0058] (4) The thiophene violet functional layer solution obtained in Experiment 2 was continuously used on the organic functional layer film in step (3) to spin coat at a speed of 2000 rpm for 45 s, and then annealed at 120° C. for 30 min to obtain a thiophene violet functional layer.
[0059] (5) Using a thermal evaporation method, a 100 nm thick Ag layer is deposited on the thiophene viologen functional layer in step (4) as an upper electrode to obtain an organic memristor.
[0060] Example 2: Preparation of organic memristor based on thiophene viologen composite functional layer
[0061] In this embodiment, on the basis of Embodiment 1, the thiophene viologen functional solution is a thiophene viologen compound and poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-co-HFP) in a mass ratio of 2:1, the concentration of the thiophene viologen functional layer solution is 40 mg / mL, the rotation speed is 2000 rpm / min, the spin coating is performed for 45 s, and the annealing is performed at 120°C for 30 min. The other processes are the same to obtain an organic memristor based on thiophene viologen.
[0062] Example 3: Performance test of organic memristor based on thiophene viologen
[0063] In this embodiment, on the basis of embodiments 1-2, the performance of the thiophene viologen organic memristor based on embodiment 1 of the present invention is tested, and a comparative example is set at the same time. The functional layer of the comparative example uses an unmodified ordinary viologen molecule to replace the thiophene viologen compound of the functional layer of the organic memristor of the present invention. The other process parameters and the manufacturing process are the same. A dual probe station and a Keysight B2900A source meter are used to perform voltage-current tests in air, and the tests are performed at a constant scan rate of 20 mV / s, and the following are obtained: Figure 3 The IV curve shown and the attached Figure 4 The rectification performance curve is shown in the figure. The functional layer structure was tested by scanning electron microscope. The results are shown in the attached Figure 5 .
[0064] By the attached Figure 3 A data shows that, when testing the electrical performance of the organic memristor of the present invention, at the same voltage, the conductivity of the device shows the difference between high and low resistance states. In the process of loading the cyclic voltage, different current responses will be generated to the corresponding voltage value. Figure 3 From the data of B, it can be seen that in the comparative example, the organic memristor prepared by using unmodified viologen molecules in the functional layer has current output under positive and negative voltages, and has a certain memristive effect. However, as the number of cycles increases, the resistance value of the low resistance state gradually increases, the ratio of the high resistance state to the low resistance state gradually decreases, and the stability of the device gradually decreases. The main reason is that the reduced state of the unmodified viologen molecules is unstable and can be easily oxidized to the initial state.
[0065] By the attached Figure 4 From the data of A, it can be seen that the organic memristor of the present invention has no response to the positive voltage range, but has a current response to the negative voltage; Figure 4 From the data B, it can be seen that the current response of a single voltage interval in the comparative example shows that the current responds in both the positive and negative voltage intervals, that is, there is no rectification effect; this indicates that it does not have a rectification effect. It can be seen that the organic memristor based on thiophene viologen obtained by the present invention solves the problem of the organic memristor obtained by the existing preparation method, especially the problem that the existing organic functional layer does not have a rectification function and has a limited application range. At the same time, it is of great significance for the application of viologen in memristors.
[0066] By the attached Figure 5 It can be seen that the functional layer provided by the present invention includes an organic functional layer and a thiophene violet functional layer. The physical bonding effect of the organic functional layer and the thiophene violet functional layer is good, forming a uniform thin film structure. After annealing, a flat interface between the layers is formed without cracks. In addition, the double-layer structure retains the overall light transmittance of the device. The results are shown in the attached Figure 6 A physical picture of the memristor of the present invention.
[0067] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A thiophene viologen functional layer solution, characterized in that: The solute of the solution is a thiophene viologen compound and polyvinylidene fluoride-co-hexafluoropropylene, and the solvent is N-methylpyrrolidone. The structural formula of the thiophene viologen compound is as follows: The mass ratio of the thiophene viologen compound to polyvinylidene fluoride-co-hexafluoropropylene is 1 to 2:
1.
2. A method for preparing a thiophene viologen functional layer solution, characterized in that: The specific steps include: (1) under argon protection, adding 4-pyridylboronic acid pinacol ester, (triphenylphosphine) palladium and sodium carbonate to a mixed solvent for reaction, cooling to room temperature after the reaction, and removing the solvent under reduced pressure to obtain a concentrated solution; (2) The concentrated solution of step (1) was extracted with chloroform, concentrated hydrochloric acid was added to the organic phase for precipitation, and the precipitate was dissolved in water, and the pH value was adjusted to 8-9 to precipitate compound 1. The structural formula of compound 1 is as follows: (3) dissolving the compound 1 obtained in step (2) in dichloromethane, adding methyl trifluoromethanesulfonate to precipitate, eluting and drying the precipitate to obtain a thiophene viologen compound; (4) dissolving the thiophene viologen compound and polyvinylidene fluoride-co-hexafluoropropylene obtained in step (3) in N-methylpyrrolidone to obtain a thiophene viologen functional layer solution.
3. The method for preparing the thiophene viologen functional layer solution according to claim 2, characterized in that: In the step (1), the molar ratio of 4-pyridylboronic acid pinacol ester, (triphenylphosphine) palladium and sodium carbonate is 110-130:1:290-310, the mixed solvent is toluene, 2,5-dibromothiophene and water in a volume ratio of 45-55:1-2:10-20, the reaction temperature is 80-100°C, and the reaction time is 42-56h.
4. A thiophene viologen composite functional layer, characterized in that: The composite functional layer comprises a thiophene violet functional layer and an organic functional layer, wherein the thiophene violet functional layer is located on the organic functional layer, the thiophene violet functional layer is obtained by spin coating and annealing the thiophene violet functional layer solution according to claim 1, and the organic functional layer is obtained by spin coating and annealing a poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid solution.
5. Use of the thiophene viologen functional layer solution as claimed in claim 1 in the preparation of an organic memristor.
6. Use of the thiophene viologen composite functional layer as claimed in claim 4 in the preparation of an organic memristor.
7. An organic memristor based on a thiophene viologen composite functional layer, characterized in that: The organic memristor has a vertical structure, which includes, from bottom to top, a substrate, a lower electrode, the thiophene viologen composite functional layer according to claim 4, and an upper electrode. The lower electrode is deposited on the substrate, the thiophene viologen composite functional layer is formed on the lower electrode, and the upper electrode is deposited on the thiophene viologen composite functional layer.
8. A method for preparing an organic memristor based on a thiophene viologen composite functional layer according to claim 7, characterized in that: The steps include: S1: preparing thiophene viologen functional layer solution; S2: After ultrasonic treatment of the substrate, it was air-dried with a nitrogen air gun; S3: depositing a lower electrode on the substrate in step S2 by thermal evaporation; S4: spin coating the poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) solution on the lower electrode in step S3, and annealing to form an organic functional layer; S5: Continue to spin-coat the thiophene violet functional layer solution on the organic functional layer of step S4, and anneal to form a thiophene violet functional layer; S6: thermally evaporate an upper electrode on the thiophene viologen functional layer of step S5 to obtain an organic memristor based on the thiophene viologen composite functional layer.
9. The method for preparing an organic memristor based on a thiophene viologen composite functional layer according to claim 7, characterized in that: In the step S3 and the step S6, the deposition thickness of the upper electrode and the lower electrode is 90-110 nm.
10. The method for preparing an organic memristor based on a thiophene viologen composite functional layer according to claim 7, characterized in that: In the step S4 and step S5, the spin coating speed is 1500-2500 rpm, the spin coating time is 40-50 s, the annealing temperature is 110-130° C., and the annealing time is 20-40 min.
Citation Information
Cited By
Monomolecular memristor based on viologen derivative and preparation method thereof
CN121152556A
Monomolecular memristor based on viologen derivative and preparation method thereof
CN121152556B