Graphene-titanium dioxide nano composite material and preparation method thereof
Through the composite material of graphene and nanotitanium dioxide, the problem of poor formaldehyde purification in the existing technology is solved, and low-cost and efficient formaldehyde purification is achieved. It is suitable for interior decoration and decoration, with good photodegradation efficiency and long-term effect. .
Patent Information
- Application Number
- CN202411092560.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art has problems in the purification of formaldehyde, the physical adsorption effect is limited, the photodegradable materials have high requirements for light sources, and the cost is expensive, and the biological removal ability is weak, which limits its application in indoor formaldehyde purification.
Using a composite material of graphene and nanotitanium dioxide, titanium dioxide is uniformly mounted on graphene through specific chemical methods to form a heterojunction interface, enhance light absorption intensity, and change the inertia of the graphene surface through polytetrahydrofuran diamine to improve nanometers The formaldehyde removal properties of composite materials.
It realizes high-efficiency formaldehyde purification with low cost and no equipment investment. The material has good photodegradation efficiency and long-term effectiveness. It is suitable for interior decoration and decoration applications and has a high cost-effectiveness.
Abstract
Description
Technical Field
[0001] The invention relates to a composite material, in particular to a graphene-titanium dioxide nanocomposite material and a preparation method thereof. Background Art
[0002] Formaldehyde is a colorless gas with a pungent odor that can be released from new furniture, decoration materials, coatings, textiles, etc. Long-term exposure to formaldehyde can cause a variety of human health problems, including eye irritation, upper respiratory tract irritation, skin allergic reactions, and even cancer. Therefore, the control of indoor formaldehyde has become an important research direction. In addition to ventilation, the main methods for purifying formaldehyde include physical adsorption, photodegradation, and biological removal. However, physical adsorption has limited effect on the removal of formaldehyde that has been released into the air, and the adsorbent needs to be replaced regularly after saturation, otherwise secondary pollution may occur; the commonly used photodegradable materials have certain requirements for light sources and are relatively expensive; the biological removal method has relatively weak formaldehyde removal ability and cannot achieve ideal purification effects for severe formaldehyde pollution.
[0003] Nano-titanium dioxide is a widely used nano-material with excellent photocatalytic properties. It can catalytically decompose benzene, formaldehyde, acetone, ammonia, sulfur dioxide and other substances emitted from building materials, decorative materials and daily chemicals under ultraviolet light without producing intermediate products. Nano-titanium dioxide itself is non-toxic and harmless, stable in nature and relatively inexpensive. However, people have found in applications that nano-titanium dioxide can only work under sufficient sunlight or specially set ultraviolet light, which limits its use.
[0004] Graphene is a two-dimensional material composed of a single layer of carbon atoms arranged in a honeycomb shape. Since its discovery in 2004, it has attracted much attention for its excellent physical and chemical properties. Graphene has a large surface area, good electrical conductivity, strong chemical stability, and high mechanical strength and thermal conductivity. These properties make it have broad application prospects in many fields, especially in catalyst loading, which can greatly improve the catalytic efficiency of the catalyst. Combining the unique properties of graphene and titanium dioxide can improve the adsorption and photodegradation of formaldehyde.
[0005] Although the product of graphene combined with nano-titanium dioxide has excellent performance, the current production process hinders its practical application. Moreover, this new material is still a photodegradable material and needs to be installed on the surface of indoor walls of buildings. Therefore, the graphene-nano-titanium dioxide material is mixed with latex paint to develop a low-cost graphene / titanium dioxide nanocomposite material for indoor decoration and renovation projects, which is expected to solve the formaldehyde hazard problem in decoration and renovation projects. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing a graphene-titanium dioxide nanocomposite material, which can achieve uniform compounding of graphene and titanium dioxide, and the prepared graphene-titanium dioxide nanocomposite material has good formaldehyde removal performance.
[0007] In order to solve the above technical problems, the technical solution of the present invention is:
[0008] A method for preparing a graphene-titanium dioxide nanocomposite material comprises the following steps:
[0009] S1. Add granular natural graphite and sodium nitrate to a three-necked flask, cool to 0°C with a cold bath, add concentrated sulfuric acid to the three-necked flask, stir and react for 10-30 minutes, and keep the temperature of the reaction system not higher than 5°C; add the first batch of potassium permanganate to the three-necked flask, stir and react for 10-30 minutes, and keep the temperature of the reaction system not higher than 10°C; add the second batch of potassium permanganate to the three-necked flask in 3 equal portions within 1 hour, and keep the temperature of the reaction system not higher than 20°C; remove the cold bath, use a water bath to heat the reaction system to 35-45°C, stir and react for 2 hours to obtain a suspension; add distilled water dropwise to the suspension, raise the system temperature to 50°C, add polytetrahydrofuran diamine, and then keep warm for 2-4 hours to obtain a reaction solution; add an aqueous hydrogen peroxide solution to the reaction solution, stir at 50°C for 30 minutes, then add a hydrochloric acid solution, stir at 50°C for 30 minutes, and cool to room temperature to obtain a graphene oxide solution;
[0010] S2. Filter the graphene oxide solution obtained in step S1 under reduced pressure to obtain a solid, wash the solid with ethanol aqueous solution 5 times, and freeze-dry to obtain layered graphene;
[0011] S3. adding the layered graphene obtained in step S2 to an aqueous solution of titanyl sulfate, allowing to stand for 8-12 hours, and then filtering to obtain a layered graphene composite material containing an aqueous solution of titanyl sulfate between the layers;
[0012] S4. adding the layered graphene composite material obtained in step S3 to an aqueous sodium hydroxide solution, stirring for 2-3 hours to obtain a precipitate, filtering the precipitate, washing with water until neutral, and freeze-drying to obtain a graphene-titanium hydroxide composite;
[0013] S5. calcining the graphene-titanium hydroxide composite obtained in step S4 for 2-5 hours under a nitrogen atmosphere to obtain a graphene-titanium dioxide nanocomposite material.
[0014] Furthermore, in step S1 of the present invention, the average particle size of the granular natural graphite is 50 μm, the mass concentration of concentrated sulfuric acid is 98%, the number average molecular weight of polytetrahydrofuran diamine is 2000, the mass concentration of aqueous hydrogen peroxide is 30%, the mass concentration of hydrochloric acid solution is 10%, and the ratio of granular natural graphite, sodium nitrate, concentrated sulfuric acid, the first batch of potassium permanganate, the second batch of potassium permanganate, distilled water, polytetrahydrofuran diamine, aqueous hydrogen peroxide, and hydrochloric acid solution is 5 g: 5 g: 50 mL: 1 g: 9 g: 80 mL: (5-10) g: 40 mL: 200 mL.
[0015] Furthermore, in step S2 of the present invention, a PTFE microporous filter membrane with a pore size of 0.22 μm is used during the reduced pressure filtration, and the volume fraction of the ethanol aqueous solution is 95%.
[0016] Furthermore, in step S2 of the present invention, the freeze-drying temperature is -30°C and the time is 2-4 hours.
[0017] Furthermore, in step S3 of the present invention, the concentration of the titanyl sulfate aqueous solution is 0.5-1 mol / mL, and the ratio of the layered graphene obtained in step S2 to the titanyl sulfate aqueous solution is (0.5-1) g:(10-20) mL.
[0018] Furthermore, in step S4 of the present invention, the concentration of the sodium hydroxide aqueous solution is 0.5-1 mol / mL, and the ratio of the layered graphene composite material obtained in step S3 to the sodium hydroxide aqueous solution is (2-5) g:(50-100) mL.
[0019] Furthermore, in step S4 of the present invention, the freeze-drying temperature is -30°C and the time is 2-4 hours.
[0020] Furthermore, in step S5 of the present invention, the calcination temperature is 500-700°C.
[0021] Another technical problem to be solved by the present invention is to provide a graphene-titanium dioxide nanocomposite material prepared by the above preparation method.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) Compared with the existing formaldehyde catalytic purifier, the raw materials of the present invention are easy to obtain, low in price, mild in preparation conditions, and suitable for large-scale industrial production in factories.
[0024] (2) The present invention adopts a chemical method to uniformly load the formaldehyde photodegradation catalyst - titanium dioxide on the two-dimensional material - graphene, so that the light receiving area of titanium dioxide is larger. A heterojunction interface is formed between titanium dioxide and graphene, which can expand the light absorption range of titanium dioxide and enhance the light absorption intensity. In addition, the ultra-high room temperature carrier migration rate of graphene can promote the transmission of photogenerated electrons, accelerate the separation of photogenerated electron-hole pairs, and inhibit their recombination, thereby improving the catalytic degradation efficiency of formaldehyde.
[0025] (3) The oxygen-containing functional groups on the surface of the graphene-titanium dioxide nanocomposite material prepared by the present invention can combine with formaldehyde molecules through hydrogen bonds, electrostatic forces, etc., and the reduced conjugated benzene ring region can quickly and continuously adsorb formaldehyde on the catalyst surface through π-π interactions, thereby improving the catalytic efficiency. This mechanism forms a closed loop and can exert a long-term effect, so it has good formaldehyde removal performance.
[0026] (4) The polytetrahydrofuran diamine used in the present invention changes the inertness of the graphene surface, increases the spacing between graphene sheets, and increases the loading amount of titanium dioxide, so that titanium dioxide can be evenly compounded with graphene, thereby effectively improving the formaldehyde removal effect of the graphene-titanium dioxide nanocomposite material.
[0027] (5) At present, indoor air purification mostly adopts air purifiers, which belong to the category of small household appliances. The quality varies greatly and the overall demand has seriously declined. Unlike air purifiers, the graphene-titanium dioxide nanocomposite material prepared by the present invention is a material with both formaldehyde removal and decorative functions. It does not require equipment investment or energy supply. For users, a one-time investment can obtain long-term benefits, which is more cost-effective.
[0028] (6) The graphene-titanium dioxide nanocomposite material provided by the present invention can be applied to coatings to prepare high-efficiency formaldehyde purification functional coatings, which are environmentally friendly, economical, and meet the sustainable development strategy. DETAILED DESCRIPTION
[0029] The present invention will be described in detail below in conjunction with specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0030] Example 1
[0031] The graphene-titanium dioxide nanocomposite was prepared by the following steps:
[0032] S1. Add granular natural graphite with an average particle size of 50 μm and sodium nitrate into a three-necked flask, cool to 0°C in a cold bath, add concentrated sulfuric acid with a mass concentration of 98% into the three-necked flask, stir and react for 20 minutes, and keep the temperature of the reaction system no higher than 5°C; add the first batch of potassium permanganate into the three-necked flask, stir and react for 20 minutes, and keep the temperature of the reaction system no higher than 10°C; add the second batch of potassium permanganate into the three-necked flask in 3 equal portions within 1 hour, and keep the temperature of the reaction system no higher than 20°C; remove the cold bath, heat the reaction system to 40°C in a water bath, and stir and react for 2 hours to obtain a suspension; add distilled water droplets into the suspension, and heat the system to 40°C. The temperature was raised to 50°C, polytetrahydrofuran diamine with a number average molecular weight of 2000 was added, and the mixture was kept warm for reaction for 3 hours to obtain a reaction solution; a 30% aqueous hydrogen peroxide solution was added to the reaction solution, and the mixture was stirred at 50°C for 30 minutes, and then a 10% hydrochloric acid solution was added, and the mixture was stirred at 50°C for 30 minutes, and the mixture was cooled to room temperature to obtain a graphene oxide solution, wherein the proportions of granular natural graphite, sodium nitrate, concentrated sulfuric acid, the first batch of potassium permanganate, the second batch of potassium permanganate, distilled water, polytetrahydrofuran diamine, aqueous hydrogen peroxide solution, and hydrochloric acid solution were 5g:5g:50mL:1g:9g:80mL:8g:40mL:200mL;
[0033] S2. Using a PTFE microporous filter with a pore size of 0.22 μm, the graphene oxide solution obtained in step S1 was filtered under reduced pressure to obtain a solid, the solid was washed 5 times with a 95% ethanol aqueous solution by volume fraction, and freeze-dried at -30°C for 3 h to obtain layered graphene;
[0034] S3. The layered graphene obtained in step S2 was added to an aqueous solution of titanyl sulfate at a concentration of 0.8 mol / mL according to a ratio of 0.7 g: 15 mL, and filtered to obtain a layered graphene composite material containing an aqueous solution of titanyl sulfate between the layers after standing for 10 h;
[0035] S4. The layered graphene composite material obtained in step S3 was added to a sodium hydroxide aqueous solution having a concentration of 0.7 mol / mL in a ratio of 4 g:80 mL, stirred for 2.5 h to obtain a precipitate, the precipitate was filtered and washed with water to neutrality, and freeze-dried at -30 ° C for 3 h to obtain a graphene-titanium hydroxide composite;
[0036] S5. The graphene-titanium hydroxide composite obtained in step S4 is calcined at 600° C. for 4 h under a nitrogen atmosphere to obtain a graphene-titanium dioxide nanocomposite material.
[0037] Example 2
[0038] The graphene-titanium dioxide nanocomposite was prepared by the following steps:
[0039] S1. Add granular natural graphite with an average particle size of 50 μm and sodium nitrate into a three-necked flask, cool to 0°C in a cold bath, then add concentrated sulfuric acid with a mass concentration of 98% into the three-necked flask, stir and react for 10 minutes, and keep the temperature of the reaction system no higher than 5°C; add the first batch of potassium permanganate into the three-necked flask, stir and react for 10 minutes, and keep the temperature of the reaction system no higher than 10°C; add the second batch of potassium permanganate into the three-necked flask in 3 equal portions within 1 hour, and keep the temperature of the reaction system no higher than 20°C; remove the cold bath, heat the reaction system to 35°C in a water bath, and stir and react for 2 hours to obtain a suspension; add distilled water droplets into the suspension, and heat the system to 40°C. The temperature was raised to 50°C, polytetrahydrofuran diamine with a number average molecular weight of 2000 was added, and the mixture was kept warm for 2 hours to obtain a reaction solution; a 30% aqueous hydrogen peroxide solution was added to the reaction solution, and the mixture was stirred at 50°C for 30 minutes, and then a 10% hydrochloric acid solution was added, and the mixture was stirred at 50°C for 30 minutes, and the mixture was cooled to room temperature to obtain a graphene oxide solution, wherein the proportions of granular natural graphite, sodium nitrate, concentrated sulfuric acid, the first batch of potassium permanganate, the second batch of potassium permanganate, distilled water, polytetrahydrofuran diamine, aqueous hydrogen peroxide solution, and hydrochloric acid solution were 5g:5g:50mL:1g:9g:80mL:5g:40mL:200mL;
[0040] S2. Using a PTFE microporous filter with a pore size of 0.22 μm, the graphene oxide solution obtained in step S1 was filtered under reduced pressure to obtain a solid, the solid was washed 5 times with a 95% ethanol aqueous solution by volume, and freeze-dried at -30°C for 2 h to obtain layered graphene;
[0041] S3. The layered graphene obtained in step S2 was added to an aqueous solution of titanyl sulfate at a concentration of 0.5 mol / mL according to a ratio of 0.5 g: 10 mL, and the layered graphene composite material containing an aqueous solution of titanyl sulfate between the layers was filtered after standing for 8 h;
[0042] S4. The layered graphene composite material obtained in step S3 was added to a sodium hydroxide aqueous solution having a concentration of 0.5 mol / mL in a ratio of 2 g:50 mL, stirred for 2 h to obtain a precipitate, the precipitate was filtered and washed with water to neutrality, and freeze-dried at -30 ° C for 2 h to obtain a graphene-titanium hydroxide composite;
[0043] S5. The graphene-titanium hydroxide composite obtained in step S4 is calcined at 500° C. for 5 h under a nitrogen atmosphere to obtain a graphene-titanium dioxide nanocomposite material.
[0044] Example 3
[0045] The graphene-titanium dioxide nanocomposite was prepared by the following steps:
[0046] S1. Add granular natural graphite with an average particle size of 50 μm and sodium nitrate into a three-necked flask, cool to 0°C in a cold bath, then add concentrated sulfuric acid with a mass concentration of 98% into the three-necked flask, stir and react for 30 minutes, and keep the temperature of the reaction system no higher than 5°C; add the first batch of potassium permanganate into the three-necked flask, stir and react for 30 minutes, and keep the temperature of the reaction system no higher than 10°C; add the second batch of potassium permanganate into the three-necked flask in 3 equal portions within 1 hour, and keep the temperature of the reaction system no higher than 20°C; remove the cold bath, heat the reaction system to 45°C in a water bath, and stir and react for 2 hours to obtain a suspension; add distilled water droplets into the suspension, and the system temperature The temperature was raised to 50° C., polytetrahydrofuran diamine with a number average molecular weight of 2000 was added, and the mixture was kept warm for 4 hours to obtain a reaction solution; a 30% aqueous hydrogen peroxide solution was added to the reaction solution, and the mixture was stirred at 50° C. for 30 minutes, and then a 10% hydrochloric acid solution was added, and the mixture was stirred at 50° C. for 30 minutes, and the mixture was cooled to room temperature to obtain a graphene oxide solution, wherein the proportions of granular natural graphite, sodium nitrate, concentrated sulfuric acid, the first batch of potassium permanganate, the second batch of potassium permanganate, distilled water, polytetrahydrofuran diamine, aqueous hydrogen peroxide solution, and hydrochloric acid solution were 5 g: 5 g: 50 mL: 1 g: 9 g: 80 mL: 10 g: 40 mL: 200 mL;
[0047] S2. Using a PTFE microporous filter with a pore size of 0.22 μm, the graphene oxide solution obtained in step S1 was filtered under reduced pressure to obtain a solid, the solid was washed 5 times with a 95% ethanol aqueous solution by volume, and freeze-dried at -30°C for 4 h to obtain layered graphene;
[0048] S3. The layered graphene obtained in step S2 was added to an aqueous solution of titanyl sulfate at a concentration of 1 mol / mL according to a ratio of 1 g: 20 mL, and filtered to obtain a layered graphene composite material containing an aqueous solution of titanyl sulfate between the layers after standing for 12 h;
[0049] S4. The layered graphene composite material obtained in step S3 was added to a sodium hydroxide aqueous solution having a concentration of 1 mol / mL at a ratio of 5 g:100 mL, stirred for 3 h to obtain a precipitate, the precipitate was filtered and washed with water until neutral, and freeze-dried at -30 ° C for 4 h to obtain a graphene-titanium hydroxide composite;
[0050] S5. The graphene-titanium hydroxide composite obtained in step S4 is calcined at 700° C. for 2 h under a nitrogen atmosphere to obtain a graphene-titanium dioxide nanocomposite material.
[0051] Comparative Example 1: The difference from Example 1 is that polytetrahydrofuran diamine is not used in step S1.
[0052] Experimental Example 1:
[0053] The experimental objects are the graphene-titanium dioxide nanocomposites prepared in Examples 1-3 and Comparative Example 1. 500 g of the experimental objects are placed in a volume of 1 m 3 0.6 mg of formaldehyde gas was introduced into the sealed glass cover. After 2 hours, the formaldehyde concentration in each sealed glass cover was measured, and the formaldehyde adsorption rate was calculated according to the following formula:
[0054] Formaldehyde adsorption rate = (0.6-formaldehyde concentration) / 0.6×100%; where formaldehyde adsorption rate, %; formaldehyde concentration, mg / m 3 .
[0055] The higher the formaldehyde adsorption rate, the better the formaldehyde removal performance. The experimental results are shown in Table 1:
[0056] Table 1
[0057] Experimental samples Formaldehyde adsorption rate (%) Example 1 95.8 Example 2 95.3 Example 3 95.5 Comparative Example 1 82.2
[0058] As can be seen from Table 1, the formaldehyde adsorption rates of Examples 1-3 of the present invention are all relatively high, indicating that the graphene-titanium dioxide nanocomposite prepared by the present invention has good formaldehyde removal performance. Part of the raw materials of Comparative Example 1 are different from those of Example 1. Compared with Example 1, the formaldehyde adsorption rate of Comparative Example 1 is significantly reduced, indicating that the polytetrahydrofuran diamine used in the preparation method of the present invention can effectively improve the formaldehyde removal performance of the graphene-titanium dioxide nanocomposite.
[0059] Application Example 1: Graphene-titanium dioxide nanocomposite latex paint
[0060] The graphene-titanium dioxide nanocomposite material prepared in Example 1 is further used to prepare a graphene-titanium dioxide nanocomposite latex paint. The components of the composite latex paint are, by weight, 240 parts of vinyl acetate-ethylene copolymer emulsion, 120 parts of pigment, 50 parts of the graphene-titanium dioxide nanocomposite material prepared in Example 1, 280 parts of filler, 4 parts of hydroxyethyl cellulose, 6 parts of dispersant, 2 parts of defoamer, 6 parts of thickener, 1 part of wetting agent, 2 parts of pH regulator, and 280 parts of water.
[0061] The preparation method of the graphene-titanium dioxide nanocomposite latex paint comprises the following steps:
[0062] S1: Start the disperser, adjust the speed to 500r / min, add half the weight of dispersant and defoamer, stir for 2 minutes, add filler and stir for 1 minute; add hydroxyethyl cellulose, adjust the speed to 1000r / min; add pigment, wetting agent and half the weight of water, adjust the speed of the disperser and the feeding speed during the addition of pigment to ensure that the powder does not accumulate; add pH regulator, adjust the speed to 1200r / min, and disperse at high speed for 20 minutes to make the fineness below 50μm;
[0063] S2: Adjust the speed to 1200r / min, add thickener, vinyl acetate-ethylene copolymer emulsion, remaining dispersant, defoamer and water in sequence, and stir for 4 minutes;
[0064] S3: adjusting the speed to 500 r / min, adding the graphene-titanium dioxide nanocomposite material prepared in Example 1, and stirring for 2 min to obtain a latex paint;
[0065] S4: Use a 120-mesh sieve to filter the prepared latex paint to prevent solid particles or other impurities from mixing in and affecting the effect;
[0066] S5: Take samples to test product quality, put the treated latex paint into barrels, and seal them to prevent oxidation or contamination of the latex paint.
[0067] Comparative Example 2: The difference from Application Example 1 is that the composition of the composite latex paint does not include the graphene-titanium dioxide nanocomposite material prepared in Example 1.
[0068] Application Example 2: Graphene-titanium dioxide nanocomposite wood paint
[0069] The graphene-titanium dioxide nanocomposite material prepared in Example 1 is further used to prepare a graphene-titanium dioxide nanocomposite wood paint. The composite wood paint comprises, in parts by weight, 15 parts of ethyl acrylate, 5 parts of n-butyl acrylate, 20 parts of a composite monomer of methyl methacrylate and vinyl triisopropoxy silane, 1 part of an initiator, 2 parts of sodium vinyl sulfonate, 1 part of sodium dodecyl sulfate, 1 part of a pH adjuster, 5 parts of the graphene-titanium dioxide nanocomposite material prepared in Example 1, and 50 parts of water.
[0070] The preparation method of the graphene-titanium dioxide nanocomposite wood paint comprises the following steps:
[0071] S1: In an emulsification tank, add water, initiator, sodium vinyl sulfonate and sodium vinyl sulfonate, dissolve and mix;
[0072] S2: Start the disperser, adjust the speed to 200r / min, slowly add ethyl acrylate, n-butyl acrylate, methyl methacrylate and vinyl triisopropoxysilane to react for 3h;
[0073] S3: adjusting the speed to 500 r / min, adding the graphene-titanium dioxide nanocomposite material prepared in Example 1, and stirring for 2 min;
[0074] S4: adding a pH adjuster to adjust the pH value to below 9 to obtain a wood paint;
[0075] S5: Use a 500-mesh sieve to filter the wood paint to prevent solid particles or other impurities from mixing in and affecting the effect;
[0076] S6: Take samples to test product quality, put the treated wood paint into barrels and seal them to prevent oxidation or contamination.
[0077] Comparative Example 3: The difference from Application Example 2 is that the composition of the composite wood paint does not include the graphene-titanium dioxide nanocomposite material prepared in Example 1.
[0078] Experimental Example 2:
[0079] The experimental objects are application examples 1-2 and comparative examples 2-3. The formaldehyde purification efficiency of each experimental object is tested with reference to "JCT2008-2013 Purification Performance of Indoor Air Purification Adsorption Materials". The higher the formaldehyde purification efficiency, the better the formaldehyde removal performance of the coating. The experimental results are shown in Table 2.
[0080] Table 2
[0081] Experimental samples Formaldehyde purification efficiency (%) Application Example 1 ≥75 Comparative Example 2 ≤10 Application Example 2 ≥80 Comparative Example 3 ≤10
[0082] It can be seen from Table 2 that the formaldehyde purification efficiency of Application Examples 1-2 of the present invention is relatively high, while the formaldehyde purification efficiency of Comparative Examples 2 and 3 is very low, indicating that the graphene-titanium dioxide nanocomposite material prepared by the present invention can greatly improve the formaldehyde removal performance of the coating after being applied to the coating.
[0083] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a graphene-titanium dioxide nanocomposite material, characterized in that: The following steps are involved: S1. Add granular natural graphite and sodium nitrate to a three-necked flask, cool to 0°C with a cold bath, add concentrated sulfuric acid to the three-necked flask, stir and react for 10-30 minutes, and keep the temperature of the reaction system not higher than 5°C; add the first batch of potassium permanganate to the three-necked flask, stir and react for 10-30 minutes, and keep the temperature of the reaction system not higher than 10°C; add the second batch of potassium permanganate to the three-necked flask in 3 equal portions within 1 hour, and keep the temperature of the reaction system not higher than 20°C; remove the cold bath, use a water bath to heat the reaction system to 35-45°C, stir and react for 2 hours to obtain a suspension; add distilled water dropwise to the suspension, raise the system temperature to 50°C, add polytetrahydrofuran diamine, and then keep warm for 2-4 hours to obtain a reaction solution; add an aqueous hydrogen peroxide solution to the reaction solution, stir at 50°C for 30 minutes, then add a hydrochloric acid solution, stir at 50°C for 30 minutes, and cool to room temperature to obtain a graphene oxide solution; S2. Filter the graphene oxide solution obtained in step S1 under reduced pressure to obtain a solid, wash the solid with ethanol aqueous solution 5 times, and freeze-dry to obtain layered graphene; S3. adding the layered graphene obtained in step S2 to an aqueous solution of titanyl sulfate, allowing to stand for 8-12 hours, and then filtering to obtain a layered graphene composite material containing an aqueous solution of titanyl sulfate between layers; S4. adding the layered graphene composite material obtained in step S3 to an aqueous sodium hydroxide solution, stirring for 2-3 hours to obtain a precipitate, filtering the precipitate, washing with water until neutral, and freeze-drying to obtain a graphene-titanium hydroxide composite; S5. calcining the graphene-titanium hydroxide composite obtained in step S4 for 2-5 hours under a nitrogen atmosphere to obtain a graphene-titanium dioxide nanocomposite material.
2. The method for preparing a graphene-titanium dioxide nanocomposite material according to claim 1, characterized in that: In the step S1, the average particle size of the granular natural graphite is 50 μm, the mass concentration of concentrated sulfuric acid is 98%, the number average molecular weight of polytetrahydrofuran diamine is 2000, the mass concentration of the hydrogen peroxide aqueous solution is 30%, the mass concentration of the hydrochloric acid solution is 10%, and the ratio of the granular natural graphite, sodium nitrate, concentrated sulfuric acid, the first batch of potassium permanganate, the second batch of potassium permanganate, distilled water, polytetrahydrofuran diamine, hydrogen peroxide aqueous solution, and hydrochloric acid solution is 5g:5g:50mL:1g:9g:80mL:(5-10)g:40mL:200mL.
3. The method for preparing a graphene-titanium dioxide nanocomposite material according to claim 1, characterized in that: In the step S2, a PTFE microporous filter membrane with a pore size of 0.22 μm is used during the reduced pressure filtration, and the volume fraction of the ethanol aqueous solution is 95%.
4. The method for preparing a graphene-titanium dioxide nanocomposite material according to claim 1, characterized in that: In step S2, the freeze-drying temperature is -30°C and the time is 2-4 hours.
5. The method for preparing a graphene-titanium dioxide nanocomposite material according to claim 1, characterized in that: In the step S3, the concentration of the titanyl sulfate aqueous solution is 0.5-1 mol / mL, and the ratio of the layered graphene obtained in the step S2 to the titanyl sulfate aqueous solution is (0.5-1) g:(10-20) mL.
6. The method for preparing a graphene-titanium dioxide nanocomposite material according to claim 1, characterized in that: In the step S4, the concentration of the sodium hydroxide aqueous solution is 0.5-1 mol / mL, and the ratio of the layered graphene composite material obtained in the step S3 to the sodium hydroxide aqueous solution is (2-5) g: (50-100) mL.
7. The method for preparing a graphene-titanium dioxide nanocomposite material according to claim 1, characterized in that: In step S4, the freeze-drying temperature is -30°C and the time is 2-4 hours.
8. The method for preparing a graphene-titanium dioxide nanocomposite material according to claim 1, characterized in that: In the step S5, the calcination temperature is 500-700°C.
9. The graphene-titanium dioxide nanocomposite material obtained according to the preparation method of claims 1 to 8.
Citation Information
Patent Citations
Modified graphene oxide and epoxy resin composite material and method for preparing same
CN105906842A
Preparation method and application of reduced graphene oxide / TiO2 composite photocatalyst material
CN107519856A
Lamellate graphene / metallic oxide nanocomposite and preparation method thereof
CN108946801A
Modified graphene enhanced impact-resistant polyurea coating and preparation method thereof
CN114015333A