Pt-based catalyst based on SMSI effect regulation and control as well as preparation method and application of Pt-based catalyst
By modulating the SMSI effect, a Pt-based catalyst was prepared, which solved the problem of insufficient selectivity in the selective hydrogenation reaction of cinnamaldehyde in the existing technology, achieving high efficiency catalysis and cost reduction, and facilitating industrial application.
Patent Information
- Application Number
- CN202411073465.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing technology, the selective hydrogenation catalysts for α,β-unsaturated aldehydes have insufficient selectivity, and it is difficult to effectively control the electronic and geometric effects of the catalyst, resulting in poor product selectivity.
By modulating the SMSI effect, a Pt-based catalyst containing a reducible metal oxide composite support was prepared. Pt metal was loaded using precipitation deposition and wet chemical impregnation methods to form a Pt-based catalyst for the selective hydrogenation reaction of cinnamaldehyde.
It achieves highly efficient catalysis of the hydrogenation reaction of cinnamaldehyde, enhances the selectivity and activity of the catalyst, reduces costs, and has universality, making it easy for industrial production.
Smart Images

Figure CN118988315A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of nanomaterials, and in particular relates to a universal method for flexibly regulating the surface structure of a Pt noble metal catalyst and thus regulating the selective hydrogenation of unsaturated functional groups by regulating the SMSI effect. Technical Background
[0002] Common α,β-unsaturated aldehydes include cinnamaldehyde, citral, crotonaldehyde, and furfural. The selective hydrogenation of these compounds is an important chemical transformation process in the production of fine chemicals such as fragrances, medicines, and cosmetics. However, the selective hydrogenation of α,β-unsaturated aldehydes involves a variety of products. Taking cinnamaldehyde (CAL) as an example, without considering other by-products, its catalytic hydrogenation products mainly include three types: cinnamylalcohol (COL) obtained by selective hydrogenation of the C=O double bond, hydrocinnamaldehyde (HCAL) obtained by selective hydrogenation of the C=C double bond, and hydrocinnamylalcohol (HCOL) obtained by hydrogenation of both the C=C double bond and the C=O double bond. Strong metal-support interaction (SMSI) is a special form of interaction that is usually observed between metal nanoparticles (NPs) and reducible supports. In 1978, Tauster et al. first discovered that the chemical adsorption ability of TiO2-supported Group VIII noble metals for small gas molecules such as CO and H2 suddenly disappeared after reduction treatment at 500°C. In this case, the term SMSI was proposed to describe this phenomenon, which was once believed to be caused by the electronic perturbation formed by the Pt-Ti bond. Later, subsequent studies confirmed the coating of metal NPs by migrating supporting species. In addition, this reduction-induced SMSI is reversible after high-temperature oxidation treatment, and the coating layer disappears. The SMSI effect forms a coating structure, causes electronic effects, and can also regulate the geometric structure and regulate the electronic or coordination environment. Therefore, understanding the SMSI behavior is of great significance for regulating the catalytic performance of metal species. Due to the limited selectivity of catalytic hydrogenation of cinnamaldehyde, the industry still needs catalysts with better selectivity. Summary of the invention
[0003] In view of this, the present invention provides a Pt-based catalyst regulated based on the SMSI effect, a preparation method and use thereof, wherein a composite carrier material containing a reducible metal oxide is prepared, the SMSI effect is regulated, and Pt metal is loaded, and a Pt-based catalyst is synthesized by a precipitation deposition method and a wet chemical impregnation method. The catalyst is used in the selective hydrogenation reaction of cinnamaldehyde and has the effect of efficient catalytic hydrogenation.
[0004] To this end, the technical solution of the present invention is as follows: a method for preparing a Pt-based catalyst regulated by SMSI effect, comprising the following steps:
[0005] S1: preparing the oxide composite support by a precipitation deposition method, followed by aging and calcination;
[0006] S2: mixing the platinum salt solution and the composite carrier in a solvent, and removing the solvent to obtain a mixture of the platinum salt and the composite carrier; the solvent is deionized water or ethanol;
[0007] S3: reducing the mixture under H2 atmosphere to obtain a Pt-based catalyst regulated based on SMSI effect, wherein the mass fraction of Pt in the catalyst is 0.5-3wt%.
[0008] The composite carrier is a composite material formed by a reducible metal oxide and a non-reducible metal oxide or a carbon material.
[0009] Furthermore, the reducible metal oxide includes one of the oxides of Fe, Co, Ni, Sn, Zr, Ce, Ti, Gd and Nb; the non-reducible metal oxide includes aluminum oxide or magnesium oxide; and the carbon material includes one of BP2000, diamond carbon, EC-300J and carbon nanotubes.
[0010] Furthermore, the weight ratio of the reducible metal oxide to the non-reducible metal oxide or carbon material is 1:(1-5).
[0011] The reducible metal oxide is obtained by precipitation of a soluble metal salt solution in an alkaline environment. The metal salt is a nitrate, acetate or acetylacetonate of Fe, Co, Ni, Sn, Zr, Ce, Ti, Gd and Nb; the alkaline environment is obtained by dripping ammonia water, urea or sodium hydroxide solution.
[0012] Furthermore, in step S1, the aging temperature is 50-100° C., the time is 0.5-3 h, the calcination temperature is 200-400° C., and the calcination time is 1-5 h.
[0013] Furthermore, in step S3, the reduction temperature is 300-1000°C.
[0014] The present invention also protects a Pt-based catalyst regulated based on the SMSI effect, which is prepared according to the above method. The use of the obtained Pt-based catalyst regulated based on the SMSI effect is that it can be used in hydrogenation reactions, such as the reaction of preparing cinnamyl alcohol by hydrogenation of cinnamaldehyde. By regulating the SMSI effect, the electronic effect and geometric effect of the catalyst are adjusted, and the catalytic activity and selectivity can be flexibly regulated. Not only does it increase the effective utilization of platinum atoms, it can also reduce the cost of the catalyst, which is beneficial to catalytic research and application. At the same time, the method is simple and universal, and is easy to industrialize.
[0015] Compared with the prior art, the beneficial effect of the present invention is that the reducible component in the oxide composite carrier of the present invention forms a coordination bond with the noble metal, thereby improving the interaction between the metal and the composite carrier. The catalyst obtained by the present invention can flexibly regulate the catalytic activity and selectivity by regulating the SMSI effect, thereby adjusting the electronic effect and geometric effect of the catalyst. Not only does it increase the effective utilization of platinum atoms, but it can also reduce the cost of the catalyst, which is beneficial to catalytic research and application. At the same time, the method is simple and universal, and is easy to industrialize. It can be used in the hydrogenation reaction of cinnamaldehyde, and has the effect of efficient catalytic hydrogenation. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is the nitrogen adsorption-desorption curve of the AF composite carrier provided in Example 1 of the present invention.
[0017] Figure 2 This is the XRD diagram of the AF composite carrier provided in Example 1 of the present invention.
[0018] Figure 3 This is the nitrogen adsorption-desorption curve of the F composite carrier provided in Example 2 of the present invention.
[0019] Figure 4 This is the XRD diagram of the F composite carrier provided in Example 2 of the present invention.
[0020] Figure 5 This is the TEM image of Pt / AF provided in Example 3 of the present invention.
[0021] Figure 6 This is the EDX-mapping diagram of Pt / AF provided in Example 3 of the present invention.
[0022] Figure 7 This is the HRTEM image of Pt / AF provided in Example 3 of the present invention.
[0023] Figure 8 TEM image of the Pt / Al2O3 catalyst provided in Example 4.
[0024] Fig. 9HRTEM image of the Pt / Al2O3 catalyst provided in Example 4.
[0025] Fig.10 This is the reaction formula for the selective hydrogenation of cinnamaldehyde.
[0026] Fig.11 This is a comparison chart of the selective hydrogenation performance of cinnamaldehyde using different catalysts in Examples 6-9.
[0027] Fig.12 This is a kinetic curve diagram of the selective hydrogenation of cinnamaldehyde in Example 6 of the present invention. Specific implementation methods
[0029] The composite carrier of the Pt-based catalyst and the preparation method of the catalyst used in the present invention will be further described in detail below in conjunction with the accompanying drawings and specific examples.
[0030] Example 1
[0031] The synthesis of the Fe2O3-Al2O3 composite carrier is carried out as follows:
[0032] After dissolving 2-3g of hydrated ferric nitrate in 100-200mL of deionized water, add about 0.5g of alumina, add ammonia water drop by drop to adjust the pH to 10-12, so that the metal salt solution is precipitated in an alkaline environment, and then the above mixture is placed in an oven and maintained at 70-100°C for 30-90min to mature the required composite carrier. After maturation, vacuum filter and wash the ammonia water with deionized water several times. The above solid is placed in a vacuum oven and dried at 60-100°C for 10-18h. After drying, the above solid is placed in a muffle furnace and heated to 200-400°C at a rate of 3-10°C / min, and maintained for 1-5h to calcine the composite carrier, in which the weight ratio of Fe2O3 to Al2O3 is 1:5.
[0033] The calcined solid was ground into powder and labeled as composite carrier AF for use in the next step of preparing the catalyst. Figure 1 , Figure 2 The nitrogen adsorption-desorption curve and X-ray diffraction (XRD) diagram of the AF composite material provided in Example 1 of the present invention are shown in FIG. The specific surface area of the material is 210 m 2 / g, and the average pore size is 17nm. The XRD results are compared with the standard card, indicating that there is no obvious characteristic peak of iron oxide, indicating that the crystallinity of iron oxide is relatively poor and it is an amorphous material.
[0034] Example 2
[0035] Preparation of Fe2O3 composite carrier
[0036] After dissolving hydrated ferric nitrate in deionized water, add ammonia water to adjust the pH to 10-12, and then place the mixture in an oven at 70-100°C for 30-90 minutes to mature the desired composite carrier. After maturation, use a filter funnel to vacuum filter and wash off the ammonia water with deionized water for several times; after filtering out most of the water, place the solid in a vacuum oven and dry at 60-100°C for 10-18 hours. After drying, place the solid in a muffle furnace and heat to 200-400°C at a rate of 3-10°C / min for 1-5 hours to calcine the composite carrier.
[0037] The calcined solid was ground into powder, marked as composite carrier F, and used for the next step of preparing the catalyst. Figure 3 , Figure 4 The nitrogen adsorption-desorption curve and XRD diagram of the F composite material provided in Example 2 of the present invention are shown in FIG. The specific surface area of the material is 50 m 2 / g, and the average pore size is 18nm. The XRD results are compared with the standard card, and the prepared material is a typical Fe2O3 material.
[0038] Example 3
[0039] Preparation of Pt / Fe2O3-Al2O3 Composite Support Catalyst (Pt / AF for short)
[0040] Weigh 200 mg of the Fe2O3-Al2O3 composite carrier obtained in Example 1 and add it to a round-bottom flask containing 30-50 mL of deionized water, add a certain amount of Pt salt solution and mix it evenly. Ultrasonicate the mixed solution obtained above for 30 minutes, and then stir it at room temperature for 12 hours to make the precursor and the composite carrier fully mixed. The mixed solution is rotary evaporated to obtain a dry powder mixture, and then the mixture is transferred to a crucible for reduction in a 5vol% H2 / Ar mixed gas, the heating rate is controlled at 5-10℃ / min, the temperature is raised to 300-1000℃, and the temperature is kept for 2-4 hours. The amount of Pt salt solution added makes the mass fraction of Pt in the Pt / Fe2O3-Al2O3 composite carrier catalyst be 1wt%.
[0041] The catalyst was Pt / Fe2O3-Al2O3 composite carrier catalyst (Pt / AF for short) and the temperature was naturally lowered to room temperature. Transmission electron microscopy (TEM) showed that the size of Pt nanoparticles was generally 3-5nm ( Figure 5 ), and some large particles were also generated. EDX-mapping showed that Pt and Fe partially formed alloys ( Figure 6 ), and high-resolution transmission electron microscopy (HRTEM) showed that a coating layer ( Figure 7 ).
[0042] Example 4
[0043] Preparation of Pt / Al2O3 Catalyst
[0044] Weigh 200 mg of the Al2O3 oxide composite carrier obtained in Example 2 and add it to a round-bottom flask containing 30-50 mL of deionized water, add a certain amount of Pt salt solution thereto and mix evenly. Ultrasonicate the mixed solution obtained above for 30 minutes, and then stir it at room temperature for 12 hours to fully mix the precursor and the composite carrier. The mixed solution is rotary evaporated to obtain a dry powder mixture, and then the mixture is transferred to a crucible for reduction in a 5 vol% H2 / Ar mixed gas, the heating rate is controlled at 5-10°C / min, the temperature is raised to 300-1000°C, and the temperature is kept for 1-2 hours. The amount of Pt salt solution added is such that the mass fraction of Pt in the Pt / Al2O3 catalyst is 1wt%.
[0045] The Pt / Al2O3 (Pt / A for short) catalyst can be obtained by naturally cooling the temperature to room temperature. Figure 8 It can be seen from the TEM image that the particle size of the prepared catalyst is mostly concentrated in the range of 3-5 nm. Fig. 9 HRTEM electron microscope surface showed that there was no obvious coating on the catalyst surface.
[0046] Example 5
[0047] Preparation of Pt / Fe2O3 catalyst (Pt / F for short)
[0048] Weigh 200 mg of composite carrier Fe2O3 (abbreviated as F) and add it to a round-bottom flask containing 30-50 mL of deionized water, add a certain amount of Pt salt solution and mix evenly. Ultrasonicate the obtained mixed solution for 30 minutes, and then stir it at room temperature for 12 hours to make the precursor and the composite carrier fully mixed. The mixed solution is rotary evaporated to obtain a dry powder mixture, and then the mixture is transferred to a crucible for reduction in a 5 vol% H2 / Ar mixed gas, the heating rate is controlled at 5-10℃ / min, the temperature is raised to 300-1000℃, and the temperature is kept for 1-2 hours.
[0049] The temperature is naturally lowered to room temperature to obtain a Pt / Fe2O3 (Pt / F for short) catalyst. Similarly, the amount of Pt salt solution added is controlled so that the mass fraction of Pt in the Pt / Fe2O3 catalyst is 1wt%.
[0050] Example 6
[0051] Selective hydrogenation of cinnamaldehyde using Pt / AF catalyst
[0052] Use ethanol, ethyl acetate, etc. to clean the reaction bottle and the magnet, then place a mixture of 3mL isopropanol and deionized water, 0.15mol cinnamaldehyde and 10mg Pt / AF catalyst in a magnetic stirring kettle; after heating the reactor to 100℃, fill and release the high-pressure reactor with 5MPaH2 for 3-5 times to exhaust the air, and then fill it with 1MPaH2. React under this condition for 1h. Take samples in automatic injection bottles. Use gas chromatography to determine the product mixture.
[0053] Example 7
[0054] Selective hydrogenation of cinnamaldehyde using Pt / A catalyst
[0055] Use ethanol, ethyl acetate, etc. to clean the reaction bottle and the magnet, then place a mixture of 3mL isopropanol and deionized water, 0.15mol cinnamaldehyde and 10mg Pt / A catalyst in a magnetic stirring kettle; after heating the reactor to 100℃, fill and release the high-pressure reactor with 5MPaH2 for 3-5 times to exhaust the air, and then fill it with 1MPaH2. React under this condition for 1h. Take samples in automatic injection bottles. Use gas chromatography to determine the product mixture.
[0056] Example 8
[0057] Selective hydrogenation of cinnamaldehyde using Pt / F catalyst
[0058] Use ethanol, ethyl acetate, etc. to clean the reaction bottle and the magnet, then place a mixture of 3mL isopropanol and deionized water, 0.15mol cinnamaldehyde and 10mg Pt / F catalyst in a magnetic stirring kettle; after heating the reactor to 100℃, fill and release the high-pressure reactor with 5MPaH2 for 3-5 times to exhaust the air, and then fill it with 1MPaH2. React under this condition for 1h. Take samples in automatic injection bottles. Use gas chromatography to determine the product mixture.
[0059] Example 9
[0060] Selective hydrogenation of cinnamaldehyde using commercial Pt / C catalyst
[0061] Use ethanol, ethyl acetate, etc. to clean the reaction bottle and the magnet. Then place 3mL of a mixture of isopropanol and deionized water, 0.15mol of cinnamaldehyde, and 2mg of a commercial Pt / C catalyst in a magnetic stirring kettle. After heating the reactor to 100°C, fill and release the high-pressure reactor with 5MPaH2 for 3-5 times to exhaust the air, and then fill it with 1MPaH2. React under this condition for 1h. Take samples in an automatic injection bottle. Use gas chromatography to determine the product mixture.
[0062] The test results of different catalysts are as follows Fig.11As shown, the reaction conditions are: 100℃, 0.15mol cinnamaldehyde, 3mL solvent (isopropanol: water = 6:1), 10mg catalyst, 1MPaH2, 1h, 800rpm. From the test results, the catalyst Pt / FA, in the reaction of selective hydrogenation of cinnamaldehyde, after 1 hour of reaction, the conversion rate is as high as about 88%, and the selectivity of hydrogenation C=O bond reaches 88%. The activity of commercial Pt / C and 300J-loaded Pt catalysts is not only poor but also very low in the hydrogenation selectivity of C=O bond. Although the Pt catalyst supported by iron oxide also has high selectivity, the catalyst activity is very low, and the catalyst is almost completely deactivated under the reduction condition of 700℃. The Pt catalyst supported by alumina also has very low selectivity for hydrogenation of C=O bond and poor activity. Through the above comparison, we found that our Pt catalyst supported by Fe2O3-Al2O3 composite carrier has good application in the selective hydrogenation of cinnamaldehyde to prepare cinnamyl alcohol. Fig.12 This is the kinetic curve of the selective hydrogenation of cinnamaldehyde over Pt / AF catalyst.
[0063] Example 10
[0064] Preparation of Pt / CNT-Fe2O3 catalyst and selective hydrogenation of cinnamaldehyde
[0065] After dissolving hydrated ferric nitrate in deionized water, carbon nanotubes (CNTs) are dispersed in the above solution, and ammonia water is added to adjust the pH to 10-12. Then, the above mixture is placed in an oven and maintained at 70-100°C for 30-90 minutes to mature the required composite carrier. After maturation, vacuum filter and wash the ammonia water with deionized water several times. The above solid is placed in a vacuum oven and dried at 60-100°C for 10-18 hours. After drying, the above solid is placed in a muffle furnace and heated to 200-400°C at a rate of 3-10°C / min for 1-5 hours. The preparation method of Pt catalyst is the same as that in Example 3, except that AF is replaced by CNT-Fe2O3 composite material.
[0066] Use ethanol, ethyl acetate, etc. to clean the reaction bottle and the magnet, then place 3mL of isopropanol, 0.75mol of cinnamaldehyde and 5mg of Pt / CNT-Fe2O3 catalyst in a magnetic stirring kettle; after heating the reactor to 100℃, fill and discharge the high-pressure reactor with 5MPaH2 for 3-5 times to exhaust the air, and then fill it with 1MPaH2. And react under this condition for 2h. Take samples in automatic injection bottles. The product mixture is determined by gas chromatography. The conversion rate of the reaction result is 43.7%, and the selectivity is as high as 94.3%, which proves that this preparation method has universal applicability.
[0067] The composite carrier of the present invention is a composite material formed by a reducible metal oxide and an irreducible metal oxide or a carbon material. The reducible metal oxide includes one of the oxides of Fe, Co, Ni, Sn, Zr, Ce, Ti, Gd and Nb; the irreducible metal oxide includes aluminum oxide or magnesium oxide; the carbon material includes one of BP2000, diamond carbon, EC-300J and carbon nanotubes. The weight ratio of the reducible metal oxide to the irreducible metal oxide or carbon material is 1:(1-5). That is, the weight ratio of the reducible metal oxide to the irreducible metal oxide is 1:(1-5), or the weight ratio of the reducible metal oxide to the carbon material is 1:(1-5). Example 3 only lists the combination of Fe oxide and aluminum oxide, and the oxides of Co, Ni, Sn, Zr, Ce, Ti, Gd and Nb also have the same technical effect. Example 10 lists the combination of carbon nanotubes and Fe2O3, and the carbon nanotubes can also be replaced by BP2000, diamond carbon, and EC-300J. The obtained catalysts all have highly efficient catalytic effects on the selective hydrogenation reaction of cinnamaldehyde.
[0068] The above-mentioned reducible metal oxides are obtained by precipitation of soluble metal salt solutions in an alkaline environment. The metal salts are nitrates, acetates or acetylacetonates of Fe, Co, Ni, Sn, Zr, Ce, Ti, Gd and Nb; the alkaline environment is obtained by dripping ammonia water, urea or sodium hydroxide solution. The aging temperature is 50-100°C, the time is 0.5-3h, the calcination temperature is 200-400°C, and the calcination time is 1-5h. The reduction temperature is 300-1000°C.
[0069] On the basis of Example 1, the weight ratio of Fe2O3 to Al2O3 was changed, and the Pt / Fe2O3-Al2O3 composite carrier catalyst was prepared according to Example 3 and tested according to the conditions of Example 6. The results are shown in the following table:
[0070] Serial number <![CDATA[Weight ratio of Fe2O3 to Al2O3]]> Cinnamyl alcohol conversion rate Catalyst selectivity 1 1:4 15% 78% 2 1:2 20% 83% 3 1:1 88% 88% 4 1:0.5 11% 81%
[0071] It can be seen from the above table that when the weight ratio of Fe2O3 to Al2O3 is 1:1, the conversion rate of cinnamyl alcohol and the catalyst selectivity are better.
[0072] On the basis of Example 3, the amount of Pt salt solution added was changed to make the mass fraction of Pt in the Pt / Fe2O3-Al2O3 composite carrier catalyst and tested according to the conditions of Example 6. The results are shown in the following table:
[0073] Serial number Mass fraction of Pt (wt%) Cinnamyl alcohol conversion rate Catalyst selectivity 1 0.1 24% 73% 2 0.5 31% 85% 3 1.0 88% 88% 4 3.0 6% 83%
[0074] It can be seen from the above table that when the mass fraction of Pt is 1wt%, the conversion rate of cinnamyl alcohol and the catalyst selectivity are better.
[0075] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field can make some substitutions and deformations to some technical features therein according to the disclosed technical content without creative labor, and these substitutions and deformations are all within the protection scope of the present invention.
Claims
1. A method for preparing a Pt-based catalyst regulated by SMSI effect, characterized in that The steps include: S1: preparing the oxide composite support by a precipitation deposition method, followed by aging and calcination; S2: mixing the platinum salt solution and the composite carrier in a solvent, and removing the solvent to obtain a mixture of the platinum salt and the composite carrier; the solvent is deionized water or ethanol; S3: reducing the mixture under H2 atmosphere to obtain a Pt-based catalyst regulated by SMSI effect, wherein the mass fraction of Pt in the catalyst is 0.5-3 wt%.
2. The method for preparing a Pt-based catalyst based on SMSI effect regulation according to claim 1, characterized in that: The oxide composite carrier is a composite material formed by a reducible metal oxide and a non-reducible metal oxide or a carbon material.
3. The method for preparing a Pt-based catalyst based on SMSI effect regulation according to claim 2, characterized in that: The reducible metal oxide includes one of oxides of Fe, Co, Ni, Sn, Zr, Ce, Ti, Gd and Nb; the non-reducible metal oxide includes aluminum oxide or magnesium oxide; and the carbon material includes one of BP2000, diamond carbon, EC-300J and carbon nanotubes.
4. The method for preparing a Pt-based catalyst based on SMSI effect regulation according to claim 3, characterized in that: The weight ratio of the reducible metal oxide to the non-reducible metal oxide or carbon material is 1:(1-5).
5. The method for preparing a Pt-based catalyst based on SMSI effect regulation according to claim 3, characterized in that: The reducible metal oxide is obtained by precipitation of a soluble metal salt solution in an alkaline environment.
6. The method for preparing a Pt-based catalyst based on SMSI effect regulation according to claim 5, characterized in that: The metal salt is nitrate, acetate or acetylacetonate of Fe, Co, Ni, Sn, Zr, Ce, Ti, Gd and Nb; the alkaline environment is obtained by dripping ammonia water, urea or sodium hydroxide solution.
7. The method for preparing a Pt-based catalyst based on SMSI effect regulation according to claim 1, characterized in that: In step S1, the aging temperature is 50-100°C, the time is 0.5-3 h, the calcination temperature is 200-400°C, and the calcination time is 1-5 h.
8. The method for preparing a Pt-based catalyst based on SMSI effect regulation according to claim 1, characterized in that: In step S3, the reduction temperature is 300-1000°C.
9. A Pt-based catalyst regulated by SMSI effect, characterized in that: Prepared according to the method according to any one of claims 1 to 8.
10. The use of a Pt-based catalyst regulated by SMSI effect according to claim 9, characterized in that: Used in the hydrogenation reaction of cinnamaldehyde.
Citation Information
Cited By
Preparation method and application of Al2O3-MgO-C for preparing cinnamyl alcohol through selective hydrogenation of cinnamyl aldehyde
CN120695807A
Catalyst for preparing cinnamyl alcohol through selective hydrogenation of cinnamyl aldehyde as well as preparation method and application of catalyst
CN122076432A