Micron flower-ball-shaped Ca-doped ZnIn2S4 material, preparation method and application of micron flower-ball-shaped Ca-doped ZnIn2S4 material in photocatalytic hydrogen production
By synthesising micron spherical Ca-doped ZnIn2S4 material by calcium doping and one-step hydrothermal method, the band gap structure and light absorption capacity are optimized, and the existing photocatalyst light absorption range and carrier separation efficiency are solved. The photocatalytic hydrogen production performance has been significantly improved.
Patent Information
- Application Number
- CN202411327097.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing photocatalysts have shortcomings in the light absorption range and the separation efficiency of photogenerated carriers, which limits their application effect in photocatalytic hydrogen production.
By calcium doping on ZnIn2S4 material, a one-step hydrothermal method is used to synthesize micron spherical Ca-doped ZnIn2S4 material to optimize the band gap structure, improve the light absorption capacity and light utilization rate, and enhance the photocatalytic activity.
The photocatalytic activity and cyclic stability of ZnIn2S4 material are significantly improved, and the catalytic hydrogen production performance under visible light is improved, especially when the Ca doping amount is 0.71%, it shows relatively optimal photocatalytic hydrogen production activity.
Smart Images

Figure CN118988348A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photocatalytic material synthesis, and in particular, relates to a micron flower ball-shaped Ca-doped ZnIn2S4 material, a preparation method and application thereof in photocatalytic hydrogen production. Background Art
[0002] Photocatalytic hydrogen production is the process of decomposing water into hydrogen and oxygen under light conditions using photocatalytic materials. This technology is seen as a key solution for sustainable energy. With the growth of global energy demand and the intensification of environmental problems, especially the air pollution and excessive emissions of greenhouse gases caused by the burning of fossil fuels, the development of clean energy has become particularly important. Photocatalytic hydrogen production uses solar energy to convert water into hydrogen, providing a pollution-free, renewable source of energy that can effectively reduce dependence on fossil fuels and the environmental damage it brings. However, existing photocatalysts have deficiencies in the light absorption range and the separation efficiency of photogenerated carriers, which limits the effectiveness of their practical applications. Therefore, improving the performance of photocatalysts is the key to achieving efficient hydrogen production and meeting environmental challenges.
[0003] ZnIn2S4 is a semiconductor material with photocatalytic potential. It exhibits superior performance in photocatalytic applications due to its moderate band gap (about 2.0-2.2eV) and good photostability. However, due to the weak migration and separation efficiency of photogenerated carriers in ZnIn2S4 during photocatalytic reactions, its photocatalytic activity is limited when used as a single component. Therefore, it is necessary to modify the ZnIn2S4 material to further improve its photocatalytic performance. Summary of the invention
[0004] In view of the problem that the photocatalytic activity of the existing photocatalytic material ZnIn2S4 is limited, the purpose of the present invention is to provide a micron flower-shaped Ca-doped ZnIn2S4 material, a preparation method and its application in photocatalytic hydrogen production. The present invention adopts calcium doping on the photocatalytic material ZnIn2S4, and synthesizes ZnIn2S4 materials with different calcium doping amounts based on a one-step hydrothermal method. The prepared calcium-doped photocatalytic material has a micron flower-shaped morphology structure, which is conducive to multiple reflections and refractions of light, improves the light absorption capacity and light utilization rate, and appropriate calcium doping can optimize the band gap structure, reduce the recombination of photogenerated carriers, and help improve the photocatalytic activity and cycle stability of the ZnIn2S4 material, further expanding the development and application of the ZnIn2S4 material.
[0005] Based on the above purpose, the technical solution adopted by the present invention is as follows:
[0006] In a first aspect, the present invention provides a micron flower ball-shaped Ca-doped ZnIn2S4 material, in which the Ca doping mass is 0.25% to 2%; the morphology of the material is a micron flower ball-shaped material formed by stacking Ca-doped ZnIn2S4 nanosheets.
[0007] The micron-flower-ball-like morphology structure formed by stacking ZnIn2S4 nanosheets is conducive to multiple reflections and refractions of light, improves light absorption capacity and light utilization, and helps to improve the photocatalytic activity of ZnIn2S4 materials.
[0008] Preferably, the doping mass of Ca in the material is 0.25% to 0.75%.
[0009] Preferably, the doping mass of Ca in the material is 0.71%.
[0010] The present invention performs calcium doping on the photocatalytic material ZnIn2S4 material. Calcium (Ca) doping introduces defect energy levels, optimizes the band gap structure, reduces the recombination of photogenerated carriers, and improves the catalytic performance of the material under visible light, so that the material exhibits higher catalytic hydrogen production activity under visible light. When the doping mass of Ca is 0.25% to 0.75%, the photocatalytic activity of the ZnIn2S4 material is significantly improved, especially when the doping mass of Ca is 0.71%, the calcium-doped ZnIn2S4 material exhibits a relatively optimal photocatalytic hydrogen production activity.
[0011] In a second aspect, the present invention provides a method for preparing the above-mentioned micron flower ball-shaped Ca-doped ZnIn2S4 material, comprising the following steps:
[0012] Calcium salt and zinc salt in a stoichiometric ratio are dissolved in water, and then indium salt and thioacetamide are added and mixed, and then hydrothermally reacted at 180°C to 200°C for 12 to 18 hours, cooled to room temperature, and washed, solid-liquid separated, and dried to obtain Ca-doped ZnIn2S4 material.
[0013] The present invention uses calcium salt, zinc salt, indium salt and thioacetamide as raw materials, and can prepare Ca-doped ZnIn2S4 material through a one-step hydrothermal reaction. The preparation process is simple and easy, and the method does not use template materials and surfactants, which simplifies the preparation steps and avoids excessive raw material and energy consumption.
[0014] Preferably, the ratio of the sum of the molar amounts of the calcium salt and the zinc salt to the sum of the molar amounts of the indium salt and thioacetamide is 1:10.
[0015] Preferably, the molar ratio of calcium salt to zinc salt is 1:(0.25-9).
[0016] Preferably, the molar ratio of calcium salt to zinc salt is 1:(2-9).
[0017] Preferably, the molar ratio of indium salt to thioacetamide is 1:4.
[0018] The present invention regulates the doping amount of calcium by regulating the ratio of each component of the raw material. Appropriate Ca doping in the catalyst helps to broaden the light absorption range of the catalyst, improve the migration and separation efficiency of carriers, and reduce the overpotential of hydrogen evolution. In addition, appropriate calcium doping in the catalyst can improve the band gap. Ca doping reduces the band gap width of the material, thereby reducing the energy required for electrons to transition from the valence band to the conduction band, improving the utilization rate of visible light, and enhancing the photocatalytic performance of the catalyst. In short, through the combined effect of the catalyst structure and components, the micron flower ball-shaped Ca-doped ZnIn2S4 material prepared by the method of the present invention exhibits efficient photocatalytic hydrogen production performance.
[0019] Preferably, the calcium salt is selected from at least one of anhydrous calcium chloride and calcium nitrate, the zinc salt is selected from at least one of zinc chloride and zinc nitrate, and the indium salt is selected from at least one of indium chloride tetrahydrate and indium nitrate.
[0020] In a third aspect, the present invention provides the use of the above-mentioned micron flower ball-shaped Ca-doped ZnIn2S4 material in photocatalytic hydrogen production.
[0021] In a fourth aspect, the present invention provides a method for producing hydrogen by photocatalytic water decomposition, comprising the following steps: mixing the above-mentioned micron flower ball-shaped Ca-doped ZnIn2S4 material, a sacrificial agent and water, and reacting under visible light irradiation to obtain hydrogen.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The present invention adopts a simple one-step hydrothermal method to prepare a micron flower ball-shaped Ca-doped ZnIn2S4 material. Calcium (Ca) doping introduces defect energy levels, optimizes the band gap structure, reduces the recombination of photogenerated carriers, and improves the catalytic performance of the material under visible light, so that it exhibits higher hydrogen production activity under visible light.
[0024] (2) The present invention uses only calcium salt, zinc salt, indium salt and thioacetamide as raw materials, and the preparation method does not use template materials and surfactants, which simplifies the preparation steps and avoids excessive consumption of raw materials and energy.
[0025] (3) The morphology of the calcium-doped ZnIn2S4 material prepared by the method of the present invention is a micron flower ball structure formed by stacking ZnIn2S4 nanosheets, which is conducive to multiple reflections and refractions of light, thereby improving light absorption capacity and light utilization efficiency.
[0026] (4) The present invention adjusts the doping amount of calcium in the Ca-doped ZnIn2S4 material by adjusting the ratio of the raw material components. Experiments have found that when the molar ratio of Ca to Zn precursor is 1:(2-9), especially 1:4, the photocatalytic hydrogen production activity of the prepared calcium-doped ZnIn2S4 material is 2.36 times higher than that of the pure ZnIn2S4 material, and it shows good stability in long-term cyclic stability experiments.
[0027] In summary, the present invention regulates the appropriate Ca doping amount in the catalyst by adjusting the raw material component ratio. On the one hand, the introduction of calcium broadens the light absorption range of the catalyst, improves the migration and separation efficiency of carriers, and reduces the hydrogen evolution overpotential; on the other hand, appropriate calcium doping helps to improve the band gap. Ca doping reduces the band gap width of the material, thereby reducing the energy required for electrons to transition from the valence band to the conduction band, improving the utilization rate of visible light, and enhancing the photocatalytic performance of the catalyst. Through the combined effect of structure and components, the micron flower ball-shaped Ca-doped ZnIn2S4 material prepared by the method of the present invention exhibits efficient photocatalytic hydrogen production performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a scanning electron microscope image (SEM) of the Ca-doped ZnIn2S4 material (20CZ) in Example 2;
[0029] Figure 2 High-resolution transmission electron microscopy (HRTEM) image (a) and selected element distribution maps (b-f) of the Ca-doped ZnIn2S4 material (20CZ) in Example 2;
[0030] Figure 3 The crystal structure diagram (XRD) of ZnIn2S4 materials with different Ca doping amounts and pure ZnIn2S4 and pure CaIn2S4 photocatalytic materials in Examples 1 to 4;
[0031] Figure 4 UV-visible diffuse reflection absorption spectra (DRS) (a) of ZnIn2S4 materials with different Ca doping amounts in Examples 1 to 4 and the comparative example pure ZnIn2S4 photocatalytic material and the band gap value calculation (αhν) 2 Relationship diagram with hν (b);
[0032] Figure 5 Linear sweep voltammetry (LSV) (a), photocurrent (b) and electrochemical impedance spectroscopy (EIS) (c) of ZnIn2S4 materials with different Ca doping amounts and pure ZnIn2S4 photocatalytic materials in Examples 1 to 4;
[0033] Figure 6The comparison diagram of the photocatalytic decomposition of water to produce hydrogen with different Ca-doped ZnIn2S4 materials and pure ZnIn2S4 photocatalytic materials in Examples 1 to 4 (a) and the cyclic stability test result diagram of the most active sample 20CZ (b) are shown. DETAILED DESCRIPTION
[0034] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The test methods used in the examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified.
[0035] Example 1
[0036] This embodiment provides a method for preparing a ZnIn2S4 material doped with 0.25% Ca, comprising the following steps:
[0037] (1) Use an electronic balance to accurately weigh 0.1 mmol (0.0111 g) of anhydrous calcium chloride and 0.9 mmol (0.1227 g) of zinc chloride, put them into a 100-mL beaker, add 40 mL of distilled water, place on a magnetic stirrer, stir vigorously at room temperature for 30 min, then transfer to an ultrasonic machine and sonicate for 30 min until clarified to obtain an aqueous solution containing calcium chloride and zinc chloride.
[0038] (2) Add 2 mmol (0.5864 g) of indium chloride tetrahydrate and 8 mmol (0.6010 g) of thioacetamide to the aqueous solution containing calcium chloride and zinc chloride obtained in step (1), stir at room temperature for 30 min, and perform ultrasonication for 30 min until the mixture is uniformly mixed to form a mixed solution.
[0039] (3) The mixed solution obtained in step (2) was transferred to a 100 mL steel autoclave lined with polytetrafluoroethylene and heated in an oven at 180° C. for 12 hours. After the sample was cooled to room temperature, it was washed three times with deionized water and anhydrous ethanol respectively, and the centrifuge speed was set to 10,000 rpm and the centrifugation time was 1 min to perform a centrifugal solid-liquid separation operation, and the precipitate was collected.
[0040] (4) The obtained precipitate was dried in an oven at 60°C for 8 hours to obtain a ZnIn2S4 material with a Ca doping mass of 0.25%, named 10CZ.
[0041] Then, 20 mg of the ZnIn2S4 material powder (10CZ) with a Ca doping content of 0.25% prepared in this example was accurately weighed and placed in a photocatalytic water decomposition reaction device for hydrogen production performance testing.
[0042] Example 2
[0043] This embodiment provides a method for preparing a ZnIn2S4 material doped with 0.71% Ca, comprising the following steps:
[0044] (1) Use an electronic balance to accurately weigh 0.2 mmol (0.0222 g) of anhydrous calcium chloride and 0.8 mmol (0.1088 g) of zinc chloride, put them into a 100-mL beaker, add 40 mL of distilled water, place on a magnetic stirrer, stir vigorously at room temperature for 30 min, then transfer to an ultrasonic machine and sonicate for 30 min until clarified to obtain an aqueous solution containing calcium chloride and zinc chloride.
[0045] (2) Add 2 mmol (0.5864 g) of indium chloride tetrahydrate and 8 mmol (0.6010 g) of thioacetamide to the aqueous solution containing calcium chloride and zinc chloride obtained in step (1), stir at room temperature for 30 min, and perform ultrasonication for 30 min until the mixture is uniformly mixed to form a mixed solution.
[0046] (3) The mixed solution obtained in step (2) was transferred to a 100 mL steel autoclave lined with polytetrafluoroethylene and heated in an oven at 180° C. for 12 hours. After the sample was cooled to room temperature, it was washed three times with deionized water and anhydrous ethanol respectively, and the centrifuge speed was set to 10,000 rpm and the centrifugation time was 1 min to perform a centrifugal solid-liquid separation operation, and the precipitate was collected.
[0047] (4) The obtained precipitate was dried in an oven at 60°C for 8 hours to obtain a ZnIn2S4 material with a Ca doping mass of 0.71%, named 20CZ.
[0048] Then, 20 mg of the ZnIn2S4 material powder (20CZ) with a Ca doping content of 0.71% prepared in this example was accurately weighed and placed in a photocatalytic water decomposition reaction device for hydrogen production performance testing.
[0049] Example 3
[0050] This embodiment provides a method for preparing a ZnIn2S4 material doped with 0.75% Ca, comprising the following steps:
[0051] (1) Use an electronic balance to accurately weigh 0.3 mmol (0.0333 g) of anhydrous calcium chloride and 0.7 mmol (0.0954 g) of zinc chloride, put them into a 100-mL beaker, add 40 mL of distilled water, place on a magnetic stirrer, stir vigorously at room temperature for 30 min, then transfer to an ultrasonic machine and sonicate for 30 min until clarified to obtain an aqueous solution containing calcium chloride and zinc chloride.
[0052] (2) Add 2 mmol (0.5864 g) of indium chloride tetrahydrate and 8 mmol (0.6010 g) of thioacetamide to the aqueous solution containing calcium chloride and zinc chloride obtained in step (1), stir at room temperature for 30 min, and perform ultrasonication for 30 min until the mixture is uniformly mixed to form a mixed solution.
[0053] (3) The mixed solution obtained in step (2) was transferred to a 100 mL steel autoclave lined with polytetrafluoroethylene and heated in an oven at 180° C. for 12 hours. After the sample was cooled to room temperature, it was washed three times with deionized water and anhydrous ethanol respectively, and the centrifuge speed was set to 10,000 rpm and the centrifugation time was 1 min to perform a centrifugal solid-liquid separation operation, and the precipitate was collected.
[0054] (4) The obtained precipitate was dried in an oven at 60°C for 8 hours to obtain a ZnIn2S4 material with a Ca doping mass of 0.75%, named 30CZ.
[0055] Then, 20 mg of the ZnIn2S4 material powder (30CZ) with a Ca doping content of 0.75% prepared in this example was accurately weighed and placed in a photocatalytic water decomposition reaction device for hydrogen production performance testing.
[0056] Example 4
[0057] This embodiment provides a method for preparing a ZnIn2S4 material doped with 2% Ca, comprising the following steps:
[0058] (1) Use an electronic balance to accurately weigh 0.8 mmol (0.0888 g) of anhydrous calcium chloride and 0.2 mmol (0.0273 g) of zinc chloride, put them into a 100-mL beaker, add 40 mL of distilled water, place on a magnetic stirrer, stir vigorously at room temperature for 30 min, then transfer to an ultrasonic machine and sonicate for 30 min until clarified to obtain an aqueous solution containing calcium chloride and zinc chloride.
[0059] (2) Add 2 mmol (0.5864 g) of indium chloride tetrahydrate and 8 mmol (0.6010 g) of thioacetamide to the aqueous solution containing calcium chloride and zinc chloride obtained in step (1), stir at room temperature for 30 min, and perform ultrasonication for 30 min until the mixture is uniformly mixed to form a mixed solution.
[0060] (3) The mixed solution obtained in step (2) was transferred to a 100 mL steel autoclave lined with polytetrafluoroethylene and heated in an oven at 180° C. for 12 hours. After the sample was cooled to room temperature, it was washed three times with deionized water and anhydrous ethanol respectively, and the centrifuge speed was set to 10,000 rpm and the centrifugation time was 1 min to perform a centrifugal solid-liquid separation operation, and the precipitate was collected.
[0061] (4) The obtained precipitate was dried in an oven at 60°C for 8 hours to obtain a ZnIn2S4 material with a Ca doping mass of 2.0%, named 80CZ.
[0062] Then, 20 mg of the ZnIn2S4 material powder (80CZ) with a Ca doping content of 2% prepared in this example was accurately weighed and placed in a photocatalytic water decomposition reaction device for hydrogen production performance testing.
[0063] Comparative Example
[0064] This comparative example provides a preparation method of an undoped pure ZnIn2S4 material, comprising the following steps:
[0065] (1) Use an electronic balance to accurately weigh 1 mmol (0.1136 g) of zinc chloride, put it into a 100-mL beaker, add 40 mL of distilled water, place it on a magnetic stirrer, stir vigorously at room temperature for 30 min, then transfer it to an ultrasonic machine and sonicate for 30 min until it is clear, to obtain a zinc chloride aqueous solution.
[0066] (2) Add 2 mmol (0.5864 g) of indium chloride tetrahydrate and 8 mmol (0.6010 g) of thioacetamide to the aqueous zinc chloride solution, stir at room temperature for 30 min, and perform ultrasonication for 30 min until the mixture is uniformly mixed to form a mixed solution.
[0067] (3) The mixed solution obtained in step (2) was transferred to a 100 mL steel autoclave lined with polytetrafluoroethylene and heated in an oven at 180° C. for 12 hours. After the sample was cooled to room temperature, it was washed three times with deionized water and anhydrous ethanol respectively, and the centrifuge speed was set to 10,000 rpm and the centrifugation time was 1 min to perform a centrifugal solid-liquid separation operation, and the precipitate was collected.
[0068] (4) The precipitate was dried in an oven at 60°C for 8 hours to obtain undoped pure ZnIn2S4 material, named ZnIn2S4.
[0069] Then, 20 mg of the undoped ZnIn2S4 material powder prepared in this comparative example was accurately weighed and placed in a photocatalytic water decomposition reaction device for hydrogen production performance testing.
[0070] Example 5 Performance Test
[0071] 1. Structural performance testing of materials
[0072] The SEM image of the micron flower ball-shaped Ca-doped ZnIn2S4 material (20CZ) prepared in Example 2 is shown in FIG. Figure 1 As shown, high-resolution transmission electron microscopy HRTEM photos are shown Figure 2 As shown in a, Figure 1 and Figure 2a Comprehensive characterization results show that the morphology of the Ca-doped ZnIn2S4 material (20CZ) prepared in Example 2 is a micron flower ball formed by stacking ZnIn2S4 nanosheets.
[0073] The distribution of elements in Ca-doped ZnIn2S4 material (20CZ) is as follows Figure 2 As shown in b~f, it can be seen that the Ca element is uniformly doped in the ZnIn2S4 lattice.
[0074] The crystal structure diagrams (XRD) of ZnIn2S4 materials with different Ca doping amounts and pure ZnIn2S4 and pure CaIn2S4 photocatalytic materials in Examples 1 to 4 are as follows: Figure 3 As shown, due to the influence of doping, Ca 2+ The radius is larger than Zn 2+ With the increase of Ca doping amount, the characteristic peak at the (102) plane of ZnIn2S4 gradually shifts to a smaller 2θ degree, and the characteristic peak of CaIn2S4 does not appear in the spectrum, which excludes the possibility of synthesizing CaIn2S4.
[0075] The UV-visible diffuse reflection absorption spectra (DRS) of the ZnIn2S4 materials with different Ca doping amounts in Examples 1 to 4 and the pure ZnIn2S4 photocatalytic material in the comparative example are shown in FIG. Figure 4 As shown in a, it shows that with the increase of Ca 2+ As the amount of introduction increases, the spectrum edge red-shifts and the sample color gradually deepens, which is consistent with the enhanced light absorption result. For 20CZ, the inherent absorption edge not only red-shifts to 563nm, but also the light absorption capacity in the near-infrared region is significantly enhanced. The band gap results obtained by calculation are as follows Figure 4 As shown in b, it can be seen that 20CZ has a narrower band gap, which means that Ca doping introduces defect energy levels and reduces the band gap width, reducing the energy required for electrons to transition from the valence band to the conduction band, thereby improving the utilization rate of visible light.
[0076] The linear sweep voltammetry (LSV) curves of the ZnIn2S4 materials with different Ca doping amounts and the pure ZnIn2S4 photocatalytic material in Examples 1 to 4 are as follows: Figure 5 As shown in a, it shows that Ca doping reduces the overpotential of hydrogen evolution. Photocurrent ( Figure 5 b) and impedance ( Figure 5 c) Analysis shows that Ca doping improves the photogenerated carrier migration and separation efficiency of the catalyst.
[0077] 2. Testing of hydrogen production performance of materials
[0078] This example tests the photocatalytic decomposition of water to produce hydrogen activity of ZnIn2S4 materials with different Ca doping amounts and pure ZnIn2S4 photocatalytic materials in Examples 1 to 4, and the detection method is as follows:
[0079] A Labsolar-6A fully automatic online trace gas analysis system (Perfectly Technology Co., Ltd.) connected to a GC-9790 gas chromatograph was used to store and quantify the hydrogen produced by the material under simulated sunlight (300 W xenon lamp, AM1.5 filter).
[0080] The photocatalytic reaction was carried out in a 100 mL reaction system. Before the test, 20 mg of the catalyst was weighed and then added to a beaker containing 90 mL of deionized water, followed by 10 mL of triethanolamine (TEOA) sacrificial agent. After a uniform solution was formed, it was transferred to a 150 mL Pyrex heat-resistant and radiation-proof glass photocatalytic reactor with a magnetic stirrer at the bottom of the reactor.
[0081] The photocatalytic reactor was connected to the above-mentioned trace gas analysis system and stirred continuously until the end of the test. During the entire reaction process, argon was used as the carrier gas and the condensed water temperature was maintained at 5°C. Each test cycle was 30 minutes, and a total of 5 cycles were tested. According to the above procedures and reaction systems, a cyclic photocatalytic stability test was carried out. The analysis system was shut down every two hours, and the system was reopened after the hydrogen entered the gas chromatograph for analysis. This operation was carried out four times in total to compare the hydrogen production rate of the photocatalytic material in each cycle, and finally the test was ended.
[0082] Comparison of the photocatalytic decomposition of water to produce hydrogen activity of ZnIn2S4 materials with different Ca doping amounts and pure ZnIn2S4 photocatalytic materials in Examples 1 to 4 Figure 6 As shown in a, in the hydrogen production activity test of each photocatalyst under simulated sunlight, the photocatalytic hydrogen production rates of 10CZ, 20CZ, and 30CZ were 438.34 μmol g -1 h -1 , 611.32 μmol g -1 h -1 and 383.14 μmol g -1 h -1 The photocatalytic hydrogen production rate of pure ZnIn2S4 is 259.39 μmol g -1 h -1 Compared with pure ZnIn2S4 photocatalytic materials, the calcium-doped photocatalytic materials of the present invention, such as 10CZ, 20CZ, and 30CZ, show significantly enhanced hydrogen production activity, among which 20CZ has the highest activity. However, the photocatalytic hydrogen production rate of 80CZ is less than 1 / 2 of that of pure ZnIn2S4 photocatalytic materials, which may mean that excessive calcium doping affects the polymerization and structural integrity of ZnIn2S4, and loses its hydrogen production activity.
[0083] The hydrogen production cycle performance of the catalyst 20CZ with the highest hydrogen production activity was further tested. The results are as follows: Figure 6As shown in b, in the four-cycle cycling test, the most active 20CZ showed higher cycling stability.
Claims
1. A micron flower ball-shaped Ca-doped ZnIn2S4 material, characterized in that: The doping mass of Ca in the material is 0.25% to 2%; the morphology of the material is a micron flower ball formed by stacking Ca-doped ZnIn2S4 nanosheets.
2. The micron flower ball-shaped Ca-doped ZnIn2S4 material according to claim 1 is characterized in that: The doping mass of Ca in the material is 0.25% to 0.75%.
3. A method for preparing the micron flower ball-shaped Ca-doped ZnIn2S4 material according to claim 1 or 2, characterized in that: The steps include: Calcium salt and zinc salt in a stoichiometric ratio are dissolved in water, and then indium salt and thioacetamide are added and mixed, and then hydrothermally reacted at 180°C to 200°C for 12 to 18 hours, cooled to room temperature, and washed, solid-liquid separated, and dried to obtain Ca-doped ZnIn2S4 material.
4. The method for preparing the micron flower ball-shaped Ca-doped ZnIn2S4 material according to claim 3 is characterized in that: The ratio of the sum of the molar amounts of the calcium salt and the zinc salt to the sum of the molar amounts of the indium salt and thioacetamide is 1:
10.
5. The method for preparing the micron flower ball-shaped Ca-doped ZnIn2S4 material according to claim 4 is characterized in that: The molar ratio of the calcium salt to the zinc salt is 1:(0.25-9).
6. The method for preparing the micron flower ball-shaped Ca-doped ZnIn2S4 material according to claim 5, characterized in that: The molar ratio of the calcium salt to the zinc salt is 1:(2-9).
7. The method for preparing the micron flower ball-shaped Ca-doped ZnIn2S4 material according to claim 4, characterized in that: The molar ratio of the indium salt to the thioacetamide is 1:
4.
8. The method for preparing the micron flower ball-shaped Ca-doped ZnIn2S4 material according to claim 3, characterized in that: The calcium salt is selected from at least one of anhydrous calcium chloride and calcium nitrate, the zinc salt is selected from at least one of zinc chloride and zinc nitrate, and the indium salt is selected from at least one of indium chloride tetrahydrate and indium nitrate.
9. Use of the micron flower ball-shaped Ca-doped ZnIn2S4 material according to claim 1 or 2 in photocatalytic hydrogen production.
10. A method for producing hydrogen by photocatalytic water decomposition, characterized in that: The method comprises the following steps: mixing the micron flower ball-shaped Ca-doped ZnIn2S4 material according to claim 1 or 2, a sacrificial agent and water, and reacting them under visible light irradiation to obtain hydrogen.
Citation Information
Patent Citations
Preparation method for 2D / 2D nitrogen-doped lanthanum titanate / sulfur-indium-zinc heterojunction photocatalyst
CN111085234A
Preparation method of MoS2 quantum dot doped ZnIn2S4 composite photocatalyst and application thereof
CN113019400A