Flotation separation method for copper-sulfur polymetallic ore

By using different crystals to different responses to collectors and inhibitors, combined with multiple selection and step-strengthening flotation, the problem of separation difficulties between chalcopyrite and pyrite is solved, and the recovery rate of copper and sulfur is improved , realizes efficient copper resource recycling.

CN118988549AActive Publication Date: 2024-11-22JIANGXI COPPER +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410975196.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

During the flotation separation process, the chemical properties of chalcopyrite and pyrite are similar, resulting in the inability of conventional collectors and inhibitors to effectively recover copper and inhibit pyrite minerals, resulting in the loss of copper resources.

Method used

By adjusting the response differences of different crystal surfaces of chalcopyrite and pyrite to collectors and inhibitors, sodium cyanamide, sodium dicyanamide, sodium polylamine and sodium polysulfide are used as collectors and inhibitors. Combined with multiple selection and step-strengthened flotation, improve the recovery of copper and sulfur.

Benefits of technology

Differential flotation of chalcopyrite and pyrite with similar floating properties was achieved, which improved the copper recovery rate by more than 89%, and reduced the copper content and lime consumption in sulfur-containing tailings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988549A_ABST
    Figure CN118988549A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flotation, in particular to a flotation separation method for copper-sulfur polymetallic ore. The flotation separation method for the copper-sulfur polymetallic ore comprises the following steps that S1, raw ore is subjected to ore grinding treatment, and ore grinding materials with the exposure ratios of the 112 crystal face, the 204 crystal face and the 312 crystal face of copper pyrites being 55%-65%, 5%-18% and 3%-10% respectively and the exposure ratio of the 100 crystal face of iron pyrites being 60%-80% are obtained; s2, the ore grinding material, a collecting agent A, an inhibitor B and a foaming agent are mixed and subjected to primary roughing, and roughing concentrate and roughing tailings are obtained; s3, the roughing concentrate and a collecting agent A are mixed and subjected to multiple times of concentration, and copper concentrate is obtained; s4, the roughing tailings are subjected to gradient enhanced flotation, and sulfur-containing tailings are obtained; the collecting agent A comprises a # imgabs 0 # inhibitor; the B comprises sodium cyanamide, sodium dicyanamide, sodium polycyanamide and sodium polysulfide; the flotation method improves the recovery rate of copper and sulfur.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of flotation technology, and in particular to a flotation separation method for copper-sulfur polymetallic ore. Background Art

[0002] Copper and sulfur are important metal resources in modern industry and have important applications in the fields of chemical industry, industrial manufacturing, fireproof materials and aerospace. Chalcopyrite has attracted widespread attention because it contains three metal elements: iron, copper and sulfur. Chalcopyrite is mainly produced in polymetallic sulfide deposits and coexists with sulfide ores such as pyrite, molybdenite and arsenopyrite. In the flotation separation process, due to the similarity of the chemical properties of chalcopyrite and pyrite, and the fact that chalcopyrite and pyrite are extremely easy to oxidize and have similar floatability, chalcopyrite concentrate is usually obtained by preferential flotation. However, conventional collectors and inhibitors cannot effectively recover copper and inhibit pyrite minerals, resulting in the loss of copper resources.

[0003] In view of this, this invention is proposed. Summary of the invention

[0004] The object of the present invention is to provide a flotation separation method for copper-sulfur polymetallic ore, thereby improving the recovery rate of copper and sulfur.

[0005] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0006] The present invention provides a flotation separation method for copper-sulfur polymetallic ore, comprising the following steps:

[0007] S1. Grinding the raw ore to obtain a ground material; in the ground material, the exposure ratio of the 112 crystal plane of chalcopyrite is 55% to 65%, the exposure ratio of the 204 crystal plane is 5% to 18%, the exposure ratio of the 312 crystal plane is 3% to 10%, and the exposure ratio of the 100 crystal plane of pyrite is 60% to 80%;

[0008] S2, after the ground material is slurried and pH adjusted in sequence, collector A, inhibitor B and frother are added to carry out a roughing, to obtain a roughing concentrate and a roughing tailing;

[0009] S3, the rougher concentrate and collector A are mixed and subjected to multiple concentrations to obtain a copper concentrate;

[0010] S4, the roughing tailings are subjected to cascade enhanced flotation to obtain sulfur-containing tailings;

[0011] The collector A comprises

[0012] The inhibitor B includes sodium cyanamide, sodium dicyanamide, sodium polymelamide and sodium polysulfide.

[0013] Furthermore, in step S1, in the raw ore, the average grade of copper is 0.2% to 0.6%, and the average grade of sulfur is 1% to 2%.

[0014] Furthermore, in step S1, the grinding process includes sequentially performing a first-stage grinding process and a second-stage grinding process, wherein the first-stage grinding process includes semi-autogenous grinding, and the second-stage grinding process includes ball milling and / or segment milling.

[0015] Furthermore, in step S2 and step S4, the mass ratio of the sodium cyanamide, the sodium dicyanamide, the sodium polymelamide and the sodium polysulfide is (1-5): (10-17): (2-7): (1-2).

[0016] Furthermore, in step S2, during the primary roughing process, the amount of collector A added is 1000-2000 g / t, and the amount of inhibitor B added is 50-1500 g / t.

[0017] Furthermore, in step S3, the multiple selections include three selections or four selections.

[0018] Furthermore, in step S3, in the first stage and the second stage of the multiple cleanings, the amount of the collector A added is independently 50 to 200 g / t.

[0019] Further, in step S4, the step-enhanced flotation comprises:

[0020] The rougher tailings are subjected to three open-circuit roughing operations to obtain an open-circuit rougher concentrate;

[0021] The open-circuit roughing concentrate is subjected to flotation to obtain the sulfur-containing tailings; the flotation includes primary roughing, secondary cleaning and tertiary scavenging.

[0022] Furthermore, in step S4, the three open-circuit roughing includes: adding 10-80 g / t of the collector A to perform three open-circuit roughing.

[0023] Furthermore, in step S4, the first roughing includes: adding 10-35 g / t of activator and 50-150 g / t of butyl xanthate for a first roughing; the third sweeping includes: adding 10-50 g / t of butyl xanthate for three sweepings.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The flotation separation method of the copper-sulfur polymetallic ore of the present invention realizes the differential flotation of chalcopyrite and pyrite with similar floatability according to the difference in the responsiveness of different crystal faces of chalcopyrite to the collector and the selective unsaturated coordination of the inhibitor to the crystal face properties of chalcopyrite and pyrite, solves the problem of separation of chalcopyrite and pyrite under low alkalinity conditions, and improves the recovery rates of copper and sulfur, and the recovery rate of copper can reach more than 89%. DETAILED DESCRIPTION

[0026] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0027] In some embodiments of the present invention, a flotation separation method for copper-sulfur polymetallic ore is provided, comprising the following steps:

[0028] S1. Grinding the raw ore to obtain a ground material; in the ground material, the exposure ratio of the 112 crystal plane of chalcopyrite is 55% to 65%, the exposure ratio of the 204 crystal plane is 5% to 18%, the exposure ratio of the 312 crystal plane is 3% to 10%, and the exposure ratio of the 100 crystal plane of pyrite is 60% to 80%;

[0029] S2, after the ground material is slurried and pH adjusted in sequence, collector A, inhibitor B and frother are added to carry out a roughing, and roughing concentrate and roughing tailings are obtained;

[0030] S3, the rougher concentrate and the collector A are mixed and subjected to multiple concentrations to obtain a copper concentrate;

[0031] S4, the roughing tailings are subjected to cascade enhanced flotation to obtain sulfur-containing tailings;

[0032] Collector A includes

[0033] Inhibitor A includes sodium cyanamide (CAS: 17292-62-5), sodium dicyanamide (CAS: 1934-75-4), sodium polymelamine (molecular weight of 1000-1500) and sodium polysulfide.

[0034] The flotation separation method of the copper-sulfur polymetallic ore of the present invention is a method for improving the flotation efficiency of copper-sulfur based on the difference of crystal planes.

[0035] According to the action mode of different crystal faces of chalcopyrite and pyrite on the unsaturated coordination of collectors and inhibitors, the invention realizes the low-alkalinity recovery of easily floatable chalcopyrite and pyrite, does not need to use a large amount of lime to inhibit pyrite, reduces the copper content in sulfur-containing tailings and the amount of lime used, and the copper recovery rate can reach more than 89%.

[0036] For chalcopyrite, the most sparse crystal face is the 112 crystal face, followed by the 204 crystal face; the CN group in collector A can adsorb to the 112 crystal face of chalcopyrite; while the inhibitory ability of inhibitor B cannot replace the adsorption of the CN group in collector A on the 112 crystal face of chalcopyrite, mainly because the 4-coordinated iron on the surface of chalcopyrite is replaced by the CN group in collector A to become 6-coordinated iron under high-spin conditions. At this time, the iron ions in chalcopyrite are in a saturated state, which weakens or reduces the mutual coordination between inhibitor B and chalcopyrite, thereby increasing the floatability of chalcopyrite.

[0037] The 112-faced atoms of chalcopyrite have a large number of broken bonds, and the Cu ions and Fe ions are transformed from 4-coordinated to 3-coordinated. Both are in a ligand-deficient state, are more active, and are easily strongly adsorbed by collector A. The iron in pyrite is a regular octahedron with a 6-coordinated structure, and the iron ions are in a low-spin state, which is easier to be oxidized under the action of collector A, causing the 6-coordinated iron ions in pyrite to change from a low-spin state to a high-spin state, and the iron becomes highly oxidized iron, thereby achieving the inhibition of pyrite.

[0038] In the process of multiple roughing, collector A is added to the part of chalcopyrite that is not completely dissociated. The CN group in collector A increases the contact opportunity with the 112 crystal face of chalcopyrite. On the other hand, the change in the ball distribution method of the semi-autogenous grinding equipment increases the exposure ratio of the 112 crystal face of chalcopyrite and the 100 crystal face of pyrite. Under the action of inhibitor B, pyrite is inhibited to obtain the final high-quality copper concentrate. In the process of multiple roughing, collector A is easier to contact with chalcopyrite, and inhibitor B is added as an auxiliary collector to achieve comprehensive recovery of difficult-to-float copper minerals.

[0039] In some embodiments of the present invention, in step S1, the raw ore includes chalcopyrite and pyrite.

[0040] In some embodiments of the present invention, in step S1, the average copper grade in the raw ore is 0.2% to 0.6%, and the average sulfur grade is 1% to 2%; preferably, the average iron grade in the raw ore is 1.5% to 2.5%; more preferably, the average copper grade in the raw ore is 0.35% to 0.45%, the average sulfur grade is 1.55 to 1.65%, and the average iron grade is 1.95% to 2.05%.

[0041] In some embodiments of the present invention, in step S1, the grinding treatment includes sequentially performing a first-stage grinding treatment and a second-stage grinding treatment, the first-stage grinding treatment includes semi-autogenous grinding, and the second-stage grinding treatment includes ball milling and / or segment milling; preferably, the time of the first-stage grinding treatment is 0.1 to 0.2 h, and the time of the second-stage grinding treatment is 0.15 to 0.3 h.

[0042] In some embodiments of the present invention, in step S1, in the ground material, the mass of solid particles with a particle size of less than 0.074 mm accounts for 60% to 70% of the total mass of solid particles.

[0043] The exposure ratio of the crystal plane is determined based on the XRD test data using the ratio of the normalized peak intensities of the characteristic peaks representing each crystal plane.

[0044] In some embodiments of the present invention, in step S1, typically but not limiting, for example, in the ground material, the exposure ratio of the 112 crystal plane of chalcopyrite can be 55%, 58%, 60%, 62%, 65% or a range consisting of any two thereof; the exposure ratio of the 204 crystal plane of chalcopyrite can be 5%, 8%, 10%, 13%, 15%, 18% or a range consisting of any two thereof; the exposure ratio of the 312 crystal plane of chalcopyrite can be 3%, 5%, 7%, 10% or a range consisting of any two thereof; the exposure ratio of the 100 crystal plane of pyrite can be 60%, 65%, 70%, 75%, 80% or a range consisting of any two thereof.

[0045] In some embodiments of the present invention, slurry adjustment includes adding water to the ground material to adjust the slurry concentration to 30 wt % to 35 wt %.

[0046] In some embodiments of the present invention, in step S2, pH adjustment includes: adding lime to adjust the pH of the slurry to 7-12.

[0047] In some embodiments of the present invention, in step S2, the mass ratio of sodium cyanamide, sodium dicyanamide, sodium polymelamine and sodium polysulfide is (1-5): (10-17): (2-7): (1-2); typically but not limitatively, for example, the mass ratio of sodium cyanamide, sodium dicyanamide, sodium polymelamine and sodium polysulfide can be 1:8:2:1, 2:8:3:1, 3:9:3:1, 4:10:5:1, 5:12:3:1, 3:15:4:1, 5:17:6:1, 4:16:6:2, 5:15:7:2 and the like.

[0048] In some embodiments of the present invention, in step S2, the foaming agent includes but is not limited to pine oil.

[0049] In some embodiments of the present invention, in step S2, during a roughing process, the amount of collector A added is 1000-2000 g / t; typically but not limitatively, for example, in step S2, during a roughing process, the amount of collector A added can be 1000 g / t, 1200 g / t, 1400 g / t, 1600 g / t, 1800 g / t, 2000 g / t or a range consisting of any two of them.

[0050] In some embodiments of the present invention, in step S2, during a roughing process, the amount of inhibitor B added is 50 to 1500 g / t; typically but not limitatively, for example, in step S2, during a roughing process, the amount of inhibitor B added can be 50 g / t, 200 g / t, 500 g / t, 700 g / t, 1000 g / t, 1200 g / t, 1500 g / t or a range consisting of any two of them.

[0051] In some embodiments of the present invention, in step S2, during the primary roughing process, the amount of the foaming agent added is 10 to 30 g / t; typically but not limitatively, for example, in step S2, during the primary roughing process, the amount of the foaming agent added can be 10 g / t, 15 g / t, 20 g / t, 25 g / t, 30 g / t or a range consisting of any two of them.

[0052] In some embodiments of the present invention, in step S3, the multiple refinements include three refinements or four refinements.

[0053] In some embodiments of the present invention, in step S3, in the first stage and the second stage of multiple selections, the amount of collector A added is independently 50-200 g / t; preferably, in step S3, in the first stage of multiple selections, the amount of collector A added is 100-200 g / t; in the second stage of multiple selections, the amount of collector A added is 50-100 g / t.

[0054] In some embodiments of the present invention, in step S3, multiple selections are performed, including the following steps:

[0055] 100-200 g / t of collector A is added to the rougher concentrate for one-stage concentration to obtain concentrated ore I and concentrated middlings I; 50-100 g / t of collector A is added to the concentrated concentrate I for two-stage concentration to obtain concentrated ore II and concentrated middlings II; the concentrated concentrate II is subjected to three-stage concentration to obtain copper concentrate and concentrated middlings III; among them, the concentrated middlings II and the concentrated middlings III are returned to the previous stage for re-selection.

[0056] In some embodiments of the present invention, in step S4, the step-enhanced flotation comprises:

[0057] The rougher tailings are subjected to three open-circuit roughing operations to obtain open-circuit rougher concentrate;

[0058] The open-circuit rougher concentrate is subjected to flotation to obtain sulfur-containing tailings; flotation includes primary roughing, secondary cleaning and tertiary scavenging.

[0059] In some embodiments of the present invention, in step S4, the three open circuit roughing includes: adding 10-80 g / t of collector A for three open circuit roughing; typically but not limitatively, for example, in step S4, the amount of collector A added during the three open circuit roughing process can be 10 g / t, 20 g / t, 30 g / t, 40 g / t, 50 g / t, 60 g / t, 70 g / t, 80 g / t or a range value composed of any two of them.

[0060] In some embodiments of the present invention, in step S4, the first roughing includes: adding 10-35 g / t of activator and 50-150 g / t of butyl xanthate for a first roughing; the third sweeping includes: adding 10-50 g / t of butyl xanthate for three sweepings.

[0061] In some embodiments of the present invention, in step S4, the step-enhanced flotation comprises the following steps:

[0062] Adding 70-80 g / t of collector A to the roughing tailings for one-stage open-circuit roughing to obtain open-circuit roughing concentrate I and open-circuit roughing tailings I; adding 50-60 g / t of collector A to the open-circuit roughing tailings I for two-stage open-circuit roughing to obtain open-circuit roughing concentrate II and open-circuit roughing tailings II; adding 10-30 g / t of collector A to the open-circuit roughing tailings II for three-stage open-circuit roughing to obtain open-circuit roughing concentrate III and open-circuit roughing tailings III; the open-circuit roughing concentrate I, the open-circuit roughing concentrate II and the open-circuit roughing concentrate III are mixed to obtain an open-circuit roughing concentrate;

[0063] Adding 10-35 g / t of activator and 50-150 g / t of butyl xanthate (collector) to the open-circuit roughing concentrate to carry out a roughing operation to obtain a roughing concentrate IV and a roughing tailing IV;

[0064] The rougher concentrate IV is subjected to a first-stage concentration to obtain a concentrated concentrate V and a concentrated middling V; the concentrated concentrate V is subjected to a second-stage concentration to obtain a concentrated concentrate VI and a concentrated middling VI;

[0065] 10-50 g / t of butyl xanthate is added to the concentrated ore VI for one-stage scavenging to obtain scavenged ore VII and scavenged tailings VII; 10-50 g / t of butyl xanthate is added to the scavenged tailings VII for two-stage scavenging to obtain scavenged ore VIII and scavenged tailings VIII; 10-50 g / t of butyl xanthate is added to the scavenged tailings VIII for three-stage scavenging to obtain scavenged ore IX and scavenged tailings IX, and the scavenged tailings IX are sulfur-containing tailings.

[0066] In some embodiments of the present invention, in step S4, the activator includes but is not limited to copper sulfate.

[0067] In the flotation separation method of the copper-sulfur polymetallic ore of the present invention, the added amount of each reagent is the mass of the reagent added per ton of ore pulp.

[0068] Example 1

[0069] The flotation separation method of the copper-sulfur polymetallic ore provided in this embodiment comprises the following steps:

[0070] S1. The original ore is a copper-sulfur polymetallic ore; the metal minerals include chalcopyrite and pyrite, and the gangue ores include quartz and mica; the average grade of copper in the original ore is 0.4%, the average grade of sulfur is 1.6%, and the average grade of iron is 2.0%;

[0071] The raw ore is semi-autogenously ground for 0.15 h, and then segment-milled or ball-milled for 0.2 h to obtain ground ore;

[0072] The particles with a particle size of less than 0.074 mm account for 65wt% of the grinding material; in the grinding material, the exposure ratio of the 112 crystal plane of chalcopyrite is 57%, the exposure ratio of the 204 crystal plane is 8%, the exposure ratio of the 312 crystal plane is 5%, and the exposure ratio of the 100 crystal plane of pyrite is 63%;

[0073] S2, adding water to the grinding material to adjust the mass concentration of the slurry to 30wt%, adding lime to adjust the pH to 7, adding 1200g / t collector A, 500g / t inhibitor B and 20g / t pine oil to perform a roughing, and obtaining a roughing concentrate and a roughing tailing;

[0074] S3, add 150g / t collector A to the rougher concentrate for one-stage concentration to obtain concentrated ore I and concentrated middlings I; add 50g / t collector A to the concentrated concentrate I for two-stage concentration to obtain concentrated ore II and concentrated middlings II; the concentrated concentrate II is subjected to three-stage concentration to obtain copper concentrate and concentrated middlings III; wherein, the concentrated middlings II and the concentrated middlings III are returned to the previous stage for re-selection;

[0075] S4, adding 70g / t collector A to the roughing tailings for one-stage open circuit roughing to obtain open circuit roughing concentrate I and open circuit roughing tailings I; adding 50g / t collector A to the open circuit roughing tailings I for two-stage open circuit roughing to obtain open circuit roughing concentrate II and open circuit roughing tailings II; adding 15g / t collector A to the open circuit roughing tailings II for three-stage open circuit roughing to obtain open circuit roughing concentrate III and open circuit roughing tailings III; the open circuit roughing concentrate I, the open circuit roughing concentrate II and the open circuit roughing concentrate III are mixed to obtain an open circuit roughing concentrate;

[0076] Add 20 g / t of copper sulfate as an activator and 100 g / t of butyl xanthate as a collector to the open-circuit rougher concentrate for a rougher separation to obtain a rougher concentrate IV and a rougher tailing IV;

[0077] The rougher concentrate IV is subjected to a first-stage concentration to obtain a concentrated concentrate V and a concentrated middling V; the concentrated concentrate V is subjected to a second-stage concentration to obtain a concentrated concentrate VI and a concentrated middling VI;

[0078] 20 g / t of butyl xanthate was added to the concentrated ore VI for one-stage scavenging to obtain scavenged ore VII and scavenged tailings VII; 20 g / t of butyl xanthate was added to the scavenged tailings VII for two-stage scavenging to obtain scavenged ore VIII and scavenged tailings VIII; 10 g / t of butyl xanthate was added to the scavenged tailings VIII for three-stage scavenging to obtain scavenged ore IX and scavenged tailings IX (sulfur-containing tailings).

[0079] Wherein, collector A comprises

[0080] The inhibitor B comprises sodium cyanamide, sodium dicyanamide, sodium polymelamine (molecular weight of 1000-1500) and sodium polysulfide in a mass ratio of 2:10:3:1.5.

[0081] Example 2

[0082] The flotation separation method of the copper-sulfur polymetallic ore provided in this embodiment comprises the following steps:

[0083] S1. The original ore is a copper-sulfur polymetallic ore; the metal minerals include chalcopyrite and pyrite, and the gangue ores include quartz and mica; the average grade of copper in the original ore is 0.4%, the average grade of sulfur is 1.6%, and the average grade of iron is 2.0%;

[0084] The raw ore is semi-autogenously ground for 0.17h, and then segment-milled or ball-milled for 0.23h to obtain ground ore;

[0085] The particles with a particle size of less than 0.074 mm accounted for 69wt% of the grinding material; in the grinding material, the exposure ratio of the 112 crystal plane of chalcopyrite was 62%, the exposure ratio of the 204 crystal plane was 13%, the exposure ratio of the 312 crystal plane was 8%, and the exposure ratio of the 100 crystal plane of pyrite was 75%;

[0086] S2, adding water to the grinding material to adjust the mass concentration of the slurry to 30wt%, adding lime to adjust the pH to 7, adding 1500g / t collector A, 1000g / t inhibitor B and 25g / t pine oil to perform a roughing, and obtaining a roughing concentrate and a roughing tailing;

[0087] S3, adding 200g / t collector A to the rougher concentrate for one-stage concentration to obtain concentrated ore I and concentrated middlings I; adding 100g / t collector A to the concentrated concentrate I for two-stage concentration to obtain concentrated ore II and concentrated middlings II; the concentrated concentrate II is subjected to three-stage concentration to obtain copper concentrate and concentrated middlings III; wherein, the concentrated middlings II and the concentrated middlings III are returned to the previous stage for re-selection;

[0088] S4, adding 80g / t collector A to the roughing tailings for one-stage open circuit roughing to obtain open circuit roughing concentrate I and open circuit roughing tailings I; adding 60g / t collector A to the open circuit roughing tailings I for two-stage open circuit roughing to obtain open circuit roughing concentrate II and open circuit roughing tailings II; adding 30g / t collector A to the open circuit roughing tailings II for three-stage open circuit roughing to obtain open circuit roughing concentrate III and open circuit roughing tailings III; the open circuit roughing concentrate I, the open circuit roughing concentrate II and the open circuit roughing concentrate III are mixed to obtain an open circuit roughing concentrate;

[0089] 30 g / t of copper sulfate as an activator and 150 g / t of butyl xanthate as a collector were added to the open-circuit rougher concentrate to perform a rougher separation to obtain a rougher concentrate IV and a rougher tailing IV;

[0090] The rougher concentrate IV is subjected to a first-stage concentration to obtain a concentrated concentrate V and a concentrated middling V; the concentrated concentrate V is subjected to a second-stage concentration to obtain a concentrated concentrate VI and a concentrated middling VI;

[0091] 40 g / t of butyl xanthate was added to the concentrated ore VI for one-stage scavenging to obtain scavenged ore VII and scavenged tailings VII; 40 g / t of butyl xanthate was added to the scavenged tailings VII for two-stage scavenging to obtain scavenged ore VIII and scavenged tailings VIII; 20 g / t of butyl xanthate was added to the scavenged tailings VIII for three-stage scavenging to obtain scavenged ore IX and scavenged tailings IX (sulfur-containing tailings).

[0092] Wherein, collector A comprises

[0093] The inhibitor B comprises sodium cyanamide, sodium dicyanamide, sodium polymelamine (molecular weight of 1000-1500) and sodium polysulfide in a mass ratio of 3:12:6:2.

[0094] Example 3

[0095] The flotation separation method of the copper-sulfur polymetallic ore provided in this embodiment comprises the following steps:

[0096] S1. The original ore is a copper-sulfur polymetallic ore; the metal minerals include chalcopyrite and pyrite, and the gangue ores include quartz and mica; the average grade of copper in the original ore is 0.4%, the average grade of sulfur is 1.6%, and the average grade of iron is 2.0%;

[0097] The raw ore is semi-autogenously ground for 0.15 h, and then segment-milled or ball-milled for 0.18 h to obtain ground ore;

[0098] The particles with a particle size of less than 0.074 mm account for 62wt% of the grinding material; in the grinding material, the exposure ratio of the 112 crystal plane of chalcopyrite is 55%, the exposure ratio of the 204 crystal plane is 5%, the exposure ratio of the 312 crystal plane is 3%, and the exposure ratio of the 100 crystal plane of pyrite is 60%;

[0099] S2, adding water to the grinding material to adjust the mass concentration of the slurry to 30wt%, adding lime to adjust the pH to 7, adding 1000g / t collector A, 300g / t inhibitor B and 15g / t pine oil to perform a roughing, and obtaining a roughing concentrate and a roughing tailing;

[0100] S3, add 120g / t collector A to the rougher concentrate for one-stage concentration to obtain concentrated ore I and concentrated middlings I; add 50g / t collector A to the concentrated concentrate I for two-stage concentration to obtain concentrated ore II and concentrated middlings II; the concentrated concentrate II is subjected to three-stage concentration to obtain copper concentrate and concentrated middlings III; wherein, the concentrated middlings II and the concentrated middlings III are returned to the previous stage for re-selection;

[0101] S4, adding 70g / t collector A to the roughing tailings for one-stage open circuit roughing to obtain open circuit roughing concentrate I and open circuit roughing tailings I; adding 50g / t collector A to the open circuit roughing tailings I for two-stage open circuit roughing to obtain open circuit roughing concentrate II and open circuit roughing tailings II; adding 10g / t collector A to the open circuit roughing tailings II for three-stage open circuit roughing to obtain open circuit roughing concentrate III and open circuit roughing tailings III; the open circuit roughing concentrate I, the open circuit roughing concentrate II and the open circuit roughing concentrate III are mixed to obtain an open circuit roughing concentrate;

[0102] 15 g / t of copper sulfate as an activator and 80 g / t of butyl xanthate as a collector were added to the open-circuit rougher concentrate to perform a rougher separation to obtain a rougher concentrate IV and a rougher tailing IV;

[0103] The rougher concentrate IV is subjected to a first-stage concentration to obtain a concentrated concentrate V and a concentrated middling V; the concentrated concentrate V is subjected to a second-stage concentration to obtain a concentrated concentrate VI and a concentrated middling VI;

[0104] 20 g / t of butyl xanthate was added to the concentrated ore VI for one-stage scavenging to obtain scavenged ore VII and scavenged tailings VII; 20 g / t of butyl xanthate was added to the scavenged tailings VII for two-stage scavenging to obtain scavenged ore VIII and scavenged tailings VIII; 10 g / t of butyl xanthate was added to the scavenged tailings VIII for three-stage scavenging to obtain scavenged ore IX and scavenged tailings IX (sulfur-containing tailings).

[0105] Wherein, collector A comprises

[0106] The inhibitor B comprises sodium cyanamide, sodium dicyanamide, sodium polymelamine (molecular weight of 1000-1500) and sodium polysulfide in a mass ratio of 2:8:3:1 (4:16:6:2).

[0107] Comparative Example 1

[0108] The flotation separation method of the copper-sulfur polymetallic ore provided in this comparative example refers to Example 1, except that, in step S1, the raw ore is crushed and screened to -10 mm, accounting for 95wt%, and then ball milled for 0.2h to obtain a ground material; the particles with a particle size of less than 0.074mm account for 62wt% of the ground material; in the ground material, the exposure ratio of the 112 crystal plane of chalcopyrite is 53%, the exposure ratio of the 204 crystal plane is 7%, the exposure ratio of the 312 crystal plane is 5%, and the exposure ratio of the 100 crystal plane of pyrite is 55%;

[0109] Comparative Example 2

[0110] The flotation separation method of copper-sulfur polymetallic ore provided in this comparative example refers to Example 1, except that the collector A is ethionamide and the inhibitor B is lime.

[0111] Test Example 1

[0112] In the flotation separation methods of copper-sulfur polymetallic ores of Examples 1 to 3 and Comparative Examples 1 to 2, the average grades and recoveries of copper and sulfur are shown in Table 1.

[0113] Table 1

[0114]

[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A flotation separation method for copper-sulfur polymetallic ore, characterized in that: The steps include: S1. Grinding the raw ore to obtain a ground material; in the ground material, the exposure ratio of the 112 crystal plane of chalcopyrite is 55% to 65%, the exposure ratio of the 204 crystal plane is 5% to 18%, the exposure ratio of the 312 crystal plane is 3% to 10%, and the exposure ratio of the 100 crystal plane of pyrite is 60% to 80%; S2, after the ground material is slurried and pH adjusted in sequence, collector A, inhibitor B and frother are added to carry out a roughing, to obtain a roughing concentrate and a roughing tailing; S3, the rougher concentrate and collector A are mixed and subjected to multiple concentrations to obtain a copper concentrate; S4, the roughing tailings are subjected to cascade enhanced flotation to obtain sulfur-containing tailings; The collector A comprises The inhibitor B includes sodium cyanamide, sodium dicyanamide, sodium polymelamide and sodium polysulfide.

2. The flotation separation method of copper-sulfur polymetallic ore according to claim 1, characterized in that: In step S1, in the raw ore, the average copper grade is 0.2% to 0.6%, and the average sulfur grade is 1% to 2%.

3. The flotation separation method of copper-sulfur polymetallic ore according to claim 1, characterized in that: In step S1, the grinding process includes sequentially performing a first-stage grinding process and a second-stage grinding process, wherein the first-stage grinding process includes semi-autogenous grinding, and the second-stage grinding process includes ball milling and / or segment milling.

4. The flotation separation method of copper-sulfur polymetallic ore according to claim 1, characterized in that: In step S2, the mass ratio of the sodium cyanamide, the sodium dicyanamide, the sodium polymelamine and the sodium polysulfide is (1-5): (10-17): (2-7): (1-2).

5. The flotation separation method of copper-sulfur polymetallic ore according to claim 1, characterized in that: In step S2, during the primary roughing process, the amount of collector A added is 1000-2000 g / t, and the amount of inhibitor B added is 50-1500 g / t.

6. The flotation separation method of copper-sulfur polymetallic ore according to claim 1, characterized in that: In step S3, the multiple selections include three selections or four selections.

7. The flotation separation method of copper-sulfur polymetallic ore according to claim 6, characterized in that: In step S3, in the first stage and second stage of the multiple cleanings, the amount of collector A added is independently 50-200 g / t.

8. The flotation separation method of copper-sulfur polymetallic ore according to claim 1, characterized in that: In step S4, the step-enhanced flotation comprises: The rougher tailings are subjected to three open-circuit roughing operations to obtain an open-circuit rougher concentrate; The open-circuit roughing concentrate is subjected to flotation to obtain the sulfur-containing tailings; the flotation includes primary roughing, secondary cleaning and tertiary scavenging.

9. The flotation separation method of copper-sulfur polymetallic ore according to claim 8, characterized in that: In step S4, the three open-circuit roughing includes: adding 10-80 g / t of the collector A to perform three open-circuit roughing.

10. The flotation separation method of copper-sulfur polymetallic ore according to claim 8, characterized in that: In step S4, the first roughing includes: adding 10-35 g / t of activator and 50-150 g / t of butyl xanthate for a first roughing; the third sweeping includes: adding 10-50 g / t of butyl xanthate for three sweeps.

Citation Information

Patent Citations

  • Floating method for finely disseminated copper sulfide ores

    CN106733202A

  • Ore grinding and flotation method for improving separation effect of copper-sulfur minerals

    CN113713958A

  • Mineral processing technology for recovering copper from copper-sulfur ore containing secondary copper sulfide ore

    CN114749270A

  • Flotation method of copper sulfide ore

    CN117943212A